Titanium alloy composite material and preparation method thereof

By synthesizing carbon nanotubes in situ on the surface of titanium alloy powder, and forming a nanoparticle Ti2Cu micro-mesh structure with magnetron sputtering and low-energy ball milling, the problem of insufficient mechanical properties of titanium alloy composites is solved, and the high mechanical properties of the material is achieved Performance and simplified production process, suitable for high-performance materials applications.

CN119016723AInactive Publication Date: 2024-11-26宁波尚材三维科技有限公司
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411507901.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-28
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing titanium alloy composite materials have shortcomings in mechanical properties and large-scale production efficiency, and it is difficult to meet the needs of high mechanical properties and lightweight materials in fields such as aerospace.

Method used

The carbon nanotubes were synthesized in situ on the surface of titanium alloy powder by chemical vapor deposition. Combined with magnetron sputtering method and low-energy ball milling method, the nanoparticle Ti2Cu micro-mesh structure and discontinuous mesh structure were formed to enhance the mechanical properties of the material. The density and hardness of the material are enhanced by discharge plasma sintering treatment.

Benefits of technology

It significantly enhances the stiffness, toughness and mechanical properties of titanium alloy composite materials, simplifies the preparation process, facilitates large-scale production, and is suitable for aerospace, biomedicine and marine equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a titanium alloy composite material and a preparation method thereof.The preparation method comprises the following steps that titanium alloy powder is provided, carbon nanotubes are synthesized on the surface of the titanium alloy powder in situ through a chemical vapor deposition method, and first composite powder is obtained; sputtering Cu atoms on the first composite powder by adopting a magnetron sputtering method to prepare second composite powder; the surface of the second composite powder is coated with a TiB2 reinforcing material through a low-energy ball milling method, and third composite powder is obtained; and sintering the third composite powder to obtain the titanium alloy composite material. According to the titanium alloy composite material prepared through the method, due to in-situ synthesis of CNTs on the surface, the rigidity and toughness of the titanium alloy composite material are remarkably enhanced, and then the mechanical property of the titanium alloy composite material is further enhanced through a micro-net structure formed by nano-particles Ti2Cu and a discontinuous net structure formed by TiB whiskers in sintering treatment; the preparation process is simple, large-scale production can be realized, and the production efficiency is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of composite materials, and particularly relates to a titanium alloy composite material and a preparation method thereof. Background Art

[0002] Titanium and titanium alloys are widely used in aerospace, marine, military and biomedical fields due to their low density, high specific strength, strong biocompatibility, low Young's modulus, strong corrosion resistance, good antibacterial properties, wide operating temperature range and good weldability. As we all know, titanium and titanium alloys are most widely used in the aerospace field. However, with my country's growing energy demand and green environmental protection development ideas, as well as the rapid improvement of national economic, scientific and technological, and military strength, especially the vigorous development of aerospace and high-performance military equipment, the requirements for titanium alloy materials are getting higher and higher, so lightweight materials with higher mechanical properties and operating temperatures are needed. Therefore, metal matrix composites (MMCs) are gradually being developed and applied.

[0003] MMCs are new high-strength materials prepared by combining a metal or alloy matrix with a reinforcement phase with excellent performance using special technical means. Titanium-based composites (TMCs) refer to a composite material obtained by adding a reinforcement phase to titanium or titanium alloy through casting, powder metallurgy and other methods. Since the development of TMCs, it has been widely used in aerospace, biomedicine, petrochemical and automotive industries due to its excellent specific strength, specific stiffness, good high temperature resistance, excellent wear resistance and corrosion resistance, and good biocompatibility, and has attracted much attention from researchers. Summary of the invention

[0004] An object of the present invention is to provide a titanium alloy composite material and a preparation method thereof, which are beneficial to enhancing the mechanical properties of the titanium alloy composite material.

[0005] Another object of the present invention is to provide a titanium alloy composite material and a preparation method thereof, which has a simple preparation process, is easy to operate, and can be mass-produced.

[0006] In order to achieve the above objectives, the technical solution adopted in this application is: a titanium alloy composite material and a preparation method thereof, the method comprising the following steps: S100, providing titanium alloy powder, and synthesizing carbon nanotubes in situ on the surface of the titanium alloy powder by chemical vapor deposition to obtain a first composite powder; S200, sputtering Cu atoms on the first composite powder by magnetron sputtering to obtain a second composite powder; S300, coating the surface of the second composite powder with a TiB2 reinforcement material by a low-energy ball milling method to obtain a third composite powder; S400, sintering the third composite powder to obtain a titanium alloy composite material.

