Preparation method of holographic layer, holographic IMR membrane, air conditioner holographic IMR panel and air conditioner
The heat resistance and compatibility problems of the IMR diaphragm molded layer and evaporated layer are solved through ultraviolet radiation grafting of cycloolefin copolymer and maleic anhydride and ultraviolet radiation polymerization of nano zinc sulfide and vinyl acetate. , holographic layer preparation with high light transmittance and molding performance is achieved, reducing process costs and substrate damage.
Patent Information
- Application Number
- CN202310588995.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-23
AI Technical Summary
The molded layer and vapor deposition layer of the existing IMR diaphragm have problems with heat resistance, light transmittance and toughness. The vapor deposition process is high and the process is complex, which has great damage to the substrate and poor compatibility with the substrate.
UV irradiation grafting is used for cycloolefin copolymer and maleic anhydride as the molding layer, and nano zinc sulfide and vinyl acetate mixed solution as the vapor deposition layer. The molding of the holographic layer is achieved through ultraviolet radiation polymerization, replacing the traditional molding Process plus evaporation process to reduce substrate damage.
The excellent flatness, gloss, high light transmittance and molding performance of the holographic layer are achieved, reducing the preparation cost, simplifying the process flow, and reducing damage to the substrate.
Smart Images

Figure CN119017738A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of in-mold decoration, and in particular relates to a method for preparing a holographic layer, a holographic IMR film, an air-conditioning holographic IMR panel and an air-conditioning. Background Art
[0002] In-mold transfer (IMR) technology usually uses polyethylene terephthalate (PET) as the main substrate, prints decorative patterns and various functional coatings on the substrate, and uses a precise positioning film feeding device to feed the roll into a special mold for injection molding, and transfers the pattern on the substrate to the surface of the plastic part. The decorative effect and injection molding are integrated into one, with the advantages of rich pattern effects and easy replacement. Ordinary IMR films are composed of a substrate layer, a release layer, a protective layer, a pattern layer, an adhesive layer, etc. Bright or gorgeous effects can quickly attract users, so introducing holographic technology into IMR films, that is, adding a holographic layer to ordinary IMR films, helps to improve the appearance of the product.
[0003] The holographic layer of an IMR film generally consists of a molded layer and an evaporation layer, wherein the molded layer acts as a grating for recording information, and the evaporation layer mainly acts as a reflection / refraction layer; when light is incident on the surface of the IMR film, the light is controlled by the combined action of the molded layer grating and the evaporation layer, thereby displaying a holographic effect. Therefore, the molded layer needs to have a high light transmittance to facilitate the entry of light, and also needs to have high heat resistance and high toughness to facilitate high-temperature molding processes; the evaporation layer requires a high refractive index / reflectivity. However, the commonly used polyethylene terephthalate (PET) substrate has the problem of poor heat resistance, polymethyl methacrylate (PMMA) has the problem of high light transmittance but poor toughness, cycloolefin copolymer has the problem of low surface energy and reaction inertness, and difficulty in copolymerization and grafting with other polymers; the evaporation layer is generally made of aluminum, but has the problems of high cost, complex process, and damage to the substrate, and zinc sulfide as an evaporation layer has the problem of poor compatibility between zinc sulfide and the substrate. Summary of the invention
[0004] In view of the above-mentioned problems existing in the prior art, the present invention proposes a method for preparing a holographic layer, a holographic IMR film, an air conditioner holographic IMR panel and an air conditioner, wherein the holographic layer material has excellent flatness, glossiness, high light transmittance and molding performance, realizes one-piece molding by molding, and has a simple preparation process and low industrial cost, replacing the traditional molding process plus evaporation process, reducing the damage of the evaporation process to the substrate.
[0005] In order to achieve the above object, the present invention provides a method for preparing a holographic layer, comprising the following steps:
[0006] The preparation steps of the cycloolefin copolymer and the maleic anhydride prepolymer are as follows: pre-treating the cycloolefin copolymer film, coating it with a mixed solution of maleic anhydride and a photocatalyst, and then pre-polymerizing it by ultraviolet irradiation to prepare the cycloolefin copolymer and the maleic anhydride prepolymer;
[0007] The steps of preparing the mixed solution of nano zinc sulfide and vinyl acetate are as follows: firstly preparing nano zinc sulfide particles, and then preparing the mixed solution of nano zinc sulfide and vinyl acetate;
[0008] The steps of preparing the holographic layer by molding are as follows: coating a mixture of nano zinc sulfide and vinyl acetate on cycloolefin copolymer and maleic anhydride prepolymer, polymerizing by ultraviolet irradiation, then ultrasonically cleaning with acetone, and molding to prepare the holographic layer.
[0009] In some of the embodiments, in the step of preparing the cycloolefin copolymer and the maleic anhydride prepolymer, the step of pretreating the cycloolefin copolymer film is to immerse the cycloolefin copolymer film in an acetone solution at 40° C. to 60° C. for 10 min to 30 min.
[0010] In some embodiments, in the step of preparing the cycloolefin copolymer and the maleic anhydride prepolymer, the method for preparing the maleic anhydride and photocatalyst mixed solution includes taking 50g to 350g of maleic anhydride and 1000g of xylene under light-proof conditions, adding 1g to 10g of photoinitiator benzophenone, and stirring evenly until all dissolved to obtain a mixed solution. It is understood that according to actual conditions, those skilled in the art can adjust the amount of each component within the above range, for example, the amount of maleic anhydride can also be 50g, 100g, 150g, 200g, 250g, 300g, 350g or any point value within the above range, and the amount of benzophenone can also be 1g, 2g, 3g, 4g, 5g, 6g, 7g, 8g, 9g, 10g or any point value within the above range.
[0011] In some embodiments, in the step of preparing the cycloolefin copolymer and the maleic anhydride prepolymer, when the ultraviolet light is irradiated for prepolymerization, the ultraviolet light wavelength is set to 254 nm and the irradiation intensity is set to 6000 uW / cm 2 ~8000uW / cm 2 , the irradiation time is set to 3s~10s.
