Preparation method of large-size homogeneous compact molybdenum rod billet

Through powder metallurgy technology and multi-step processes of vacuum consumable smelting, bidirectional extrusion and precision forging, the problem of poor density and homogeneity of molybdenum rod blanks is solved, and high-density and homogeneity of molybdenum rods are achieved. Blank preparation, suitable for high-demand fields such as aerospace.

CN119016728AInactive Publication Date: 2024-11-26INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411491922.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The density and homogeneity of existing molybdenum rod billets are poor, resulting in lower performance than pure molybdenum rods in high temperature and high pressure environments, and cannot meet the high density requirements in aerospace and other fields.

Method used

Molybdenum rods are prepared by powder metallurgy technology. Through vacuum consumable smelting and bidirectional extrusion technology, combined with forging by precision forging, the density and homogeneity of the molybdenum rod blank are gradually improved.

Benefits of technology

The high density of molybdenum rod blank is achieved, with a density of 99.03% of the theoretical density and an improved yield, which is suitable for the preparation of large-size homogeneous dense molybdenum rod blanks.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a large-size homogeneous compact molybdenum rod blank, and belongs to the technical field of metal powder manufacturing. Molybdenum rods of different specifications are pressed and prepared by adopting a metal powder metallurgy technology, the molybdenum rods are prepared into casting blanks by adopting vacuum consumable smelting, and then the casting blanks are extruded into rod blanks of different sizes by adopting a bidirectional extrusion technology; and finally, a finished bar blank is forged through a precision forging machine, and preparation of the homogeneous and compact bar blank is achieved. By adopting the method provided by the invention, the density of the molybdenum rod blank can be increased and can reach 99.03% of the theoretical density to the maximum. Meanwhile, the process and the method provided by the invention can also be popularized to production of other types of products, and have wide prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal powder manufacturing, in particular to a method for preparing a large-sized homogeneous and dense molybdenum rod blank. Background Art

[0002] Molybdenum rods are widely used in aerospace, electronic information, precision casting and other fields due to their high melting point, good thermal conductivity, low thermal expansion, excellent oxidation resistance and other performance characteristics. With the development of electronic information technology and aerospace technology, the demand for homogeneous and dense rods is becoming more and more urgent.

[0003] The preparation process of sintered molybdenum rod blanks includes the following steps: molybdenum powder screening and purification, molybdenum powder mixing, isostatic pressing, medium frequency sintering, and molybdenum rod straightening. At present, the density of sintered molybdenum rods sintered by medium frequency sintering can only reach 9.5g / cm 3 , and the density between pure molybdenum rod (10.28g / cm 3 ) There is a big gap. If the density of molybdenum parts for aerospace does not meet the requirements, they will release gas in the space environment, affecting the normal operation of the instrument; in actual use, it is found that the performance of molybdenum wire and other products made from sintered molybdenum rods is lower than that of similar products made from pure molybdenum rods. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing large-sized, homogeneous and dense molybdenum rod blanks, so as to solve the problem of poor density and homogeneity of molybdenum rod blanks. The present invention can prepare large-sized, homogeneous and dense molybdenum rod blanks, and at the same time achieve a high yield of molybdenum rod blanks.

[0005] In order to achieve the above object, the present invention adopts the following technical solution:

[0006] A method for preparing a large-sized homogeneous and dense molybdenum rod blank comprises the following steps in sequence: Step 1: Using powder metallurgy technology to press and sinter molybdenum rods of different specifications; Step 2: using the molybdenum rod sintered in step 1 as an electrode, and preparing a casting billet by vacuum consumable smelting; Step 3: Use bidirectional extrusion technology to extrude rods of different sizes (with a tolerance of 0-5mm); Step 4: Forge the finished molybdenum rod blank using a precision forging machine.

[0007] In step 1, the molybdenum rod is prepared by powder metallurgy technology, and the size of the powder metallurgy molybdenum rod blank is designed and prepared according to the size of the finished product.

[0008] In step 1, the raw material for preparing the molybdenum rod is metal molybdenum powder, wherein the purity of the molybdenum powder is ≥99.97% and the particle size is 2μm~3μm.

[0009] The cold isostatic pressing pressure of powder metallurgy is 200MPa~220MPa, the diameter of the finished molybdenum rod is 110mm~120mm, and the sintering temperature is 1800℃.

[0010] In step 2, the molybdenum rod sintered in step 1 is used as an electrode, and vacuum consumable smelting is used to prepare a cast billet; during smelting, the electrode group is first placed in a vacuum consumable electrode arc furnace for the first smelting to obtain a first cast billet; then the first cast billet is used as an electrode for the second vacuum consumable smelting, and is smelted in a vacuum consumable electrode arc furnace to obtain a second cast billet; by analogy, the nth cast billet is used as an electrode for the n+1th vacuum consumable smelting, and finally the n+1th cast billet is smelted in a vacuum consumable electrode arc furnace as the cast billet n+1; the number of vacuum consumable smelting is not less than 3 times; wherein n is a positive integer, and n≥2.