[0007] In one embodiment, in step S100, the titanium alloy powder is hydrogenated dehydrogenated Ti-6Al-4V powder. Before in-situ synthesis of carbon nanotubes on the surface of the titanium alloy powder, the titanium alloy powder is first surface treated to remove impurities and an oxide layer, and then ultrasonically cleaned and dried.

[0008] In one embodiment, the hydrogenated dehydrogenated Ti-6Al-4V powder includes transition elements, and the transition elements are one or more of Fe, Ni, Zr, and Hf.

[0009] In one embodiment, the hydrogenated dehydrogenated Ti-6Al-4V powder includes one or more impurities or doping elements that are difficult to remove, wherein the impurities or doping elements include transition elements, the impurity content is ≤0.03wt.%, and the doping element content is 0.01wt.%~2wt.%.

[0010] In one embodiment, in step S200, the processing vacuum degree of the magnetron sputtering method is -1×10 -3 Pa to -6×10 -3 Pa, the sputtering time is 1h~5h, the sputtering power is 100W~400W, and the sputtering bias is 0V~200V.

[0011] In one embodiment, in step S300, the second composite powder and TiB2 powder are mixed in a mass ratio of 100: (0.2-1.5) and ball milled.

[0012] In one embodiment, the ball milling medium used in the low-energy ball milling method is selected from one or more of flux, anhydrous ethanol, stearic acid, and aviation kerosene, the ball milling protective gas is selected from one or more of argon and nitrogen, and the ball milling speed is 100rpm~400rpm.

[0013] In one embodiment, the ball milling jar used in the low-energy ball milling method is made of stainless steel, the ball-to-material ratio is 5:1-15:1, and the ball milling time is 2h-8h.

[0014] In one embodiment, in step S400, the sintering is performed in a spark plasma sintering furnace, the sintering temperature is 800°C to 1300°C, the heating rate is 60°C / min to 120°C / min, the sintering pressure is 20MPa to 60MPa, and the holding time is 5min to 10min.

[0015] According to another aspect of the present application, a titanium alloy composite material prepared by the above preparation method is also provided.

[0016] Compared with the prior art, the beneficial effects of this application are: (1) The present invention provides a titanium alloy composite material and a preparation method thereof, which synthesizes carbon nanotubes (CNTs) in situ on the surface of titanium alloy powder, thereby preventing CNTs from agglomerating in the titanium alloy composite material and hindering dislocation movement, thereby significantly enhancing the stiffness and toughness of the titanium alloy composite material. In addition, CNTs can also play a synergistic role with reinforcing materials to further improve the mechanical properties of the titanium alloy composite material; (2) The present invention provides a titanium alloy composite material and a preparation method thereof, which overcomes the shortcomings of the prior art. By combining the magnetron sputtering method with the low-energy ball milling method, Cu atoms and reinforcing materials are evenly distributed on the surface of the titanium alloy powder, and after spark plasma sintering treatment, a micro-network structure composed of nanoparticles Ti2Cu and a discontinuous network structure composed of reinforcing materials are formed in the titanium alloy composite material, thereby enhancing the mechanical properties of the titanium alloy composite material; (3) The titanium alloy composite material and the preparation method thereof provided by the present invention have the advantages of simple preparation process and easy operation, and can be put into large-scale production. Therefore, it has broad application prospects in the fields of aerospace, biomedicine, marine equipment, etc. DETAILED DESCRIPTION

[0017] Below, the present application is further described in conjunction with specific implementation methods. It should be noted that, under the premise of no conflict, the various embodiments or technical features described below can be arbitrarily combined to form new embodiments.

[0018] It should be noted that the terms "first", "second", etc. in the description and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence.

[0019] The terms "including" and "having" and any variations thereof in the specification and claims of this application are intended to cover non-exclusive inclusions. For example, a process, method, system, product or apparatus comprising a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to these processes, methods, products or apparatuses.

[0020] Specific embodiments applicable to the titanium alloy composite material and the preparation method thereof are further described below.

