Multifunctional building material integrated forming process

By using a multi-functional building material integrated molding process, employing multi-layer composite structures and nanomaterials, the problems of low processing efficiency and limited functionality of existing building materials are solved, resulting in high-efficiency, multi-functional, and environmentally friendly building materials suitable for the diverse needs of modern architecture.

CN119017625AInactive Publication Date: 2024-11-26孙东
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411216637.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-31
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing integrated building material molding processes suffer from low processing efficiency, limited functionality, insufficient structural stability, poor environmental performance, and a lack of intelligent functions, making it difficult to meet the diverse needs of modern architecture.

Method used

Employing a multifunctional building material integrated molding process, this method involves selecting substrates, bio-based composite materials, aerogels, phase change materials, nanomaterials, and carbon nanotube fibers, followed by vacuum mixing, layered injection molding, and rapid curing. Combined with an electrochromic coating and an antibacterial self-cleaning nano-coating, a multi-layered composite structure is formed.

Benefits of technology

It significantly improves processing efficiency, realizes the multi-functionality of materials, including mechanical strength, heat insulation, antibacterial and intelligent dimming functions, improves environmental performance, and meets the high standards required for modern buildings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119017625A_ABST
    Figure CN119017625A_ABST
Patent Text Reader

Abstract

The invention relates to the field of building material manufacturing, and discloses a multifunctional building material integrated forming process which comprises the following steps: S1, selecting a base material, a bio-based composite material, aerogel, a phase change material, a nano material and carbon nanotube fibers, and mixing in proportion; s2, mixing the materials in a vacuum stirrer, defoaming, mixing by using a ball mill, and uniformly dispersing the reinforced fibers and the nano material by using shearing equipment; s3, a mold is preheated, an antibacterial self-cleaning coating is coated, materials with different proportions are injected into the mold in a layered mode, layer-by-layer rapid curing is conducted, and then main curing is conducted; s4, stress release treatment is conducted in the finished product cooling process; and S5, surface coating treatment and edge sealing reinforcement are conducted, and the edge of a finished product is reinforced through UV curing and hot pressing. Through the steps of layered injection molding, rapid curing and the like, the processing efficiency of the material is remarkably improved, and meanwhile, the nano material and the reinforced fibers are adopted, so that various properties of the material are enhanced, the production process is simplified, and the production cost is effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building material manufacturing, in particular to a multifunctional building material integrated molding process. Background Art

[0002] Building materials (building materials) refer to various materials and products used in construction projects. They constitute the main structure and interior decoration of the building. There are many types of building materials, which are mainly divided into three categories: structural materials, functional materials and decorative materials. Structural materials include concrete, steel, wood, bricks and stones, etc., which are mainly used for the load-bearing and support of buildings; functional materials include thermal insulation materials, waterproof materials, sound insulation materials, etc., which are used to enhance the performance of buildings; decorative materials such as coatings, tiles, floors, etc., are used to improve the appearance and internal environment of buildings. In order to give building materials multiple functions, we may use an integrated process to manufacture the corresponding building materials, but there are still some inconveniences in the existing integrated process.

[0003] First, in the existing integrated building material molding process, there are problems such as low processing efficiency, single function, insufficient structural stability, lack of environmental protection performance and intelligent functions. The traditional material production process usually adopts simple mechanical mixing and single-layer structure molding methods, which leads to uneven material properties, especially in the dispersion of reinforcing fibers and nanomaterials. It is difficult to achieve the ideal effect, which not only limits the strength, durability and functionality of the material, but also significantly reduces the production efficiency. In addition, the process is complicated and inefficient, which makes the production cost high, especially in large-scale applications, the cost problem is more prominent;

[0004] Secondly, most existing building materials are single-function materials, such as cement boards or polymer boards, which can only provide limited functions, such as mechanical strength or thermal insulation performance, and it is difficult to meet multiple functional requirements at the same time. In complex building environments, this means that a combination of multiple different materials is required to achieve comprehensive functions, thereby increasing the complexity and cost of construction. Single-layer structural materials are prone to deformation, cracking or fatigue damage when subjected to external pressure or long-term use. Especially under climate change or mechanical stress, the durability and stability of the materials are obviously insufficient. These materials are gradually exposed in modern buildings. The limitation of being difficult to meet diverse needs;

[0005] Finally, most existing materials are made of synthetic polymers or metal materials, which have a great negative impact on the environment during production and use, and it is difficult to meet the requirements of green buildings. In addition, the intelligent dimming function is rarely used in existing building materials. Traditional methods that rely on physical shading or optical coatings cannot dynamically adjust the light transmittance and it is difficult to achieve energy-saving effects. The antibacterial properties of building materials in public places are also insufficient, making it difficult to ensure public health safety. Therefore, there is an urgent need for a building material that can significantly improve processing efficiency, integrate multiple functions, improve environmental protection performance, and have intelligent dimming and antibacterial functions to meet the diverse and high-standard needs of modern buildings. Summary of the invention

[0006] In view of the deficiencies of the prior art, the present invention provides an integrated molding process for multifunctional building materials, which solves the problems of low production efficiency and high cost.