[0012] In some of the embodiments, in the step of preparing the mixed solution of nano zinc sulfide and vinyl acetate, the preparation method of the nano zinc sulfide particles includes: first weighing 408g of zinc chloride and 4056g of thiourea and adding them into a reaction kettle, then adding 21000g of diethylenetriamine, stirring for 20min, ultrasonically dispersing for 15min, then stirring again for 20min, heating to 160°C to 180°C, refluxing for 12h, washing with deionized water and anhydrous ethanol, centrifuging, and vacuum drying to obtain nano zinc sulfide particles.
[0013] In some of the embodiments, in the step of preparing the nano zinc sulfide and vinyl acetate mixed solution, 200g to 350g of nano zinc sulfide particles are taken, 300g to 450g of vinyl acetate and 1000g of xylene are added, and after ultrasonication for 15min to 20min, stirring is performed for 10min to 20min, and 5g to 15g of photoinitiator benzophenone is added while stirring to obtain a nano zinc sulfide and vinyl acetate mixed solution. It is understandable that according to actual conditions, those skilled in the art can adjust the amount of each component within the above range. For example, the amount of nano zinc sulfide particles can also be 200g, 210g, 220g, 230g, 240g, 250g, 260g, 270g, 280g, 290g, 300g, 310g, 320g, 330g, 340g, 350g or any point value within the above range, and the amount of vinyl acetate can also be The amount of benzophenone can be 300g, 310g, 320g, 330g, 340g, 350g, 360g, 370g, 380g, 390g, 400g, 410g, 420g, 430g, 440g, 450g or any point value within the above range. The amount of benzophenone can also be 5g, 6g, 7g, 8g, 9g, 10g, 11g, 12g, 13g, 14g, 15g or any point value within the above range.
[0014] In some embodiments, in the holographic layer molding preparation step, when the ultraviolet light irradiation polymerization is performed, the ultraviolet light wavelength is set to 254nm and the irradiation intensity is set to 6000uW / cm 2 ~8000uW / cm 2 , the irradiation time is set to 10s~30s.
[0015] The present invention also provides a holographic IMR film, comprising a film layer, a release layer, a UV protective layer, a holographic layer, a logo layer, a protective layer, a pigment layer and an adhesive layer stacked in sequence, wherein the holographic layer is prepared by the above-mentioned holographic layer preparation method.
[0016] The present invention also provides an air conditioner holographic IMR panel, which is prepared by injection molding the holographic IMR film.
[0017] The present invention also provides an air conditioner, comprising the above-mentioned air conditioner holographic IMR panel.
[0018] Compared with the prior art, the advantages and positive effects of the present invention are:
[0019] 1. The present invention obtains a holographic layer by ultraviolet irradiation grafting of a cycloolefin copolymer film and maleic anhydride as a molding layer, and uses a mixed solution of nano zinc sulfide and vinyl acetate as a medium layer with a reflection / refraction effect. The mixed solution is uniformly coated on the prepolymerized cycloolefin copolymer film and then subjected to ultraviolet irradiation polymerization and molding to form an integral body. The holographic layer replaces the traditional molding process plus evaporation process, reduces the damage of the evaporation process to the substrate, and the prepared holographic layer material has excellent flatness, glossiness, high light transmittance and molding performance.
[0020] 2. The present invention prepares cycloolefin copolymer and maleic anhydride prepolymer, first pretreats the cycloolefin copolymer film, then coats the mixed solution of maleic anhydride and photocatalyst, and performs ultraviolet light irradiation prepolymerization, which can overcome the problem of difficult copolymerization and grafting of cycloolefin copolymer and other polymers; specifically, due to the low surface energy and reaction inertness of cycloolefin copolymer, in the technical scheme of the present invention, first immerses the cycloolefin copolymer film in acetone solution, which can increase the surface roughness of the cycloolefin copolymer and is conducive to the formation of grafting sites; ultraviolet light is a high-energy light, and the use of ultraviolet light irradiation to initiate polymerization reaction can effectively control the degree of polymerization, and has the characteristics of fast speed, economy and environmental protection, wide applicability, mildness and controllability, etc.
[0021] 3. When preparing nano zinc sulfide particles according to the present invention, diethylenetriamine is added to increase the content of two-dimensional flaky zinc sulfide, thereby increasing the refractive index / reflectivity; a mixed solution of nano zinc sulfide and vinyl acetate is prepared, and vinyl acetate and nano zinc sulfide are mixed and coated. Since vinyl acetate contains unsaturated double bonds and has the ability of addition reaction and polymerization reaction, it can be polymerized with maleic anhydride, thereby increasing the compatibility and bonding strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 A flow chart of the preparation process of the holographic layer provided in an embodiment of the present invention;
[0023] Figure 2 A schematic diagram of the structure of an IMR diaphragm provided in an embodiment of the present invention;
[0024] Among them, 1. film layer, 2. release layer, 3. UV protection layer, 4. holographic layer, 5. protection layer, 6. pigment layer, 7. bonding layer. DETAILED DESCRIPTION
[0025] In order to be able to understand the characteristics and technical contents of the embodiments of the present invention in more detail, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the embodiments described below are only part of the embodiments of the present invention, rather than all the embodiments of the present invention. In the following technical description, for the convenience of explanation, a full understanding of the disclosed embodiments is provided through multiple details. However, one or more embodiments can still be implemented without these details. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection requested by the present invention.
[0026] The embodiment of the present invention provides a method for preparing a holographic layer, a holographic IMR film, a panel and an air conditioner. The present invention uses ultraviolet radiation grafting of a cycloolefin copolymer film and maleic anhydride to perform prepolymerization as a molding layer, uses a mixed solution of nano zinc sulfide and vinyl acetate as a medium layer that plays a reflective / refractive role, and evenly applies the mixed solution to the prepolymerized cycloolefin copolymer film, then performs ultraviolet radiation polymerization, and performs molding and integrated molding to obtain a holographic layer. Among them, ultraviolet radiation graft polymerization has the advantages of fast reaction speed, simple operation, no damage to the substrate body, and precise control of reaction time and area, and is suitable for surface modification of polymer substrates. The holographic layer material prepared by the technical solution of the present invention not only has excellent flatness, glossiness, high light transmittance and molding performance, but also realizes molding and integrated molding, has a simple preparation process, and has a low industrial cost. It replaces the traditional molding process plus evaporation process, and reduces the damage of the evaporation process to the substrate.