[0021] According to one aspect of the present invention, a titanium alloy composite material and a preparation method thereof include the steps of: S100, providing titanium alloy powder, and synthesizing carbon nanotubes in situ on the surface of the titanium alloy powder by chemical vapor deposition to obtain a first composite powder; S200, sputtering Cu atoms on the first composite powder by magnetron sputtering to obtain a second composite powder; S300, coating the surface of the second composite powder with a TiB2 reinforcement material by a low-energy ball milling method to obtain a third composite powder; S400, sintering the third composite powder to obtain a titanium alloy composite material.

[0022] The titanium alloy composite material prepared by this method has good mechanical properties, and thanks to the in-situ synthesized CNTs uniformly distributed on the surface of the titanium alloy powder, dislocation movement is hindered, and the stiffness and toughness of the titanium alloy composite material are significantly enhanced. Then, a micro-net structure composed of nanoparticles Ti2Cu and a discontinuous net structure composed of surface-coated reinforcing materials are formed in the titanium alloy composite material during sintering treatment to enhance the mechanical properties of the titanium alloy composite material. The preparation process is simple, and large-scale production can be achieved, further improving production efficiency, and having broad application prospects in the fields of aerospace, biomedicine, marine equipment, etc.

[0023] In one embodiment, in step S100, the titanium alloy powder is hydrogenated dehydrogenated Ti-6Al-4V powder. Before in-situ synthesis of carbon nanotubes on the surface of the titanium alloy powder, the titanium alloy powder is first surface treated to remove impurities and oxide layers, and then ultrasonically cleaned and dried. By removing impurities and oxide layers on the surface, the performance and subsequent processing quality of the titanium alloy composite material are improved, thereby enhancing the mechanical properties of the titanium alloy composite material. Thanks to ultrasonic cleaning, the titanium alloy composite material can be cleaned in a short time, further improving production efficiency.

[0024] In one embodiment, the titanium alloy powder is selected from one or more of TC4 titanium alloy powder, TA15 titanium alloy powder, TC11 titanium alloy powder, and TiAl titanium alloy powder.

[0025] In one embodiment, the hydrogenated dehydrogenated Ti-6Al-4V powder includes transition elements, and the transition elements are one or more of Fe, Ni, Zr, and Hf. The transition elements are used as catalysts to significantly improve the dispersibility and uniformity of CNTs in titanium alloy composites, avoid agglomeration of CNTs due to van der Waals forces, and further promote the in-situ growth and formation of CNTs. In other words, adding CNTs to the titanium alloy composite material hinders dislocation movement and significantly enhances the stiffness and toughness of the titanium alloy composite material. In addition, CNTs enhance the mechanical properties and thermal stability of the titanium alloy composite material due to its high strength, high conductivity and excellent thermal stability.

[0026] It can be understood that the in-situ synthesized CNTs are evenly distributed on the surface of the titanium alloy powder, overcoming the serious aggregation of CNTs in traditional powder mixtures. Thanks to the in-situ growth process of CNTs directly from the titanium alloy matrix, CNTs and Ti-6Al-4V powder have good interfacial bonding strength, further enhancing the mechanical properties and thermal stability of the titanium alloy composite material.

[0027] In one embodiment, the hydrogenated dehydrogenated Ti-6Al-4V powder includes one or more impurities or doping elements that are difficult to remove, and the impurities or doping elements include transition elements, and the impurity content is ≤0.03wt.%, and the doping element content is 0.01wt.%~2wt.%. The transition elements in the impurities or doping elements catalyze the in-situ synthesis process of CNTs on the surface of the titanium alloy powder, thereby further improving the mechanical properties of the titanium alloy composite material. In other words, since the low content of impurities contained in the titanium alloy powder can catalyze the in-situ synthesis reaction of CNTs, the addition of doping elements is not necessary, further reducing production costs.

[0028] In one embodiment, in step S200, the processing vacuum degree of the magnetron sputtering method is -1×10 -3 Pa to -6×10 -3 Pa, specifically, the processing vacuum degree of the magnetron sputtering method is -1×10 -3 Pa, -2×10 -3 Pa, -3×10 -3 Pa, -4×10 -3 Pa, -5×10 -3 Pa, -6×10 -3 Pa, further preferably, the processing vacuum degree is -3×10 -3 Pa to -6×10 -3 Pa, magnetron sputtering treatment is carried out under a predetermined vacuum degree, which not only reduces the frequency of gas molecule collisions during the sputtering process, thereby improving the sputtering efficiency, but also reduces the possibility of substrate contamination during the sputtering process, further improving the quality of the sputtered film layer.