[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions: a multifunctional building material integrated molding process, comprising the following steps:

[0008] S1. Material selection and preparation: select 40-60 parts of substrate, 10-20 parts of bio-based composite materials, 5-15 parts of aerogel, 5-10 parts of phase change material, 2-8 parts of nanomaterials and 3-10 parts of carbon nanotube fibers;

[0009] S2. Material pretreatment and mixing: Pour the prepared materials into a vacuum mixer in proportion for mixing, stirring and degassing. After processing for 5 to 15 minutes, use a ball mill to control the temperature at 20°C to 50°C and mix for 30 to 120 minutes. Use a shear mixing device to evenly disperse the reinforcing fibers and nanomaterials, and shear for 10 to 30 minutes.

[0010] S3, mold processing and molding: preheat the mold to 50-150°C, and apply 0.01mm-0.05mm antibacterial self-cleaning nano coating on the mold surface, and then use multiple injection molding method to inject materials of different proportions into the mold in layers, and control the injection amount of each layer of material to 10%-30% of the overall material thickness. After each layer is injected, heat the temperature to 50°C-100°C for rapid curing, and then perform main curing at a temperature of 100°C-200°C to obtain the finished product;

[0011] S4, post-curing and stress release treatment: the finished product is placed in an open space and gradually cooled at a rate of 1°C / min to 5°C / min until the material temperature drops to room temperature, and stress release treatment is performed during the cooling process, wherein the stress release treatment includes placing the material on a vibration platform and performing low-frequency vibration treatment for 30min to 120min;

[0012] S5. Surface treatment and edge banding reinforcement: Use spraying equipment to apply intelligent dimming surface coating with a thickness of 0.1mm to 1mm to the formed building materials, and use UV curing equipment to cure for 5-15 seconds. Then, the edges of the finished products are banded and reinforced. The coating and reinforcement material method is used for treatment. The edge banding material can be a nano-composite material with antibacterial function, and is reinforced by hot pressing equipment at a pressure of 50-100MPa.

[0013] Preferably, the nanomaterial in step S1 includes nano-titanium dioxide, silver nanoparticles and carbon nanotubes, and the addition ratio of the nano-titanium dioxide, silver nanoparticles and carbon nanotubes is 1.75:0.5:2.5.

[0014] Preferably, the ratio in step S2 is that the pressure of the vacuum mixer is set to -0.05MPa to -0.1MPa, the stirring rate of the ball mill is set to 800RPM to 2000RPM, and the rotation speed of the mixing shearing device is set to 1000RPM to 3000RPM.

[0015] Preferably, in step S3, the coating contains nano-titanium dioxide and silver nano-particles, and the addition ratio of the nano-titanium dioxide and silver nano-particles is 2:0.5.

[0016] Preferably, in the step S3, the rapid curing time is 3 min to 10 min, and the main curing time is 20 min to 60 min.

[0017] Preferably, in step S4, the vibration frequency of the vibration platform is 10 Hz to 50 Hz.

[0018] Preferably, in the step S5, the smart dimming surface coating is an electrochromic material, the electrochromic material includes tungsten oxide and molybdenum oxide, the addition ratio of tungsten oxide and molybdenum oxide is 5:1.5, the wavelength of the UV curing device is 365nm-405nm, and the power density is set to 100mW / cm 2 ~200mW / cm 2 .

[0019] Preferably, the materials with different proportions in step S3 include the following layers:

[0020] Substrate layer: mainly composed of substrate, supplemented by a small amount of reinforcing fiber and nanomaterials, with the substrate accounting for 85% to 90% and the reinforcing fiber and nanomaterials accounting for 5% to 10%;

[0021] Thermal insulation layer: mainly composed of aerogel or phase change material, accounting for 70% to 80%, substrate and reinforcing fiber accounting for 15% to 20%, and nanomaterials accounting for 5% to 10%;

[0022] Surface functional layer: mainly nanomaterials and reinforcing fibers, with nanomaterials accounting for 40% to 50%, reinforcing fibers accounting for 30% to 40%, and substrates accounting for 10% to 20%;

[0023] Structural reinforcement layer: mainly reinforced fiber, accounting for 60% to 70%, base material accounting for 20% to 30%, and nanomaterials accounting for 5% to 10%;

[0024] Appearance layer: mainly composed of substrate and a small amount of nanomaterials, with the substrate accounting for 90% to 95% and the nanomaterials accounting for 5% to 10%.

[0025] Preferably, in step S3, the method for coating the reinforcing material comprises the following steps:

[0026] S31. Material selection: Nano-silver composite polymer and reinforced fiber composite material;

[0027] S32, coating process: evenly coat the reinforcing material on the edge of the finished product, and the coating thickness is controlled between 0.1mm and 0.5mm;

[0028] S33, curing: After coating, it is quickly cured by UV equipment to make the reinforcing material closely bonded with the substrate and improve the strength and wear resistance of the edge.

[0029] The present invention provides a multifunctional building material integrated molding process, which has the following beneficial effects:

[0030] 1. The present invention significantly improves the processing efficiency of materials through the steps of vacuum stirring and mixing, layered injection molding and rapid solidification. At the same time, the precise dispersion and addition of nanomaterials and reinforcing fibers not only enhance the various properties of the materials, but also simplify the production process and effectively reduce the production cost.