[0011] The vacuum consumable melting is preferably performed three times.

[0012] In step 3, the ingot prepared in step 2 is extruded into a rod of a specified size (with a tolerance of 0-5 mm) by bidirectional extrusion technology, and the bidirectional extrusion temperature is 1200°C.

[0013] In step 4, the fine forging temperature is 1200°C and the deformation is greater than 40%.

[0014] The design concept of the present invention is: using molybdenum rods prepared by powder metallurgy as electrodes, preparing them into casting billets by vacuum consumable smelting, and then extruding them into billets of different sizes by bidirectional extrusion technology; finally, forging them into finished billets by a precision forging machine to achieve the preparation of homogeneous and dense billets.

[0015] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0016] The process flow of the present invention is simple, and a homogeneous and dense molybdenum rod blank can be prepared. The homogeneity is achieved through multi-pass vacuum consumable smelting, and the problem of poor density is solved by adopting bidirectional extrusion technology combined with precision forging machine forging; in addition, the density of conventional powder metallurgy molybdenum rod blanks is only 98% of the theoretical density at most. The method provided by the present invention can improve the density of molybdenum rod blanks, and the maximum density can reach 99.03% of the theoretical density. At the same time, the process and method provided by the present invention can also be extended to the production of other types of products, and the prospects are broad. DETAILED DESCRIPTION

[0017] In the specific implementation process, the present invention proposes a method for preparing a large-sized homogeneous and dense molybdenum rod blank, which comprises the following steps in sequence:

[0018] Step 1: Molybdenum rods of different specifications are prepared by pressing and sintering metal molybdenum powder with a diameter of 2 μm to 3 μm and a purity of ≥99.97% at a powder metallurgy temperature of 1800°C, a sintering time of 30 hours, and a cold isostatic pressing pressure of 200 MPa to 220 MPa using powder metallurgy technology.

[0019] Step 2, using the molybdenum rod sintered in step 1 as an electrode, and preparing a cast billet by vacuum consumable smelting; during smelting, firstly put the electrode group into a vacuum consumable electrode arc furnace for the first smelting to obtain a first cast billet; then use the first cast billet as an electrode for the second vacuum consumable smelting, and smelt it in a vacuum consumable electrode arc furnace to obtain a second cast billet; and so on, use the nth cast billet as an electrode for the n+1th vacuum consumable smelting, and finally smelt the n+1th cast billet in a vacuum consumable electrode arc furnace as the n+1th cast billet; the number of vacuum consumable smelting is not less than 3 times; wherein n is a positive integer, and n≥2; the number of vacuum consumable smelting is preferably 3 times.

[0020] Step 3: Use bidirectional extrusion technology to extrude rods of different sizes (with a tolerance of 0-5 mm) at 1200°C.

[0021] Step 4: Use a precision forging machine to perform precision forging at 1200°C, with a precision forging deformation greater than 40%, to forge a finished bar blank with a diameter of 110mm~120mm.

[0022] Below, the present invention is further described in conjunction with the following examples.

[0023] Embodiment 1:

[0024] In this embodiment, a method for preparing a large-sized homogeneous and dense molybdenum rod blank comprises the following steps:

[0025] Step 1: Molybdenum rods of different specifications are prepared by pressing and sintering using powder metallurgy technology: Molybdenum powder with a particle size of 2 microns is used, the cold isostatic pressing pressure is 200 MPa, and the powder is sintered at 1800° C. for 30 hours.

[0026] Step 2, using the molybdenum rod sintered in step 1 as an electrode, and preparing a casting billet by vacuum consumable melting: vacuum consumable melting is performed 3 times, during melting, the electrode group is first placed in a vacuum consumable electrode arc furnace for the first melting; then the first casting billet is used as an electrode for the second vacuum consumable melting, and is melted in a vacuum consumable electrode arc furnace to obtain a second billet; the second billet is used as an electrode for the third vacuum consumable melting, and finally the third billet is melted in a vacuum consumable electrode arc furnace as the final casting billet, to obtain a rod billet with a diameter of 300 mm.

[0027] Step 3: Use bidirectional extrusion technology to extrude rods of different sizes (with a tolerance of 0-5 mm): bidirectional extrusion is performed at 1200° C. to prepare rods with a diameter of 190 mm.

[0028] Step 4: Forge the finished rod blank by using a GFM precision forging machine: Precision forging is performed at 1200° C. to obtain a finished molybdenum rod blank with a diameter of 110 mm.

[0029] The final test results of grain size and density are as follows:

[0030] 1. Molybdenum rod with diameter of 110mm and grain size of grade 4.

[0031] 2. Density of rod blank: 10.18g / cm 3 (The theoretical density of molybdenum is 10.28g / cm 3 ), reaching 99.03% of the theoretical density.