[0027] The method for preparing the holographic layer of the present invention comprises the following steps:
[0028] The preparation steps of cyclic olefin copolymer and maleic anhydride prepolymer are as follows: a certain mass of cyclic olefin copolymer (COC) film is placed in an acetone solution at 40° C. to 60° C. and immersed for 10 min to 30 min for pretreatment;
[0029] Take 50g-350g of maleic anhydride (MAH) and 1000g of xylene under light-proof conditions, add 1g-10g of photoinitiator benzophenone (BP), and stir evenly until all are dissolved to obtain a mixed solution;
[0030] The mixed solution is uniformly coated on the pretreated cycloolefin copolymer (COC) film, and ultraviolet light is irradiated and grafted to obtain cycloolefin copolymer and maleic anhydride prepolymer, wherein the ultraviolet light wavelength is set to 254nm and the irradiation intensity is set to 6000uW / cm 2 ~8000uW / cm 2 , the irradiation time is set to 3s~10s;
[0031] Preparation steps of nano zinc sulfide and vinyl acetate mixed solution: first weigh 408g zinc chloride (ZnCl2) and 4056g thiourea and add them into a reactor, then add 21000g diethylenetriamine (DETA), stir for 20min, then perform ultrasonic dispersion for 15min, then stir again for 20min, heat to 160℃~180℃, reflux for 12h, wash with deionized water and anhydrous ethanol, centrifuge, and vacuum dry to obtain nano zinc sulfide particles;
[0032] Take 200g-350g of the above-mentioned nano zinc sulfide particles, add 300g-450g of vinyl acetate (VAc) and 1000g of xylene, ultrasonically treat for 15min-20min, stir for 10min-20min, and add 5g-15g of photoinitiator benzophenone (BP) while stirring to obtain a mixed solution of nano zinc sulfide and vinyl acetate;
[0033] Holographic layer molding preparation steps: uniformly coating the mixed solution of nano zinc sulfide and vinyl acetate on the surface of cycloolefin copolymer and maleic anhydride prepolymer, polymerizing by ultraviolet irradiation, ultrasonic cleaning with acetone for 1min to 5min, and molding to prepare the holographic layer, wherein the ultraviolet wavelength is set to 254nm, and the irradiation intensity is set to 6000uW / cm 2 ~8000uW / cm 2 , the irradiation time is set to 10s~30s.
[0034] Cyclic olefin copolymer (COC) has the advantages of high light transmittance, high heat resistance, high glass transition temperature, high toughness, low density and easy processing, among which, the light transmittance of cyclic olefin copolymer (COC) is comparable to that of polymethyl methacrylate (PMMA), which can reach more than 92%; the heat resistance of cyclic olefin copolymer (COC) is higher than that of polycarbonate (PC); the glass transition temperature of cyclic olefin copolymer (COC) is 100°C to 163°C. In the preparation step of cyclic olefin copolymer and maleic anhydride prepolymer of the present invention, the cyclic olefin copolymer (COC) used has a high glass transition temperature, preferably 150°C to 163°C; the maleic anhydride (MAH) used contains unsaturated double bonds and anhydride with extremely strong reactivity, and the brand is commercially available.
[0035] The photoinitiator benzophenone (BP) belongs to the Norrish II type photoinitiator. The initiation mechanism is as follows: under the irradiation of ultraviolet light, benzophenone first transitions from the ground state to the singlet state ([BP]S), and then to the triplet state ([BP]T) through intersystem crossing. After capturing the hydrogen atoms on the surface of the cycloolefin copolymer substrate, surface free radicals and benzophenone semi-pinacol free radicals are generated. The surface free radicals can further initiate the graft polymerization reaction of the monomer, while the semi-pinacol free radical has a large steric hindrance effect due to its benzene ring structure, so it cannot be used to initiate the chain growth reaction. The chain termination reaction mainly comes from the diradical termination between the chain growth free radicals, the diradical termination between the chain growth free radical and the semi-pinacol free radical, or the diradical termination between two semi-pinacol free radicals. However, the diradical termination between the chain growth free radical and the semi-pinacol free radical belongs to the dormant species. When the light is re-applied, the dormant species will break off and regenerate the chain growth free radical to continue to initiate the chain growth reaction.
[0036] Zinc sulfide (ZnS) is a high refractive index crystal with a refractive index as high as 4.1 to 4.4, and zinc sulfide has almost no absorption in the visible light region, and can be used to replace the aluminum vapor deposition layer to achieve the refraction / reflection function. In the preparation step of the nano zinc sulfide and vinyl acetate mixed solution of the present invention, diethylenetriamine (DETA) is added to increase the content of two-dimensional flaky zinc sulfide, and the two-dimensional flaky zinc sulfide is beneficial to improve the refraction / reflectivity. Since vinyl acetate contains unsaturated double bonds and has the ability of addition reaction and polymerization reaction, cycloolefin copolymer and maleic anhydride are prepolymerized, and vinyl acetate is mixed and coated with nano zinc sulfide particles and then polymerized with maleic anhydride, which can improve compatibility and bonding strength.
[0037] The present invention also provides a holographic IMR film, comprising a film layer, a release layer, a UV protective layer, a holographic layer, a protective layer, a pigment layer and an adhesive layer stacked in sequence, wherein the holographic layer is prepared by the above method, and the holographic layer is prepared by curing, drying and other processes to obtain the holographic IMR film.
[0038] The present invention also provides an air conditioner holographic IMR panel, which is prepared by using the above-mentioned holographic IMR film. Specifically, the holographic IMR film is sent into a panel mold by a precise positioning film feeding device for injection molding to prepare the air conditioner holographic IMR panel.
[0039] The present invention also provides an air conditioner, comprising the above-mentioned air conditioner holographic IMR panel.
[0040] In order to more clearly and in detail introduce the preparation method of the holographic layer, the holographic MIR film, the panel and the air conditioner provided in the embodiments of the present invention, they will be described in conjunction with specific embodiments below, wherein Table 1 is the raw material formula of Examples 1-6 and Comparative Examples 1-5, and Table 2 is the process conditions of the preparation method of Examples 1-6 and Comparative Examples 1-5.