[0031] 2. The present invention uses a combination of multi-layer composite structures and multifunctional materials to enable building materials to have multiple functions such as excellent mechanical strength, heat insulation, antibacterial, and self-cleaning. The reasonable configuration of the substrate layer, heat insulation layer, surface functional layer, structural reinforcement layer, and appearance layer ensures that the material maintains the stability and durability of the overall structure while providing multiple functions.

[0032] 3. The present invention uses electrochromic coatings, antibacterial self-cleaning nano coatings and bio-based composite materials, which not only enable building materials to have intelligent dimming functions, but also improve the environmental performance of the materials. The electrochromic materials enable buildings to adjust light transmittance according to changes in light, thereby saving energy, while the application of nano-silver antibacterial materials enhances the safety of building materials in public places, meeting the needs of modern green buildings. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1is a process flow chart of the present invention;

[0034] Figure 2 The coating process flow chart of the present invention. DETAILED DESCRIPTION

[0035] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Example 1: Intelligent dimming and high-strength antibacterial building materials

[0037] step:

[0038] S1. Material selection and preparation:

[0039] Substrate: 60 parts of high-strength bio-based composite materials were selected;

[0040] Aerogel: 10 parts, providing thermal insulation;

[0041] Phase change material: 5 parts, used to adjust the temperature;

[0042] Nanomaterials: 5 parts of nano titanium dioxide, 3 parts of silver nanoparticles;

[0043] Carbon nanotube fiber: 10 parts, used to enhance the mechanical properties of the material;

[0044] S2. Material pretreatment and mixing:

[0045] Pour the above materials into a vacuum mixer according to proportion, control the vacuum degree at -0.08MPa, and stir for 10 minutes;

[0046] Use a ball mill to mix, control the temperature at 30°C, and mix for 60 minutes;

[0047] The reinforcing fibers and nanomaterials are uniformly dispersed by a shear mixing device and sheared for 20 minutes;

[0048] S3, mold processing and molding:

[0049] Preheat the mold to 100°C and apply 0.03mm antibacterial self-cleaning nano coating;

[0050] The substrate layer (60 parts of substrate) was injected into the mold and cured for 5 minutes;

[0051] Inject the insulation material (80% aerogel) into the mold and cure for 5 minutes;

[0052] Inject the surface functional layer (mainly nanomaterials and carbon nanotube fibers) into the mold and cure for 3 minutes;

[0053] The main curing temperature is controlled at 150°C and the curing time is 40 minutes;

[0054] S4, post-curing and stress release treatment:

[0055] The samples were gradually cooled at a rate of 3°C / min, with a vibration frequency of 20 Hz for 60 minutes;

[0056] S5. Surface treatment and edge reinforcement:

[0057] Use electrochromic material for smart dimming surface coating, the ratio of tungsten oxide to molybdenum oxide is 5:1.5, and the coating thickness is 0.5mm;

[0058] Through UV curing equipment (wavelength 365nm, power 150mW / cm 2 )Cure for 10 seconds;

[0059] The edges of the finished products were coated with a nano-silver composite material with a coating thickness of 0.2 mm and cured for 10 minutes.

[0060] Summarize:

[0061] This embodiment realizes multiple functions of building materials such as intelligent dimming, antibacterial and high mechanical strength by introducing electrochromic coating, antibacterial nano coating and high-strength carbon nanotube fiber, and is an ideal choice for public place buildings.

[0062] Example 2: Highly efficient heat insulation and self-cleaning environmentally friendly building materials

[0063] step:

[0064] S1. Material selection and preparation:

[0065] Base material: 50 parts recycled polymer composite;

[0066] Aerogel: 15 parts, providing thermal insulation;

[0067] Phase change material: 10 parts, used to adjust the temperature;

[0068] Nanomaterials: 2 parts of nano titanium dioxide, 1 part of silver nanoparticles;

[0069] Carbon nanotube fiber: 5 parts, used to enhance the mechanical properties of the material;

[0070] S2. Material pretreatment and mixing:

[0071] Pour the above materials into a vacuum mixer according to proportion, control the vacuum degree at -0.1MPa, and stir for 15 minutes;

[0072] Use a ball mill to mix, control the temperature at 40°C, and mix for 90 minutes;

[0073] The reinforcing fibers and nanomaterials are uniformly dispersed by a shear mixing device and sheared for 30 minutes;

[0074] S3, mold processing and molding:

[0075] Preheat the mold to 120°C and apply a 0.04mm antibacterial self-cleaning nano coating;

[0076] Inject the thermal insulation layer (70% aerogel) into the mold and cure for 8 minutes;

[0077] Inject the structural reinforcement layer material (mainly reinforced fiber) into the mold and cure for 5 minutes;

[0078] The main curing temperature is controlled at 180°C and the curing time is 50 minutes;

[0079] S4, post-curing and stress release treatment:

[0080] The samples were gradually cooled at a rate of 2°C / min, with a vibration frequency of 30 Hz for 90 minutes;

[0081] S5. Surface treatment and edge reinforcement:

[0082] The surface was treated with a self-cleaning coating with a ratio of 2:0.5 between nano-titanium dioxide and silver nanoparticles and a coating thickness of 0.3 mm;

[0083] Through UV curing equipment (wavelength 405nm, power 100mW / cm 2 )Cure for 12 seconds;

[0084] The edges of the finished products were coated with reinforced fibers with a thickness of 0.4 mm and cured for 15 minutes.