[0029] In one embodiment, in step S200, the sputtering time is 1h~5h, specifically, the sputtering time can be 1h, 2h, 3h, 4h, 5h, and more preferably, the sputtering time is 1h~3h. Through a certain sputtering time, the uniformity, thickness and sputtering quality of the Cu atomic layer sputtered on the surface of the titanium alloy powder are improved, and the integrity and stability of the nano-scale Ti2Cu micronetwork structure formed in the subsequent sintering eutectoid process are enhanced.

[0030] In one embodiment, in step S200, the sputtering power is 100W~400W, specifically, the sputtering power can be 100W, 200W, 300W, 400W, and more preferably, the sputtering power is 150W~250W, and the sputtering bias is 0V~200V, specifically, the sputtering bias can be 0V, 30V, 50V, 80V, 100V, 150V, 200V, and more preferably, the sputtering bias is 30V~80V. Through the predetermined sputtering power and sputtering bias, Cu atoms are evenly distributed on the surface of CNTs / Ti-6Al-4V powder, and a nano-phase dispersion-strengthened titanium alloy composite material with high performance is prepared, which significantly improves the tensile strength and ductility of the titanium alloy composite material.

[0031] In other words, since the nanoparticles of Cu are mainly distributed on β-Ti, a eutectic reaction occurs during the subsequent sintering process to form dispersion-strengthened Ti2Cu nanoparticles. The nanoscale Ti2Cu phase inhibits the fine grain strengthening and dislocation strengthening of the α phase growth, further forming a micro-network structure and enhancing the mechanical properties of the titanium alloy composite material.

[0032] In one embodiment, in step S300, the second composite powder and TiB2 powder are mixed and ball-milled in a mass ratio of 100: (0.2-1.5), and specifically, the mass fraction of TiB2 powder is 0.2wt.%, 0.4wt.%, 0.6wt.%, 0.8wt.%, 1.0wt.%, 1.2wt.%, 1.4wt.%, 1.5wt.%, and TiB2, as a metal boride material, is used as a reinforcing phase to coordinate with CNTs to further improve the hardness, bending strength and wear resistance of the titanium alloy composite material. By adhering TiB2 powder to the surface, the hardness and bending strength of the titanium alloy composite material are significantly improved, and the TiB2 powder is uniformly wrapped on the surface of the CNTs / Ti-6Al-4V composite powder by low-energy ball milling. In the subsequent sintering process, an in-situ reaction is carried out on the surface of the titanium alloy to generate TiB whiskers, forming a discontinuous network structure, significantly refining the size of the original β grains, and further enhancing the mechanical properties of the titanium alloy composite material.

[0033] In one embodiment, the ball milling medium used in the low-energy ball milling method is selected from one or more of flux, anhydrous ethanol, stearic acid, and aviation kerosene. The ball milling medium can enter the gaps between the titanium alloy powders, which is beneficial to the dispersion of the powder and avoids the agglomeration of particles. It further evenly distributes the force applied to the powder particles during the ball milling process, improves the uniformity of the ball milling process, and significantly improves the ball milling effect.

[0034] In one embodiment, the ball milling protective gas is selected from one or more of argon and nitrogen. It is understandable that, since titanium is an active metal, it is easy to react with oxygen at high and normal temperatures, resulting in the formation of an oxide film on the powder surface, thereby affecting the performance and quality of the titanium alloy composite material. Thanks to the introduction of ball milling protective gas, the air in the equipment is replaced and oxygen is prevented from entering, and the atmosphere during the ball milling process is maintained stable, thereby protecting the titanium alloy powder from oxidation and ensuring the stability of the performance and quality of the ball milled product.

[0035] In one embodiment, the ball milling speed is 100 rpm to 400 rpm, specifically, the ball milling speed can be 100 rpm, 200 rpm, 300 rpm, 400 rpm. If the speed is too high, the collision between the ball milling media may be too intense, damaging the material structure or generating too much heat, affecting the ball milling effect and product quality. When the speed is too low, it may lead to insufficient ball milling and fail to achieve the expected ball milling effect. In other words, the ball milling efficiency can be significantly improved at the predetermined ball milling speed, further reducing energy consumption.