[0041] Example 1
[0042] The method for preparing the holographic layer in this embodiment comprises the following steps:
[0043] The preparation steps of cycloolefin copolymer and maleic anhydride prepolymer are as follows: pre-treating the cycloolefin copolymer film by immersing it in a 40°C acetone solution for 30 minutes; taking 50g of maleic anhydride and 1000g of xylene under light-proof conditions, adding 1g of photoinitiator benzophenone, and stirring evenly until all are dissolved to obtain a mixed solution; evenly coating the mixed solution on the pre-treated cycloolefin copolymer film, and performing ultraviolet light irradiation grafting to obtain the cycloolefin copolymer and maleic anhydride prepolymer, wherein the ultraviolet light wavelength is set to 254nm, and the irradiation intensity is set to 6000uW / cm 2 , the irradiation time was set to 3s;
[0044] The steps for preparing the mixed solution of nano zinc sulfide and vinyl acetate are as follows: 408g of zinc chloride and 4056g of thiourea are weighed and added into a reactor, 21000g of diethylenetriamine is added, and the mixture is ultrasonically dispersed for 15min after stirring for 20min, and then stirred again for 20min, heated to 160°C, refluxed for 12h, washed with deionized water and anhydrous ethanol, centrifuged, and vacuum dried to obtain nano zinc sulfide particles; 200g of the above nano zinc sulfide particles are taken, 300g of vinyl acetate and 1000g of xylene are added, ultrasonically treated for 15min, stirred for 10min, and 5g of photoinitiator benzophenone is added while stirring to obtain a mixed solution of nano zinc sulfide and vinyl acetate;
[0045] Holographic layer molding preparation steps: evenly coating the mixed solution of nano zinc sulfide and vinyl acetate on the surface of cycloolefin copolymer and maleic anhydride prepolymer, polymerizing by ultraviolet irradiation, ultrasonic cleaning with acetone for 1 minute, and molding to prepare the holographic layer, wherein the ultraviolet wavelength is set to 254nm, and the irradiation intensity is set to 6000uW / cm 2 , the irradiation time was set to 10s.
[0046] Example 2
[0047] The method for preparing the holographic layer in this embodiment comprises the following steps:
[0048] The preparation steps of cycloolefin copolymer and maleic anhydride prepolymer are as follows: pre-treating the cycloolefin copolymer film by immersing it in a 50°C acetone solution for 20 minutes; taking 150g of maleic anhydride and 1000g of xylene under light-proof conditions, adding 3g of photoinitiator benzophenone, and stirring evenly until all are dissolved to obtain a mixed solution; evenly coating the mixed solution on the pre-treated cycloolefin copolymer film, and performing ultraviolet light irradiation grafting to obtain the cycloolefin copolymer and maleic anhydride prepolymer, wherein the ultraviolet light wavelength is set to 254nm, and the irradiation intensity is set to 6400uW / cm 2 , the irradiation time was set to 5s;
[0049] The steps for preparing a mixed solution of nano zinc sulfide and vinyl acetate are as follows: 408 g of zinc chloride and 4056 g of thiourea are weighed and added into a reactor, 21000 g of diethylenetriamine is added, the mixture is stirred for 20 min, ultrasonically dispersed for 15 min, and then stirred again for 20 min, heated to 163° C., refluxed for 12 h, washed with deionized water and anhydrous ethanol, centrifuged, and vacuum dried to obtain nano zinc sulfide particles; 220 g of the above nano zinc sulfide particles are taken, 330 g of vinyl acetate and 1000 g of xylene are added, ultrasonically treated for 16 min, stirred for 12 min, and 7 g of a photoinitiator benzophenone is added while stirring to obtain a mixed solution of nano zinc sulfide and vinyl acetate;
[0050] Holographic layer molding preparation steps: evenly coating the mixed solution of nano zinc sulfide and vinyl acetate on the surface of cycloolefin copolymer and maleic anhydride prepolymer, polymerizing by ultraviolet irradiation, ultrasonic cleaning with acetone for 2 minutes, and molding to prepare the holographic layer, wherein the ultraviolet wavelength is set to 254nm, and the irradiation intensity is set to 6400uW / cm 2 , the irradiation time was set to 14s.
[0051] Example 3
[0052] The method for preparing the holographic layer in this embodiment comprises the following steps:
[0053] The preparation steps of cycloolefin copolymer and maleic anhydride prepolymer are as follows: pre-treating the cycloolefin copolymer film by immersing it in an acetone solution at 60°C for 10 minutes; taking 200g of maleic anhydride and 1000g of xylene under light-proof conditions, adding 5g of photoinitiator benzophenone, and stirring evenly until all are dissolved to obtain a mixed solution; evenly coating the mixed solution on the pre-treated cycloolefin copolymer film, and performing ultraviolet light irradiation grafting to obtain the cycloolefin copolymer and maleic anhydride prepolymer, wherein the ultraviolet light wavelength is set to 254nm, and the irradiation intensity is set to 6900uW / cm 2 , the irradiation time was set to 7s;
[0054] The steps for preparing a mixed solution of nano zinc sulfide and vinyl acetate are as follows: 408 g of zinc chloride and 4056 g of thiourea are weighed and added into a reactor, 21000 g of diethylenetriamine is added, the mixture is stirred for 20 min, ultrasonically dispersed for 15 min, and then stirred again for 20 min, heated to 167° C., refluxed for 12 h, washed with deionized water and anhydrous ethanol, centrifuged, and vacuum dried to obtain nano zinc sulfide particles; 250 g of the above nano zinc sulfide particles are taken, 350 g of vinyl acetate and 1000 g of xylene are added, ultrasonically treated for 17 min, stirred for 14 min, and 9 g of a photoinitiator benzophenone is added while stirring to obtain a mixed solution of nano zinc sulfide and vinyl acetate;
[0055] Holographic layer molding preparation steps: evenly coating the mixed solution of nano zinc sulfide and vinyl acetate on the surface of cycloolefin copolymer and maleic anhydride prepolymer, polymerizing by ultraviolet irradiation, ultrasonic cleaning with acetone for 3 minutes, and molding to prepare the holographic layer, wherein the ultraviolet wavelength is set to 254nm, and the irradiation intensity is set to 6900uW / cm 2 , the irradiation time was set to 17s.