[0085] Summarize:

[0086] This embodiment significantly improves the thermal insulation performance and self-cleaning function of the building material by adopting an aerogel insulation layer and a nano self-cleaning coating. At the same time, the use of recycled polymers improves the environmental performance of the material, making it suitable for energy-saving buildings.

[0087] Example 3: Building materials optimized for durability and light management

[0088] step:

[0089] S1. Material selection and preparation:

[0090] Base material: 45 parts high strength polymer base material;

[0091] Aerogel: 10 parts, providing thermal insulation;

[0092] Phase change material: 5 parts, used to adjust the temperature;

[0093] Nanomaterials: 4 parts of nano titanium dioxide, 2 parts of silver nanoparticles;

[0094] Carbon nanotube fiber: 7 parts, used to enhance the mechanical properties of the material;

[0095] S2. Material pretreatment and mixing:

[0096] Pour the materials into a vacuum mixer, control the vacuum degree at -0.09MPa, and stir for 12 minutes;

[0097] Use a ball mill to mix, control the temperature at 25°C, and mix for 60 minutes;

[0098] The reinforcing fibers and nanomaterials are uniformly dispersed by a shear mixing device and sheared for 20 minutes;

[0099] S4, mold processing and molding:

[0100] Preheat the mold to 80°C and apply 0.02mm antibacterial self-cleaning nano coating;

[0101] The substrate layer (45 parts of substrate) was injected into the mold and cured for 5 minutes;

[0102] Inject the surface functional layer material (mainly nanomaterial) into the mold and cure for 7 minutes;

[0103] The main curing temperature is controlled at 160°C and the curing time is 30 minutes;

[0104] S4, post-curing and stress release treatment:

[0105] The samples were gradually cooled at a rate of 4°C / min, with a vibration frequency of 15 Hz for 60 min;

[0106] S5. Surface treatment and edge reinforcement:

[0107] The surface is treated with intelligent dimming coating, the ratio of tungsten oxide to molybdenum oxide is 7:2, and the coating thickness is 0.4mm;

[0108] By UV curing equipment (wavelength 375nm, power 175mW / cm 2 ) cures for 8 seconds;

[0109] The edges of the finished products were coated with a nano-silver composite material with a coating thickness of 0.3 mm and cured for 10 minutes.

[0110] Summarize:

[0111] This embodiment significantly improves the performance of the material in light management and long-term use by optimizing light management and durability design, and is very suitable for high-strength and high-durability construction projects.

[0112] Example 4: Highly environmentally friendly and functional integrated building materials

[0113] step:

[0114] S1. Material selection and preparation:

[0115] Base material: 50 parts of recycled polymer base material;

[0116] Aerogel: 12 parts, provides thermal insulation;

[0117] Phase change material: 8 parts, used to adjust the temperature;

[0118] Nanomaterials: 3 parts of nano titanium dioxide, 1 part of silver nanoparticles;

[0119] Carbon nanotube fiber: 6 parts, used to enhance the mechanical properties of the material;

[0120] S2. Material pretreatment and mixing:

[0121] Pour the above materials into a vacuum mixer according to proportion, control the vacuum degree at -0.1MPa, and stir for 15 minutes;

[0122] The mixing was performed using a ball mill, the temperature was controlled at 35°C, and the mixing was performed for 90 minutes;

[0123] The reinforcing fibers and nanomaterials are uniformly dispersed by a shear mixing device and sheared for 25 minutes;

[0124] S3, mold processing and molding:

[0125] Preheat the mold to 110°C and apply 0.03mm antibacterial self-cleaning nano coating;

[0126] Inject the structural reinforcement layer (mainly reinforced fiber) into the mold and cure for 5 minutes;

[0127] Inject the appearance layer material (mainly base material and nanomaterial) into the mold and cure for 3 minutes;

[0128] The main curing temperature is controlled at 170°C and the curing time is 45 minutes;

[0129] S4, post-curing and stress release treatment:

[0130] The samples were gradually cooled at a rate of 3°C / min, with a vibration frequency of 40 Hz for 90 minutes;

[0131] S5. Surface treatment and edge reinforcement:

[0132] The surface is treated with an environmentally friendly self-cleaning coating, with a ratio of 3:1 between nano-titanium dioxide and silver nanoparticles and a coating thickness of 0.5mm;

[0133] Through UV curing equipment (wavelength 395nm, power 200mW / cm 2 )Cure for 15 seconds;

[0134] The edges of the finished products were coated with reinforced fibers with a thickness of 0.4 mm and cured for 15 minutes.

[0135] Summarize:

[0136] This embodiment combines high environmental protection and multifunctional integration. The material adopts recycled polymers and green production processes while achieving high-efficiency thermal insulation, self-cleaning and antibacterial properties, and is particularly suitable for environmentally friendly building projects.