[0036] In one embodiment, the grinding balls of the ball mill used in the low-energy ball milling method are made of stainless steel, and the ball-to-material ratio is 5:1 to 15:1, specifically, the ball-to-material ratio is 5:1, 7:1, 9:1, 11:1, 13:1, 15:1, and the ball milling time is 2h to 8h, specifically, the ball milling time is 2h, 3h, 4h, 5h, 6h, 7h, 8h. The stainless steel ball mill has the advantages of corrosion resistance, rust prevention, high temperature stability and wide applicability during the ball milling process. The use of stainless steel ball mill for ball milling can effectively prevent the pollution and deterioration of the ball milling material during the ball milling process. Ball milling at a predetermined ball-to-material ratio and ball milling time can significantly improve the uniformity and microstructure of the titanium alloy powder, further optimize the ball milling effect, and enhance the performance of the titanium alloy composite material.

[0037] In one embodiment, in step S400, the sintering is performed in a spark plasma sintering furnace, and the sintering temperature is 800°C to 1300°C, specifically, the sintering temperature is 800°C, 900°C, 1000°C, 1100°C, 1200°C, 1300°C, and further preferably, the sintering temperature is 900°C, 1000°C, 1100°C, and the sintering heating rate is 60°C / min to 120°C / min, specifically, the sintering heating rate is 60°C / min, 70°C / min, 80°C / min, 90°C / min, 100°C / min, n, 110℃ / min, further preferably, the sintering heating rate is 90℃ / min, 100℃ / min, 110℃ / min, the sintering pressure is 20MPa~60MPa, specifically, the sintering pressure is 20MPa, 30MPa, 40MPa, 50MPa, 60MPa, further preferably, the sintering pressure is 30MPa, 40MPa, 50MPa, and the holding time is 5min~10min, specifically, the holding time is 5min, 6min, 7min, 8min, 9min, 10min.

[0038] In other words, the titanium alloy composite material with a network structure is formed by densification sintering using the spark plasma sintering molding process. Compared with traditional sintering, the spark plasma sintering method can effectively eliminate the porosity in the material and reduce the sintering temperature, thereby significantly limiting the growth of grains and further improving the mechanical properties of the titanium alloy composite material.

[0039] In addition, unless otherwise specified, all raw materials used are commercially available.

[0040] Example 1 (1) Preparation of CNTs / Ti-6Al-4V composite powder: First, the hydrogenated dehydrogenated Ti-6Al-4V powder was surface treated, and the treated powder was ultrasonically cleaned with ethanol and vacuum dried. Subsequently, fluidized bed chemical vapor deposition technology was used to decompose acetylene gas and in situ synthesize carbon nanotubes on the powder surface to prepare CNTs / Ti-6Al-4V composite powder.

[0041] (2) Preparation of Cu@CNTs / Ti-6Al-4V composite powder: 60 g of CNTs / Ti-6Al-4V composite powder was weighed and placed in a powder coating machine and vacuumed to -6.0×10 -3 Pa, introduce high-purity argon gas, turn on the Cu target DC power supply, set the sputtering power to 200 W, the sputtering bias to 50 V, and the sputtering duration to 2 h to prepare nanophase dispersion-strengthened Cu@CNTs / Ti-6Al-4V composite powder.

[0042] (3) Preparation of TiB2-Cu@CNTs / Ti-6Al-4V composite powder: 0.5 wt.% TiB2 powder and the Cu@CNTs / Ti-6Al-4V composite powder prepared in (2) were added into a stainless steel ball mill. The ball milling medium was a mixture of flux and anhydrous ethanol. After ball milling for 5 h at a rotation speed of 200 rpm under argon protection, the slurry mixture was dried in a vacuum oven to obtain TiB2-Cu@CNTs / Ti-6Al-4V composite powder.

[0043] (4) Preparation of TiB2-Cu@CNTs / Ti-6Al-4V composite material: The above-mentioned TiB2-Cu@CNTs / Ti-6Al-4V composite powder was placed in a graphite mold and then placed in a spark plasma sintering furnace for densification sintering. The sintering temperature was 1000°C, the heating rate was 100°C / min, the holding time was 5 min, and the sintering pressure was 40 MPa. After cooling, the sample was taken out to obtain the TiB2-Cu@CNTs / Ti-6Al-4V composite material.