[0056] Example 4
[0057] The method for preparing the holographic layer in this embodiment comprises the following steps:
[0058] The preparation steps of cycloolefin copolymer and maleic anhydride prepolymer are as follows: pre-treating the cycloolefin copolymer film by immersing it in a 50°C acetone solution for 20 minutes; taking 250g of maleic anhydride and 1000g of xylene under light-proof conditions, adding 7g of photoinitiator benzophenone, and stirring evenly until all are dissolved to obtain a mixed solution; evenly coating the mixed solution on the pre-treated cycloolefin copolymer film, and performing ultraviolet light irradiation grafting to obtain the cycloolefin copolymer and maleic anhydride prepolymer, wherein the ultraviolet light wavelength is set to 254nm, and the irradiation intensity is set to 7300uW / cm 2 , the irradiation time was set to 8s;
[0059] The steps for preparing a mixed solution of nano zinc sulfide and vinyl acetate are as follows: 408 g of zinc chloride and 4056 g of thiourea are weighed and added into a reactor, 21000 g of diethylenetriamine is added, the mixture is stirred for 20 min, ultrasonically dispersed for 15 min, and then stirred again for 20 min, heated to 171° C., refluxed for 12 h, washed with deionized water and anhydrous ethanol, centrifuged, and vacuum dried to obtain nano zinc sulfide particles; 280 g of the above nano zinc sulfide particles are taken, 380 g of vinyl acetate and 1000 g of xylene are added, ultrasonically treated for 18 min, stirred for 16 min, and 11 g of a photoinitiator benzophenone is added while stirring to obtain a mixed solution of nano zinc sulfide and vinyl acetate;
[0060] Holographic layer molding preparation steps: the mixture of nano zinc sulfide and vinyl acetate is evenly coated on the surface of cycloolefin copolymer and maleic anhydride prepolymer, and then ultraviolet light is irradiated and polymerized, and then ultrasonic cleaning is performed with acetone for 4 minutes, and molding is performed to prepare the holographic layer, wherein the ultraviolet light wavelength is set to 254nm, and the irradiation intensity is set to 7300uW / cm 2 , the irradiation time was set to 20s.
[0061] Example 5
[0062] The method for preparing the holographic layer in this embodiment comprises the following steps:
[0063] The preparation steps of cycloolefin copolymer and maleic anhydride prepolymer are as follows: pre-treating a cycloolefin copolymer film by immersing it in an acetone solution at 50°C for 20 minutes; taking 300g of maleic anhydride and 1000g of xylene under light-proof conditions, adding 8g of photoinitiator benzophenone, and stirring evenly until all are dissolved to obtain a mixed solution; evenly coating the mixed solution on the pre-treated cycloolefin copolymer film, and performing ultraviolet light irradiation grafting to obtain a cycloolefin copolymer and a maleic anhydride prepolymer, wherein the ultraviolet light wavelength is set to 254nm, and the irradiation intensity is set to 7600uW / cm 2 , the irradiation time was set to 9s;
[0064] The steps for preparing a mixed solution of nano zinc sulfide and vinyl acetate are as follows: 408 g of zinc chloride and 4056 g of thiourea are weighed and added into a reactor, 21000 g of diethylenetriamine is added, the mixture is stirred for 20 min, ultrasonically dispersed for 15 min, and then stirred again for 20 min, heated to 175° C., refluxed for 12 h, washed with deionized water and anhydrous ethanol, centrifuged, and vacuum dried to obtain nano zinc sulfide particles; 320 g of the above nano zinc sulfide particles are taken, 430 g of vinyl acetate and 1000 g of xylene are added, ultrasonically treated for 19 min, stirred for 18 min, and 13 g of a photoinitiator benzophenone is added while stirring to obtain a mixed solution of nano zinc sulfide and vinyl acetate;
[0065] Holographic layer molding preparation steps: evenly coating the mixed solution of nano zinc sulfide and vinyl acetate on the surface of cycloolefin copolymer and maleic anhydride prepolymer, polymerizing by ultraviolet irradiation, ultrasonic cleaning with acetone for 5 minutes, and molding to prepare the holographic layer, wherein the ultraviolet wavelength is set to 254nm, and the irradiation intensity is set to 7600uW / cm 2 , the irradiation time was set to 25s.
[0066] Example 6
[0067] The method for preparing the holographic layer in this embodiment comprises the following steps:
[0068] The preparation steps of cycloolefin copolymer and maleic anhydride prepolymer are as follows: pre-treating the cycloolefin copolymer film by immersing it in a 50°C acetone solution for 20 minutes; taking 350g of maleic anhydride and 1000g of xylene under light-proof conditions, adding 10g of photoinitiator benzophenone, and stirring evenly until all are dissolved to obtain a mixed solution; evenly coating the mixed solution on the pre-treated cycloolefin copolymer film, and performing ultraviolet light irradiation grafting to obtain the cycloolefin copolymer and maleic anhydride prepolymer, wherein the ultraviolet light wavelength is set to 254nm, and the irradiation intensity is set to 8000uW / cm 2 , the irradiation time was set to 10s;
[0069] The steps for preparing a mixed solution of nano zinc sulfide and vinyl acetate are as follows: 408 g of zinc chloride and 4056 g of thiourea are weighed and added into a reactor, 21000 g of diethylenetriamine is added, the mixture is stirred for 20 min, ultrasonically dispersed for 15 min, and then stirred again for 20 min, heated to 180° C., refluxed for 12 h, washed with deionized water and anhydrous ethanol, centrifuged, and vacuum dried to obtain nano zinc sulfide particles; 350 g of the above nano zinc sulfide particles are taken, 450 g of vinyl acetate and 1000 g of xylene are added, ultrasonically treated for 20 min, stirred for 20 min, and 15 g of a photoinitiator benzophenone is added while stirring to obtain a mixed solution of nano zinc sulfide and vinyl acetate;
[0070] Holographic layer molding preparation steps: evenly coating the mixture of nano zinc sulfide and vinyl acetate on the surface of cycloolefin copolymer and maleic anhydride prepolymer, polymerizing by ultraviolet irradiation, ultrasonic cleaning with acetone for 5 minutes, and molding to prepare the holographic layer, wherein the ultraviolet wavelength is set to 254nm, and the irradiation intensity is set to 8000uW / cm 2 , the irradiation time was set to 30s.