[0137] Example 5: Multi-layer structure and all-round protection building materials

[0138] step:

[0139] S1. Material selection and preparation:

[0140] Substrate: 55 parts bio-based composites;

[0141] Aerogel: 10 parts, providing thermal insulation;

[0142] Phase change material: 7 parts, used to adjust temperature;

[0143] Nanomaterials: 4 parts of nano titanium dioxide, 2 parts of silver nanoparticles;

[0144] Carbon nanotube fiber: 8 parts, used to enhance the mechanical properties of the material;

[0145] S2. Material pretreatment and mixing:

[0146] Pour the above materials into a vacuum mixer according to proportion, control the vacuum degree at -0.09MPa, and stir for 12 minutes;

[0147] Use a ball mill to mix, control the temperature at 40°C, and mix for 60 minutes;

[0148] The reinforcing fibers and nanomaterials are uniformly dispersed by a shear mixing device and sheared for 20 minutes;

[0149] S3, mold processing and molding

[0150] Preheat the mold to 120°C and apply 0.02mm antibacterial self-cleaning nano coating;

[0151] The substrate layer (55 parts of substrate) was injected into the mold and cured for 5 minutes;

[0152] Inject the insulation material (mainly aerogel) into the mold and cure for 5 minutes;

[0153] Inject the surface functional layer material (mainly nanomaterial) into the mold and cure for 3 minutes;

[0154] The main curing temperature is controlled at 180°C and the curing time is 50 minutes;

[0155] S4, post-curing and stress release treatment:

[0156] The sample was gradually cooled at a rate of 1°C / min, the vibration frequency was 30 Hz, and the vibration treatment lasted for 120 minutes;

[0157] S5. Surface treatment and edge reinforcement:

[0158] The surface is treated with intelligent dimming coating, the ratio of tungsten oxide to molybdenum oxide is 6:2, and the coating thickness is 0.4mm;

[0159] Through UV curing equipment (wavelength 365nm, power 175mW / cm 2 ) cures for 8 seconds;

[0160] The edges of the finished products were coated with a nano-silver composite material with a coating thickness of 0.3 mm and cured for 10 minutes.

[0161] Summarize:

[0162] This embodiment achieves high-efficiency performance of the material in different environments through multi-layer structural design and all-round protection, including thermal insulation, antibacterial, self-cleaning and intelligent dimming functions. It is an ideal choice for construction projects with high requirements for the environment and climate change.

[0163] Summary:

[0164] These five embodiments demonstrate the diverse performance of the integrated molding process of multifunctional building materials in different application scenarios. By adjusting the material proportions, process parameters and structural design, it is possible to integrate multiple functions such as intelligent dimming, high strength, antibacterial, heat insulation, self-cleaning and environmental protection. These embodiments are not only suitable for ordinary construction projects, but can also meet the needs of public places, high-performance buildings, energy-saving and environmentally friendly buildings, and construction projects that meet the needs of complex environments, reflecting the wide applicability and superior performance of the present invention.

[0165] Test experiment 1: Mechanical strength test (compressive strength test)

[0166] Testing process:

[0167] Sample preparation: Samples of the same size (100 mm x 100 mm x 100 mm) were cut from each example.

[0168] Test equipment: Use universal testing machine for compressive strength test.

[0169] Test steps:

[0170] S1. Place the sample on the testing machine platform;

[0171] S2. Apply pressure gradually and record the maximum pressure of the sample (maximum pressure before failure);

[0172] S3. Data recording: record the compressive strength of each sample in MPa.

[0173] Test data:

[0174]

[0175]

[0176] Test results:

[0177] Example 5 exhibits the highest compressive strength, indicating that its multi-layer structure design is effective in enhancing the mechanical strength of the material. Example 1 and Example 3 also have high compressive strengths and are suitable for application in high-strength building scenarios.

[0178] Test experiment 2: thermal insulation performance test

[0179] Testing process:

[0180] Sample preparation: Samples of the same size (100 mm x 100 mm x 10 mm) were cut from each example.

[0181] Test equipment: Use a thermal conductivity tester to measure the thermal conductivity of the sample.

[0182] Test steps:

[0183] S1. Fix the sample on the tester and set the temperature difference (for example, room temperature and high temperature side 100°C);

[0184] S2. Record thermal conductivity in W / m·K.

[0185] S3. Data recording: record the thermal conductivity of each sample.

[0186] Test data:

[0187] Example Thermal conductivity (W / m·K) Embodiment 1 0.035 Embodiment 2 0.030 Embodiment 3 0.040 Embodiment 4 0.025 Embodiment 5 0.032

[0188] Test results:

[0189] Example 4 exhibits the lowest thermal conductivity, indicating that it has the best thermal insulation performance and is particularly suitable for buildings that require efficient thermal insulation. Example 2 also has a relatively low thermal conductivity, demonstrating its advantage in thermal insulation performance.

[0190] Test experiment three: antibacterial performance test

[0191] Testing process:

[0192] Sample preparation: Samples of the same size (50 mm x 50 mm x 5 mm) were cut from each example.