[0044] Example 2 The difference between Example 2 and Example 1 is that in step (2), the sputtering power is 100 W.

[0045] Example 3 The difference between Example 3 and Example 1 is that in step (2), the sputtering power is 300 W.

[0046] Example 4 The difference between Example 4 and Example 1 is that in step (2), the sputtering bias voltage is 100V.

[0047] Example 5 The difference between Example 5 and Example 1 is that in step (2), the sputtering bias voltage is 30V.

[0048] Example 6 The difference between Example 6 and Example 1 is that in step (2), the sputtering duration is 3 hours.

[0049] Example 7 The difference between Example 7 and Example 1 is that in step (2), the sputtering duration is 1 hour.

[0050] Example 8 The difference between Example 8 and Example 1 is that in step (3), the mass fraction of TiB2 powder is 0.8 wt.%.

[0051] Example 9 The difference between Example 9 and Example 1 is that in step (3), the mass fraction of TiB2 powder is 0.2 wt.%.

[0052] Example 10 The difference between Example 10 and Example 1 is that in step (4), the sintering temperature is 800°C.

[0053] Embodiment 11 The difference between Example 11 and Example 1 is that in step (4), the sintering temperature is 1200°C.

[0054] Example 12 The difference between Example 12 and Example 1 is that in step (4), the sintering pressure is 30 MPa.

[0055] Example 13 The difference between Example 13 and Example 1 is that in step (4), the sintering pressure is 50 MPa.

[0056] Embodiment 14 The difference between Example 14 and Example 1 is that in step (4), the heating rate is 80°C / min.

[0057] Embodiment 15 The difference between Example 15 and Example 1 is that in step (4), the heating rate is 120°C / min.

[0058] Comparative Example 1 The difference between this comparative example and Example 1 is that, compared with Example 1, Comparative Example 1 lacks the process of in-situ synthesizing carbon nanotubes on the surface of the titanium alloy powder.

[0059] Comparative Example 2 The difference between this comparative example and Example 1 is that, compared with Example 1, Comparative Example 2 lacks the process of sputtering Cu atoms on the surface of the first composite powder.

[0060] Comparative Example 3 The difference between this comparative example and Example 1 is that, compared with Example 1, Comparative Example 3 lacks the process of coating the reinforcing material TiB2 powder on the surface of the second composite powder.

[0061] Comparative Example 4 The difference between this comparative example and Example 1 is that, compared with Example 1, in step (1), a ball mill is used to ball-mill and blend the carbon nanotubes and the titanium alloy powder, and the process of in-situ synthesizing carbon nanotubes on the surface of the titanium alloy powder in Example 1 is replaced.

[0062] Performance Evaluation The room temperature and high temperature tensile properties of the titanium alloy composite materials prepared in Examples 1 to 15 and Comparative Examples 1 to 4 were tested using a UTM5105X universal electronic testing machine. After the sample was processed by wire cutting, the upper and lower surfaces and sides of the sample were mechanically polished by sandpaper to eliminate the influence of machining on the surface stress of the sample. The high temperature tensile sample needs to be coated with an antioxidant. The room temperature tensile test was carried out with reference to GB / T 228.2-2010, and the tensile rate of the room temperature tensile test was 1.0 mm / min. The high temperature tensile test was carried out with reference to GB / T228.2-2015, and the temperature of the high temperature tensile test was 400℃-650℃, and the tensile rate was 0.4 mm / min. The density of the titanium alloy composite materials prepared in Examples 1 to 15 and Comparative Examples 1 to 4 was tested with reference to GB / T 3850-2015 standard, and the density of the material was calculated according to the formula. With reference to GB / T 4340.1-2009 standard, the titanium alloy composite materials prepared in Examples 1 to 15 and Comparative Examples 1 to 4 were tested for hardness using a HVS-1000 Vickers hardness tester. The results are shown in Table 1.