[0032] Embodiment 2:

[0033] In this embodiment, a method for preparing a large-sized homogeneous and dense molybdenum rod blank comprises the following steps:

[0034] Step 1: Molybdenum rods of different specifications are prepared by pressing and sintering using powder metallurgy technology: Molybdenum powder with a particle size of 3 microns is used, the cold isostatic pressing pressure is 220 MPa, and the sintering is carried out at 1800°C for 30 hours.

[0035] Step 2, using the molybdenum rod sintered in step 1 as an electrode, and preparing a cast billet by vacuum consumable smelting: vacuum consumable 3 times, during smelting, first put the electrode group into a vacuum consumable electrode arc furnace for the first smelting; then use the first cast billet as the electrode for the second vacuum consumable smelting, and smelt the second billet in the vacuum consumable electrode arc furnace; use the second billet as the electrode for the third vacuum consumable smelting, and finally smelt the third billet in the vacuum consumable electrode arc furnace as the final cast billet, to obtain a rod billet with a diameter of 320 mm.

[0036] Step 3: Use bidirectional extrusion technology to extrude rods of different sizes (with a tolerance of 0-5 mm): bidirectional extrusion at 1200° C. to form rods with a diameter of 205 mm.

[0037] Step 4: Forge the finished molybdenum bar blank by using a GFM precision forging machine: Forge the finished molybdenum bar blank at 1200° C. to a finished bar blank with a diameter of 120 mm.

[0038] The final test results of grain size and density are as follows:

[0039] 1. Molybdenum rod with a diameter of 120mm and a grain size of grade 4.

[0040] 2. Density of the rod blank is 10.15g / cm 3 (The theoretical density of molybdenum is 10.28g / cm 3 ), reaching 98.74% of the theoretical density.

[0041] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing large-sized homogeneous and dense molybdenum rod blanks, characterized in that: The following steps are included in sequence: Step 1. Prepare molybdenum rods of different specifications by pressing and sintering using powder metallurgy technology; Step 2. Using the molybdenum rod sintered in step 1 as an electrode, a casting billet is prepared by vacuum consumable smelting; Step 3. Use bidirectional extrusion technology to extrude into rods of different sizes; wherein the tolerance of the rods is 0-5mm; Step 4. Forge the finished molybdenum rod blank using a precision forging machine.

2. The method for preparing a large-sized homogeneous and dense molybdenum rod blank according to claim 1, characterized in that: In step 1, the molybdenum rod is prepared by powder metallurgy technology, and the size of the powder metallurgy molybdenum rod blank is designed and prepared according to the size of the finished product.

3. The method for preparing a large-sized homogeneous and dense molybdenum rod blank according to claim 1, characterized in that: In step 1, the raw material for preparing the molybdenum rod is metal molybdenum powder, wherein the purity of the molybdenum powder is ≥99.97% and the particle size is 2μm~3μm.

4. The method for preparing a large-sized homogeneous and dense molybdenum rod blank according to claim 1, characterized in that: In step 1, during the powder metallurgy process, the cold isostatic pressing pressure is 200MPa~220MPa, the diameter of the finished molybdenum rod is 110mm~120mm, and the sintering temperature is 1800℃.

5. The method for preparing a large-sized homogeneous and dense molybdenum rod blank according to claim 1, characterized in that: In step 2, the molybdenum rod sintered in step 1 is used as an electrode, and vacuum consumable smelting is used to prepare a cast billet; during smelting, the electrode group is first placed in a vacuum consumable electrode arc furnace for the first smelting to obtain a first cast billet; then the first cast billet is used as an electrode for the second vacuum consumable smelting, and is smelted in a vacuum consumable electrode arc furnace to obtain a second cast billet; by analogy, the nth cast billet is used as an electrode for the n+1th vacuum consumable smelting, and finally the n+1th cast billet is smelted in a vacuum consumable electrode arc furnace as the cast billet n+1; the number of vacuum consumable smelting is not less than 3 times; wherein n is a positive integer, and n≥2.

6. The method for preparing a large-sized homogeneous and dense molybdenum rod blank according to claim 5, characterized in that: The number of vacuum consumable melting is 3 times.

7. The method for preparing a large-sized homogeneous and dense molybdenum rod blank according to claim 1, characterized in that: In step 3, the biaxial extrusion temperature is 1200°C.

8. The method for preparing a large-sized homogeneous and dense molybdenum rod blank according to claim 1, characterized in that: In step 4, the finishing forging temperature is 1200° C., and the finishing forging deformation is greater than 40%.

Citation Information

Patent Citations

  • A method for preparing high-performance molybdenum cake by smelting

    CN102259182A

  • Mo-Si-B-Hf-Al alloy bar and preparation method thereof

    CN105714169A

  • Preparation method of titanium-molybdenum alloy

    CN110551919A

  • Molybdenum-rhenium alloy rod and pipe processing technology

    CN116809682A

  • Molybdenum-based alloy

    US4370299A