[0193] Test equipment: Use an antibacterial test box to conduct bacterial culture experiments.

[0194] Test steps:

[0195] S1. Inoculate common bacteria (such as Escherichia coli) on the sample surface;

[0196] S2, placing the sample in an antimicrobial test chamber and culturing it for 24 hours;

[0197] S3. Record the inhibition rate of bacterial growth.

[0198] Data recording: Inhibition rate is expressed as a percentage.

[0199] Test data:

[0200] Example Inhibition rate (%) Embodiment 1 98 Embodiment 2 85 Embodiment 3 95 Embodiment 4 88 Embodiment 5 97

[0201] Test results:

[0202] Example 1 exhibits the highest antibacterial performance, with a bacteria inhibition rate close to 100%, and is suitable for use in places with high hygiene requirements. Example 5 also exhibits relatively high antibacterial performance.

[0203] Test experiment 4: Intelligent dimming performance test

[0204] Testing process:

[0205] Sample preparation: Samples of the same size (100 mm x 100 mm x 3 mm) were cut from each example and processed with the smart dimming coating.

[0206] Test equipment: Use a light intensity tester to measure changes in light transmittance.

[0207] Test steps:

[0208] S1. Test the light transmittance of the sample at different voltages (e.g., 0V, 3V, 5V);

[0209] S2, record the change of transmittance under different voltages;

[0210] S3. Data recording: The change in transmittance is expressed as a percentage.

[0211] Test data:

[0212] Example Transmittance change (%) Embodiment 1 70 Embodiment 2 60 Embodiment 3 75 Embodiment 4 55 Embodiment 5 80

[0213] Test results:

[0214] The fifth embodiment shows the best intelligent dimming performance, has the largest change in transmittance, and can better adapt to light changes. The performances of the third and first embodiments are also good.

[0215] Test experiment 5: Self-cleaning ability test

[0216] Testing process:

[0217] Sample preparation: Samples of the same size (100 mm x 100 mm x 5 mm) were cut from each example and subjected to the self-cleaning coating treatment.

[0218] Test equipment: simulate the dust and stains in the natural environment, and use water to flush the experimental device.

[0219] Test steps:

[0220] S1. Sprinkle standard dust and stain solution on the sample surface;

[0221] S2. Use a water flushing device to simulate rainwater flushing and record the stain removal rate;

[0222] S3. Data recording: The stain removal rate is expressed as a percentage.

[0223] Test data:

[0224]

[0225]

[0226] Test results:

[0227] Example 5 exhibits the best self-cleaning ability and the highest stain removal rate, and the self-cleaning performance of Example 1 and Example 4 is also quite outstanding.

[0228] Summary

[0229] Example 1 exhibits excellent antibacterial properties and high mechanical strength, and also has excellent self-cleaning ability, and is suitable for public places and building environments with high hygiene requirements.

[0230] The second embodiment has outstanding performance in thermal insulation and environmental protection, but is relatively weak in intelligent dimming and antibacterial performance, and is suitable for energy-saving and environmentally friendly buildings.

[0231] The third embodiment performs well in terms of intelligent dimming and mechanical strength, has a relatively balanced overall performance, and is suitable for use in multifunctional buildings.

[0232] The fourth embodiment has the best thermal insulation performance and is suitable for buildings with high-efficiency thermal insulation, but its other performances are relatively average.

[0233] Example 5 performed outstandingly in almost all tests, especially in terms of intelligent dimming, self-cleaning and antibacterial properties, and is suitable for high-demand multifunctional building applications.

[0234] Overall summary: Example 5 exhibits the most comprehensive and excellent performance and is suitable for high-performance, multi-functional construction projects; while other embodiments excel in certain specific performances and are suitable for special application scenarios. Through these experiments, we can clearly identify the advantages and disadvantages of different material combinations in practical applications, which helps to select the most suitable building materials according to actual needs.

[0235] Comparative experiment 1: Mechanical strength and durability comparison experiment

[0236] Existing technical solutions:

[0237] Existing building materials usually adopt a single-layer structure, mainly based on traditional cement substrates or polymer substrates, with a small amount of reinforcing fibers or fillers added to improve strength. Common single-layer structural materials have certain limitations in pressure resistance and bending resistance, and are prone to fatigue and damage, especially under long-term loads or external forces.

[0238] Technical solution of the present invention:

[0239] The present invention adopts a multi-layer composite structure, utilizing a combination of a substrate layer, a reinforcing fiber layer, an aerogel layer, and a structural reinforcement layer, so that the material has high strength and high durability, and the addition of nanomaterials further improves the toughness and fatigue resistance of the material.

[0240] Comparison process design:

[0241] Sample preparation:

[0242] Prior art sample: a single layer of cement-based material with 5% glass fiber added, size 100mmx100mmx10mm;

[0243] The sample of the present invention adopts a multi-layer composite structure, with the specific proportions being: 60 parts of substrate layer, 10 parts of reinforcing fiber layer, 10 parts of aerogel layer, and 5 parts of nanomaterial, with a size of 100mmx100mmx10mm.