[0063] Table 1: Performance test of titanium alloy composite materials

[0064] It is understandable that different magnetron sputtering conditions of Cu make the obtained titanium alloy composite material have different properties. With reference to Example 1, Example 2 and Example 3, it can be known that increasing the magnetron sputtering power of Cu is conducive to increasing the content of Cu on the surface of the powder, further improving the nano-particle Ti2Cu network structure formed by Cu after sintering, improving the mechanical properties of the titanium alloy composite material, and improving the density of the material. Correspondingly, when the magnetron sputtering power is too high, the content of Cu on the surface of the powder is too much, which hinders TiB2 from contacting with the surface of the titanium-based material and reacting to form TiB whiskers, reduces the content of the discontinuous network structure formed, and reduces the hardness and bending strength of the titanium alloy composite material. With reference to Example 1, Example 4 and Example 5, it can be known that increasing the magnetron sputtering bias of Cu is conducive to improving the uniformity and content of Cu on the surface of the powder, further improving the nano-particle Ti2Cu network structure formed after sintering, improving the mechanical properties of the titanium alloy composite material, and improving the density of the material. Correspondingly, when the sputtering bias is too high, it is easy to cause the instability of compound sputtering in this process, thereby reducing the mechanical properties of the titanium alloy composite material.

[0065] Further, referring to Example 1, Example 6 and Example 7, it can be seen that as the sputtering time increases, Cu is deposited more evenly on the powder surface and has a higher content, so that the nanoparticle Ti2Cu network structure formed after sintering is more perfect, thereby improving the tensile strength and density of the titanium alloy composite material. Correspondingly, when the sputtering time is too long, the thickness of Cu on the powder surface is too high, which hinders the formation of the network structure on the powder surface, thereby reducing the performance of the titanium alloy composite material.

[0066] Since the added TiB2 reacts in situ with the titanium-based material to form TiB whiskers and present a discontinuous network structure, it can be seen from Examples 1, 8 and 9 that as the added TiB2 content increases, the formed TiB whisker discontinuous network structure becomes more and more perfect, and the tensile strength of the titanium alloy composite material is enhanced and the mechanical properties are improved. Correspondingly, when the added TiB2 content is too high, the uniformity of Cu distribution on the surface is hindered, and the nanoparticle Ti2Cu microstructure formed by eutectoid during the sintering process is further hindered, thereby reducing the mechanical properties of the titanium alloy composite material and reducing the tensile strength.

[0067] With reference to Example 1, Example 10 and Example 11, it can be seen that as the sintering temperature increases, the density of the titanium alloy composite material increases, and the hardness of the material further increases. Accordingly, when the sintering temperature is too high, the grains in the material grow, reducing the uniformity of the grains, thereby affecting the microstructure and mechanical properties of the material.

[0068] Further, referring to Example 1, Example 12 and Example 13, it can be seen that as the sintering pressure increases, the density of the titanium alloy composite material increases, thereby improving the mechanical properties of the titanium alloy composite material. However, when the sintering pressure is too high, excessive stress and increased lattice distortion occur inside the material, thereby affecting the performance of the titanium alloy composite material.

[0069] It is understandable that at a certain sintering heating rate, it is beneficial to enhance the mechanical properties of the titanium alloy composite material. By comparing Example 1, Example 14 and Example 15, it can be seen that with the increase of the sintering heating rate, the density of the titanium alloy composite material increases and the tensile strength is greater. However, in Example 11 where the sintering heating rate is too high, the internal temperature of the material rises rapidly due to the high heating rate, thereby causing the phenomenon of local over-temperature, which in turn causes changes in the microstructure of the material, and even cracks and other phenomena appear inside, further affecting the mechanical properties of the titanium alloy composite material.

[0070] As shown in Table 1, the results show that, through Comparative Examples 1, 2 and 3, the lack of addition of any one of carbon nanotubes, Cu and TiB2 significantly reduces the room temperature tensile strength of the titanium alloy composite material. It can be understood that the lack of the network structure formed by Ti2Cu and TiB2 reduces the high-temperature tensile properties of the titanium alloy composite material, which fully demonstrates that the network structure of Cu and TiB2 formed in the titanium alloy composite material of Example 1 has a promoting effect on enhancing the high-temperature tensile properties; the density of the titanium alloy composite material is increased by the addition of Cu; the synergistic effect of Cu and TiB2 further improves the density of the material; in addition, the TiB whiskers with a network structure distribution will inhibit the growth of grains, further refine the grain size, and play a role in refining grains and strengthening grain boundaries, the hardness of the titanium alloy composite material is enhanced, and thus plays a role in strengthening the titanium alloy composite material.