[0071] Comparative Example 1
[0072] The preparation method of the holographic layer of this comparative example comprises the following steps:
[0073] The preparation steps of cycloolefin copolymer and maleic anhydride prepolymer are as follows: pre-treating the cycloolefin copolymer film by immersing it in a 30°C acetone solution for 40 minutes; taking 350g of maleic anhydride and 1000g of xylene under light-proof conditions, adding 10g of photoinitiator benzophenone, and stirring evenly until all are dissolved to obtain a mixed solution; evenly coating the mixed solution on the pre-treated cycloolefin copolymer film, and performing ultraviolet light irradiation grafting to obtain the cycloolefin copolymer and maleic anhydride prepolymer, wherein the ultraviolet light wavelength is set to 254nm, and the irradiation intensity is set to 8000uW / cm 2 , the irradiation time was set to 10s;
[0074] The steps for preparing a mixed solution of nano zinc sulfide and vinyl acetate are as follows: 408 g of zinc chloride and 4056 g of thiourea are weighed and added into a reactor, 21000 g of diethylenetriamine is added, the mixture is stirred for 20 min, ultrasonically dispersed for 15 min, and then stirred again for 20 min, heated to 180° C., refluxed for 12 h, washed with deionized water and anhydrous ethanol, centrifuged, and vacuum dried to obtain nano zinc sulfide particles; 350 g of the above nano zinc sulfide particles are taken, 450 g of vinyl acetate and 1000 g of xylene are added, ultrasonically treated for 20 min, stirred for 20 min, and 15 g of a photoinitiator benzophenone is added while stirring to obtain a mixed solution of nano zinc sulfide and vinyl acetate;
[0075] Holographic layer molding preparation steps: evenly coating the mixture of nano zinc sulfide and vinyl acetate on the surface of cycloolefin copolymer and maleic anhydride prepolymer, polymerizing by ultraviolet irradiation, ultrasonic cleaning with acetone for 5 minutes, and molding to prepare the holographic layer, wherein the ultraviolet wavelength is set to 254nm, and the irradiation intensity is set to 8000uW / cm 2 , the irradiation time was set to 30s.
[0076] Comparative Example 2
[0077] The preparation method of the holographic layer of this comparative example comprises the following steps:
[0078] The preparation steps of cycloolefin copolymer and maleic anhydride prepolymer are as follows: pre-treating the cycloolefin copolymer film by immersing it in a 50°C acetone solution for 20 minutes; taking 40g of maleic anhydride and 1000g of xylene under light-proof conditions, adding 10g of photoinitiator benzophenone, and stirring evenly until all are dissolved to obtain a mixed solution; evenly coating the mixed solution on the pre-treated cycloolefin copolymer film, and performing ultraviolet light irradiation grafting to obtain the cycloolefin copolymer and maleic anhydride prepolymer, wherein the ultraviolet light wavelength is set to 254nm, and the irradiation intensity is set to 8000uW / cm 2 , the irradiation time was set to 10s;
[0079] The steps for preparing a mixed solution of nano zinc sulfide and vinyl acetate are as follows: 408 g of zinc chloride and 4056 g of thiourea are weighed and added into a reactor, 21000 g of diethylenetriamine is added, and the mixture is stirred for 20 min and then ultrasonically dispersed for 15 min, and then stirred again for 20 min, refluxed at 180° C. for 12 h, washed with deionized water and anhydrous ethanol, and centrifuged, and vacuum dried to obtain nano zinc sulfide particles; 350 g of the above nano zinc sulfide particles are taken, 450 g of vinyl acetate and 1000 g of xylene are added, ultrasonically treated for 20 min, and then stirred for 20 min, and 15 g of a photoinitiator benzophenone is added while stirring to obtain a mixed solution of nano zinc sulfide and vinyl acetate;
[0080] Holographic layer molding preparation steps: evenly coating the mixture of nano zinc sulfide and vinyl acetate on the surface of cycloolefin copolymer and maleic anhydride prepolymer, polymerizing by ultraviolet irradiation, ultrasonic cleaning with acetone for 5 minutes, and molding to prepare the holographic layer, wherein the ultraviolet wavelength is set to 254nm, and the irradiation intensity is set to 8000uW / cm 2 , the irradiation time was set to 30s.
[0081] Comparative Example 3
[0082] The preparation method of the holographic layer of this comparative example comprises the following steps:
[0083] The preparation steps of cycloolefin copolymer and maleic anhydride prepolymer are as follows: pre-treating the cycloolefin copolymer film by immersing it in a 50°C acetone solution for 20 minutes; taking 350g of maleic anhydride and 1000g of xylene under light-proof conditions, adding 10g of photoinitiator benzophenone, and stirring evenly until all are dissolved to obtain a mixed solution; evenly coating the mixed solution on the pre-treated cycloolefin copolymer film, and performing ultraviolet light irradiation grafting to obtain the cycloolefin copolymer and maleic anhydride prepolymer, wherein the ultraviolet light wavelength is set to 254nm, and the irradiation intensity is set to 8000uW / cm 2 , the irradiation time was set to 10s;
[0084] The steps for preparing a mixed solution of nano zinc sulfide and vinyl acetate are as follows: 408 g of zinc chloride and 4056 g of thiourea are weighed and added into a reactor, 21000 g of diethylenetriamine is added, the mixture is stirred for 20 min, ultrasonically dispersed for 15 min, and then stirred again for 20 min, heated to 180° C., refluxed for 12 h, washed with deionized water and anhydrous ethanol, centrifuged, and vacuum dried to obtain nano zinc sulfide particles; 180 g of the above nano zinc sulfide particles are taken, 450 g of vinyl acetate and 1000 g of xylene are added, ultrasonically treated for 20 min, stirred for 20 min, and 15 g of a photoinitiator benzophenone is added while stirring to obtain a mixed solution of nano zinc sulfide and vinyl acetate;
[0085] Holographic layer molding preparation steps: evenly coating the mixture of nano zinc sulfide and vinyl acetate on the surface of cycloolefin copolymer and maleic anhydride prepolymer, polymerizing by ultraviolet irradiation, ultrasonic cleaning with acetone for 5 minutes, and molding to prepare the holographic layer, wherein the ultraviolet wavelength is set to 254nm, and the irradiation intensity is set to 8000uW / cm 2 , the irradiation time was set to 30s.