[0244] Test items and parameters:

[0245] Compressive strength: Use a universal testing machine to gradually increase the pressure and record the compressive strength of the sample (MPa);

[0246] Bending strength: Use a three-point bending tester to measure the bending strength of the sample (MPa);

[0247] Fatigue test: Use a fatigue testing machine to perform repeated loading under constant pressure and record the fatigue life (number of cycles) of the sample.

[0248] Experimental data table:

[0249]

[0250] Experimental results:

[0251] The multilayer composite structure sample of the present invention is significantly higher in compressive strength and flexural strength than the prior art samples, and in particular exhibits a longer life in fatigue tests, demonstrating its excellent mechanical properties and durability.

[0252] Comparative experiment 2: Comparative experiment on thermal insulation and temperature regulation performance

[0253] Existing technical solutions:

[0254] Traditional building materials mostly use a single material layer, such as polystyrene foam, ordinary concrete, etc. These materials have limited thermal insulation performance and lack active temperature regulation function. They usually can only rely on the low thermal conductivity of the material itself to achieve thermal insulation effect.

[0255] Technical solution of the present invention:

[0256] The multifunctional building material of the present invention uses aerogel as the main thermal insulation layer and integrates phase change material for active temperature regulation. Aerogel has extremely low thermal conductivity, while phase change material can absorb or release heat, thereby greatly improving thermal insulation and temperature regulation performance.

[0257] Comparison process design:

[0258] Sample preparation:

[0259] Prior art sample: using polystyrene foam board, thickness 10mm;

[0260] The sample of the present invention adopts a multi-layer structure, mainly composed of aerogel layer (15 parts) and phase change material (10 parts), with a thickness of 10 mm.

[0261] Test items and parameters:

[0262] Thermal conductivity test: Use a thermal conductivity tester to measure the thermal conductivity (W / m·K) of the sample;

[0263] Temperature regulation ability test: A temperature sensor is built into the sample to measure the rate and magnitude of change of the sample's internal temperature when the ambient temperature changes;

[0264] Environmental simulation test: Place the sample in an environmental simulation chamber to simulate the temperature difference between day and night, and record the temperature difference between the inside and outside of the sample (℃).

[0265] Experimental data table:

[0266]

[0267]

[0268] Experimental results:

[0269] The thermal conductivity of the sample of the present invention is significantly lower than that of the prior art sample, and it shows better temperature stability and higher internal and external temperature difference in the temperature regulation ability test, indicating that it has obvious advantages in heat insulation and temperature regulation.

[0270] Comparative experiment 3: Self-cleaning and antibacterial performance comparison experiment

[0271] Existing technical solutions:

[0272] Conventional building materials are usually treated with ordinary coatings. These coatings do not have self-cleaning properties and have limited antibacterial properties. Dirt and bacteria are easily attached, especially in humid environments, where mold and stains are easily generated on the surface of the materials.

[0273] Technical solution of the present invention:

[0274] The multifunctional building material surface coating of the present invention adopts a self-cleaning antibacterial coating containing nano titanium dioxide and silver nanoparticles. The nano titanium dioxide provides a photocatalytic self-cleaning function, and the silver nanoparticles give the coating antibacterial properties.

[0275] Comparison process design:

[0276] Sample preparation:

[0277] Prior art sample: substrate coated with common architectural paint, size 100mmx100mm;

[0278] The sample of the present invention is a substrate coated with a self-cleaning antibacterial coating containing nano-titanium dioxide and silver nanoparticles, with a size of 100 mm x 100 mm.

[0279] Test items and parameters:

[0280] Self-cleaning ability test: Spray stain solution on the sample surface to simulate dust and stains in the natural environment, rinse with a water flow flushing device, and measure the stain removal rate (%);

[0281] Antibacterial performance test: Escherichia coli was inoculated on the surface of the sample and the antibacterial rate (%) was measured after 24 hours of incubation;

[0282] Durability test: simulates rain and UV exposure environment, and measures the integrity and functional retention of the coating after continuous washing and light exposure for 100 hours.

[0283] Experimental data table:

[0284] Sample type Stain removal rate (%) Antibacterial rate (%) Coating integrity (%) Function retention rate (%) Prior art samples 60 40 70 50 Sample of the present invention 95 98 95 90

[0285] Experimental results:

[0286] The samples of the present invention showed obvious advantages in the self-cleaning ability and antibacterial performance tests, with the stain removal rate and antibacterial rate being much higher than those of the prior art samples. In addition, in the durability test, the coating integrity and function retention rate of the samples of the present invention were significantly better than those of the prior art samples, indicating that they are more durable and effective in practical applications.

[0287] Summary

[0288] Through these complex comparative experiments, it is obvious that the integrated molding process of the multifunctional building materials of the present invention is superior to the existing technical solutions in terms of mechanical strength, thermal insulation performance, self-cleaning and antibacterial performance. The multi-layer composite structure design, the application of nanomaterials, and the introduction of intelligent dimming and antibacterial coatings make the building materials of the present invention perform well in a variety of environments and usage conditions, have higher durability, stability and functional integration, and adapt to the diversified demands of modern buildings for materials. These comparative experiments fully verify the innovation and superiority of the present invention and highlight its application value in the field of building materials.