[0071] Furthermore, it can be seen from Comparative Example 4 that only CNTs and Ti-6Al-4V powder are mechanically ball milled. Due to the high aspect ratio and nanoscale characteristics of CNTs, the van der Waals force causes CNTs to attract each other and aggregate, which easily leads to agglomeration. Therefore, compared with Example 1, the titanium alloy composite material in Comparative Example 4 has poor mechanical properties and density, and further reduces the tensile strength.

[0072] The foregoing examples are merely illustrative and are used to explain some features of the method of the present invention. The appended claims are intended to claim the widest possible range that can be conceived, and the embodiments presented herein are merely illustrations of selected implementations according to the combination of all possible embodiments. Therefore, it is the applicant's intention that the appended claims are not limited by the selection of examples that illustrate the features of the present invention. Some numerical ranges used in the claims also include sub-ranges therein, and changes in these ranges should also be interpreted as being covered by the appended claims where possible.

Claims

1. A method for preparing a titanium alloy composite material, It is characterized in that It includes the following steps: S100, providing titanium alloy powder, and synthesizing carbon nanotubes in situ on the surface of the titanium alloy powder by chemical vapor deposition to obtain a first composite powder; S200, sputtering Cu atoms on the first composite powder by magnetron sputtering to obtain a second composite powder; S300, coating TiB on the surface of the second composite powder by low energy ball milling 2 reinforcing the material to obtain a third composite powder; S400, sintering the third composite powder to obtain a titanium alloy composite material.

2. The preparation method according to claim 1, It is characterized in that In step S100, the titanium alloy powder is hydrogenated dehydrogenated Ti-6Al-4V powder. Before in-situ synthesis of carbon nanotubes on the surface of the titanium alloy powder, the titanium alloy powder is firstly subjected to surface treatment to remove impurities and an oxide layer, and then ultrasonically cleaned and dried.

3. The preparation method according to claim 2, It is characterized in that The hydrogenated dehydrogenated Ti-6Al-4V powder includes transition elements, and the transition elements are one or more of Fe, Ni, Zr, and Hf.

4. The preparation method according to claim 2, It is characterized in that The hydrogenated dehydrogenated Ti-6Al-4V powder includes one or more impurities or doping elements that are difficult to remove, wherein the impurities or doping elements include transition elements, the impurity content is ≤0.03wt.%, and the doping element content is 0.01wt.%~2wt.%.

5. The preparation method according to claim 1, It is characterized in that In step S200, the processing vacuum degree of the magnetron sputtering method is -1×10 -3 Pa to -6×10 -3 Pa, the sputtering time is 1h~5h, the sputtering power is 100W~400W, and the sputtering bias is 0V~200V.

6. The preparation method according to claim 1, It is characterized in that In step S300, the second composite powder is mixed with TiB 2 The powders were mixed and ball milled in a mass ratio of 100:(0.2~1.5).

7. The preparation method according to claim 6, It is characterized in that The ball milling medium used in the low-energy ball milling method is selected from one or more of flux, anhydrous ethanol, stearic acid, and aviation kerosene, the ball milling protection gas is selected from one or more of argon and nitrogen, and the ball milling speed is 100rpm~400rpm.

8. The preparation method according to claim 6, It is characterized in that The ball milling jar used in the low-energy ball milling method is made of stainless steel, the ball-to-material ratio is 5:1-15:1, and the ball milling time is 2h-8h.

9. The preparation method according to claim 1, It is characterized in that In step S400, the sintering is carried out in a spark plasma sintering furnace, the sintering temperature is 800°C to 1300°C, the heating rate is 60°C / min to 120°C / min, the sintering pressure is 20MPa to 60MPa, and the holding time is 5min to 10min.

10. A titanium alloy composite material prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of homodisperse carbon nano tube enhanced aluminium base composite material

    CN101864547A

  • Method for preparing reinforced titanium-based composite material of carbon nanometer tube through vacuum hot pressing

    CN103509962A

  • Carbon nanotube coated titanium spherical composite powder and preparation method thereof

    CN109550941A

  • Preparing method for composite powder with metal base wrapped by carbon nanotubes

    CN111020525A

  • Preparing process of carbon nanotube reinforced titanium matrix composite

    CN111155039A