[0086] Comparative Example 4
[0087] The preparation method of the holographic layer of this comparative example comprises the following steps:
[0088] The preparation steps of cycloolefin copolymer and maleic anhydride prepolymer are as follows: pre-treating the cycloolefin copolymer film by immersing it in a 50°C acetone solution for 20 minutes; taking 350g of maleic anhydride and 1000g of xylene under light-proof conditions, adding 10g of photoinitiator benzophenone, and stirring evenly until all are dissolved to obtain a mixed solution; evenly coating the mixed solution on the pre-treated cycloolefin copolymer film, and performing ultraviolet light irradiation grafting to obtain the cycloolefin copolymer and maleic anhydride prepolymer, wherein the ultraviolet light wavelength is set to 254nm, and the irradiation intensity is set to 6400uW / cm 2 , the irradiation time was set to 10s;
[0089] The steps for preparing the mixed solution of nano zinc sulfide and vinyl acetate are as follows: 408g of zinc chloride and 4056g of thiourea are weighed and added into a reactor, 21000g of diethylenetriamine is added, and the mixture is stirred for 20min and then ultrasonically dispersed for 15min, and then stirred again for 20min, heated to 163°C, refluxed for 12h, washed with deionized water and anhydrous ethanol, centrifuged, and vacuum dried to obtain nano zinc sulfide particles; 220g of the above nano zinc sulfide particles are taken, 200g of vinyl acetate and 1000g of xylene are added, ultrasonically treated for 16min, stirred for 12min, and 15g of photoinitiator benzophenone is added while stirring to obtain a mixed solution of nano zinc sulfide and vinyl acetate;
[0090] Holographic layer molding preparation steps: evenly coating the mixed solution of nano zinc sulfide and vinyl acetate on the surface of cycloolefin copolymer and maleic anhydride prepolymer, polymerizing by ultraviolet irradiation, ultrasonic cleaning with acetone for 2 minutes, and molding to prepare the holographic layer, wherein the ultraviolet wavelength is set to 254nm, and the irradiation intensity is set to 6400uW / cm 2 , the irradiation time was set to 30s.
[0091] Comparative Example 5
[0092] The preparation method of the holographic layer of this comparative example comprises the following steps:
[0093] The preparation steps of cycloolefin copolymer and maleic anhydride prepolymer are as follows: pre-treating the cycloolefin copolymer film by immersing it in a 50°C acetone solution for 20 minutes; taking 350g of maleic anhydride and 1000g of xylene under light-proof conditions, adding 10g of photoinitiator benzophenone, and stirring evenly until all are dissolved to obtain a mixed solution; evenly coating the mixed solution on the pre-treated cycloolefin copolymer film, and performing ultraviolet light irradiation grafting to obtain the cycloolefin copolymer and maleic anhydride prepolymer, wherein the ultraviolet light wavelength is set to 254nm, and the irradiation intensity is set to 8000uW / cm 2 , the irradiation time was set to 10s;
[0094] The steps for preparing a mixed solution of nano zinc sulfide and vinyl acetate are as follows: 408 g of zinc chloride and 4056 g of thiourea are weighed and added into a reactor, 21000 g of diethylenetriamine is added, the mixture is stirred for 20 min, ultrasonically dispersed for 15 min, and then stirred again for 20 min, heated to 180° C., refluxed for 12 h, washed with deionized water and anhydrous ethanol, centrifuged, and vacuum dried to obtain nano zinc sulfide particles; 350 g of the above nano zinc sulfide particles are taken, 450 g of vinyl acetate and 1000 g of xylene are added, ultrasonically treated for 20 min, stirred for 20 min, and 15 g of a photoinitiator benzophenone is added while stirring to obtain a mixed solution of nano zinc sulfide and vinyl acetate;
[0095] Holographic layer molding preparation steps: evenly coating the mixture of nano zinc sulfide and vinyl acetate on the surface of cycloolefin copolymer and maleic anhydride prepolymer, polymerizing by ultraviolet irradiation, ultrasonic cleaning with acetone for 5 minutes, and molding to prepare the holographic layer, wherein the ultraviolet wavelength is set to 254nm, and the irradiation intensity is set to 8000uW / cm 2 , the irradiation time was set to 5s.
[0096] Table 1 Raw material formula of Examples 1-6 and Comparative Examples 1-5 (unit: g)
[0097]
[0098]
[0099] Table 2 Process conditions of Examples 1-6 and Comparative Examples 1-5
[0100]
[0101]
[0102] Performance Testing
[0103] The holographic layers obtained in Examples 1-6 and Comparative Examples 1-5 were cured, dried and other processes to prepare holographic IMR films, and the transmittance, glossiness, adhesion, molding performance and holographic effect of the obtained holographic IMR films were evaluated respectively. The test standards are shown in Table 3, and the test results are shown in Table 4. In the performance test, the transmittance test standard refers to GB / T 2410, and the test conditions are haze meter method, in which the transmittance is affected by multiple factors such as COC immersion time, ultraviolet radiation grafting rate, zinc sulfide content, ultraviolet radiation polymerization rate, etc.; the glossiness test standard refers to GB / T 8807, and the test conditions are 60°; the adhesion test standard is GB / T 9286, and the test conditions are cross-cut test, and 3M tape test is used; the molding performance mainly checks the integrity; the holographic effect evaluation is a visual subjective evaluation.