[0289] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. The multifunctional building material integrated molding process is characterized by: The following steps are involved: S1. Material selection and preparation: select 40-60 parts of substrate, 10-20 parts of bio-based composite materials, 5-15 parts of aerogel, 5-10 parts of phase change material, 2-8 parts of nanomaterials and 3-10 parts of carbon nanotube fibers; S2. Material pretreatment and mixing: Pour the prepared materials into a vacuum mixer in proportion for mixing, stirring and degassing. After processing for 5 to 15 minutes, use a ball mill to control the temperature at 20°C to 50°C and mix for 30 to 120 minutes. Use a shear mixing device to evenly disperse the reinforcing fibers and nanomaterials, and shear for 10 to 30 minutes. S3, mold processing and molding: preheat the mold to 50-150°C, and apply 0.01mm-0.05mm antibacterial self-cleaning nano coating on the mold surface, and then use multiple injection molding method to inject materials of different proportions into the mold in layers, and control the injection amount of each layer of material to 10%-30% of the overall material thickness. After each layer is injected, heat the temperature to 50°C-100°C for rapid curing, and then perform main curing at a temperature of 100°C-200°C to obtain the finished product; S4, post-curing and stress release treatment: the finished product is placed in an open space and gradually cooled at a rate of 1°C / min to 5°C / min until the material temperature drops to room temperature, and stress release treatment is performed during the cooling process, wherein the stress release treatment includes placing the material on a vibration platform and performing low-frequency vibration treatment for 30min to 120min; S5. Surface treatment and edge banding reinforcement: Use spraying equipment to apply intelligent dimming surface coating with a thickness of 0.1mm to 1mm to the formed building materials, and use UV curing equipment to cure for 5-15 seconds. Then, the edges of the finished products are banded and reinforced. The coating and reinforcement material method is used for treatment. The edge banding material can be a nano-composite material with antibacterial function, and is reinforced by hot pressing equipment at a pressure of 50-100MPa.

2. The multifunctional building material integrated molding process according to claim 1, characterized in that: The nanomaterials in step S1 include nano-titanium dioxide, silver nanoparticles and carbon nanotubes, and the addition ratio of the nano-titanium dioxide, silver nanoparticles and carbon nanotubes is 1.75:0.5:2.

5.

3. The multifunctional building material integrated molding process according to claim 1, characterized in that: The proportions in the step S2 are as follows: the pressure of the vacuum mixer is set to -0.05MPa to -0.1MPa, the stirring rate of the ball mill is set to 800RPM to 2000RPM, and the rotation speed of the mixing shearing device is set to 1000RPM to 3000RPM.

4. The multifunctional building material integrated molding process according to claim 1, characterized in that: In the step S3, the coating contains nano titanium dioxide and silver nanoparticles, and the addition ratio of the nano titanium dioxide and silver nanoparticles is 2:0.

5.

5. The multifunctional building material integrated molding process according to claim 1, characterized in that: In the step S3, the rapid curing time is 3 minutes to 10 minutes, and the main curing time is 20 minutes to 60 minutes.

6. The multifunctional building material integrated molding process according to claim 1, characterized in that: In the step S4, the vibration frequency of the vibration platform is 10 Hz to 50 Hz.

7. The multifunctional building material integrated molding process according to claim 1, characterized in that: In the step S5, the intelligent dimming surface coating is an electrochromic material, which includes tungsten oxide and molybdenum oxide, and the addition ratio of tungsten oxide and molybdenum oxide is 5:1.

5. The wavelength of the UV curing device is 365nm-405nm, and the power density is set to 100mW / cm 2 ~200mW / cm 2 .

8. The multifunctional building material integrated molding process according to claim 1, characterized in that: The materials with different proportions in step S3 include the following layers: Substrate layer: mainly composed of substrate, supplemented by a small amount of reinforcing fiber and nanomaterials, with the substrate accounting for 85% to 90% and the reinforcing fiber and nanomaterials accounting for 5% to 10%; Thermal insulation layer: mainly composed of aerogel or phase change material, accounting for 70% to 80%, substrate and reinforcing fiber accounting for 15% to 20%, and nanomaterials accounting for 5% to 10%; Surface functional layer: mainly nanomaterials and reinforcing fibers, with nanomaterials accounting for 40% to 50%, reinforcing fibers accounting for 30% to 40%, and substrates accounting for 10% to 20%; Structural reinforcement layer: mainly reinforced fiber, accounting for 60% to 70%, base material accounting for 20% to 30%, and nanomaterials accounting for 5% to 10%; Appearance layer: mainly composed of substrate and a small amount of nanomaterials, with the substrate accounting for 90% to 95% and the nanomaterials accounting for 5% to 10%.

9. The multifunctional building material integrated molding process according to claim 1, characterized in that: In step S3, the method for coating the reinforcement material comprises the following steps: S31. Material selection: Nano-silver composite polymer and reinforced fiber composite material; S32, coating process: evenly coat the reinforcing material on the edge of the finished product, and the coating thickness is controlled between 0.1mm and 0.5mm; S33, curing: After coating, it is quickly cured by UV equipment to make the reinforcing material closely bonded with the substrate and improve the strength and wear resistance of the edge.