[0104] Table 3 Holographic IMR film performance test standards
[0105] project Light transmittance Glossiness Adhesion Molding performance Holographic effect evaluation Test Standards GB / T 2410 GB / T 8807 GB / T9286 / Visual Test conditions Haze meter method 60° Cross-cut, 3M tape Check integrity Visual subjective evaluation
[0106] Table 4 Performance test results of holographic IMR films prepared by holographic layers of Examples 1-6 and Comparative Examples 1-5
[0107]
[0108]
[0109] As can be seen from the above, in Examples 1-6 of the present invention, a cycloolefin copolymer film and maleic anhydride are grafted by ultraviolet radiation for pre-polymerization as a molding layer, a mixed solution of nano zinc sulfide and vinyl acetate is used as a medium layer with a reflective / refractive effect, the mixed solution is uniformly coated on the pre-polymerized cycloolefin copolymer film, and then ultraviolet light irradiation polymerization is performed, and molding is integrated to obtain a holographic layer, and then the holographic layer is prepared by printing and other processes to obtain a holographic IMR film, the transmittance is greater than 45, the glossiness is greater than 89, the molding performance test shows that the grating transfer is complete, there is no sticking to the board, the adhesion is level 0, and the holographic effect is evaluated as excellent. Comparative Examples 1-3 and 5 correspond to Example 6, wherein, unlike Example 6, the pretreatment immersion temperature of the cycloolefin copolymer in Comparative Example 1 is lower than that in Example 6, and the immersion time is longer than that in Example 6. The light transmittance and glossiness of the holographic IMR film prepared by the obtained holographic layer are significantly lower than those in Example 6, and the grating transfer in the molding performance test is incomplete, sticking to the board, the adhesion is level 4, and the holographic effect is evaluated as poor; Unlike Example 6, the amount of maleic anhydride used in Comparative Example 2 is significantly less than that in Example 6. The light transmittance and glossiness of the holographic IMR film prepared by the obtained holographic layer are significantly lower than those in Example 6, and the grating transfer in the molding performance test is incomplete, sticking to the board, the adhesion is level 4, and the holographic effect is evaluated as poor. The grating transfer is incomplete, the plate is sticky, the adhesion is level 3, and the holographic effect is evaluated as poor; different from Example 6, the amount of nano zinc sulfide used in Comparative Example 3 is less than that in Example 6, the transmittance and glossiness of the holographic IMR film prepared by the obtained holographic layer are significantly lower than those in Example 6, and the holographic effect is evaluated as poor; different from Example 6, the irradiation time of ultraviolet light irradiation polymerization in the holographic layer molding preparation step in Comparative Example 5 is lower than that in Example 6, the transmittance and glossiness of the holographic IMR film prepared by the obtained holographic layer are significantly lower than those in Example 6, and the molding performance test shows that the grating transfer is incomplete, the plate is sticky, the adhesion is level 2, and the holographic effect is evaluated as poor.
[0110] Finally, it should be noted that the present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only the preferred feasible embodiments of the present invention, and the above-mentioned embodiments are only used to illustrate the technical scheme of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various deformations, modifications, evolutions and improvements made by ordinary technicians in this field to the technical scheme of the present invention should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing a holographic layer, characterized in that: The following steps are involved: The preparation steps of the cycloolefin copolymer and the maleic anhydride prepolymer are as follows: pre-treating the cycloolefin copolymer film, coating it with a mixed solution of maleic anhydride and a photocatalyst, and then pre-polymerizing it by ultraviolet irradiation to prepare the cycloolefin copolymer and the maleic anhydride prepolymer; The steps of preparing the mixed solution of nano zinc sulfide and vinyl acetate are as follows: firstly preparing nano zinc sulfide particles, and then preparing the mixed solution of nano zinc sulfide and vinyl acetate; The steps of preparing the holographic layer by molding are as follows: coating a mixture of nano zinc sulfide and vinyl acetate on cycloolefin copolymer and maleic anhydride prepolymer, polymerizing by ultraviolet irradiation, then ultrasonically cleaning with acetone, and molding to prepare the holographic layer.
2. The method for preparing a holographic layer according to claim 1, characterized in that: In the step of preparing the cycloolefin copolymer and the maleic anhydride prepolymer, the step of pretreating the cycloolefin copolymer film is to immerse the cycloolefin copolymer film in an acetone solution at 40° C. to 60° C. for 10 min to 30 min.
3. The method for preparing a holographic layer according to claim 1, characterized in that: In the step of preparing the cycloolefin copolymer and maleic anhydride prepolymer, the method for preparing the maleic anhydride and photocatalyst mixed solution comprises taking 50g to 350g of maleic anhydride and 1000g of xylene under light-proof conditions, adding 1g to 10g of photoinitiator benzophenone, and stirring evenly until all are dissolved to obtain a mixed solution.
4. The method for preparing a holographic layer according to claim 1, characterized in that: In the step of preparing the cycloolefin copolymer and the maleic anhydride prepolymer, when the ultraviolet light is irradiated for prepolymerization, the ultraviolet light wavelength is set to 254 nm and the irradiation intensity is set to 6000 uW / cm 2 ~8000uW / cm 2 , the irradiation time is set to 3s~10s.
5. The method for preparing a holographic layer according to claim 1, characterized in that: In the step of preparing the nano zinc sulfide and vinyl acetate mixed solution, the preparation method of the nano zinc sulfide particles comprises: first weighing 408g of zinc chloride and 4056g of thiourea and adding them into a reaction kettle, then adding 21000g of diethylenetriamine, stirring for 20min, ultrasonically dispersing for 15min, stirring again for 20min, heating to 160°C to 180°C, refluxing for 12h, washing with deionized water and anhydrous ethanol, centrifuging, and vacuum drying to obtain nano zinc sulfide particles.
6. The method for preparing a holographic layer according to claim 1, characterized in that: In the step of preparing the nano zinc sulfide and vinyl acetate mixed solution, 200 g to 350 g of nano zinc sulfide particles are taken, 300 g to 450 g of vinyl acetate and 1000 g of xylene are added, and after ultrasonication for 15 min to 20 min, stirring is performed for 10 min to 20 min, and 5 g to 15 g of photoinitiator benzophenone is added while stirring to obtain the nano zinc sulfide and vinyl acetate mixed solution.
7. The method for preparing a holographic layer according to claim 1, characterized in that: In the holographic layer molding preparation step, when ultraviolet light irradiation polymerization is performed, the ultraviolet light wavelength is set to 254nm and the irradiation intensity is set to 6000uW / cm 2 ~8000uW / cm 2 , the irradiation time is set to 10s~30s.
8. A holographic IMR film, characterized in that: It comprises a film layer, a release layer, a UV protection layer, a holographic layer, a logo layer, a protection layer, a pigment layer and an adhesive layer which are stacked in sequence, wherein the holographic layer is prepared by the preparation method of the holographic layer according to any one of claims 1 to 7.
9. An air conditioner holographic IMR panel, characterized in that: The holographic IMR film is prepared by injection molding according to claim 8.
10. An air conditioner, characterized in that: An air-conditioning holographic IMR panel comprising the claim 9.
Citation Information
Patent Citations
Method of forming dual-cure nanostructure transfer film
CN107466306A
Holographic films employing cycloolefin copolymers
US20090142612A1