X-ray protection material with double-layer fiber net structure and preparation method of X-ray protection material

Through the design of the double-layer fiber mesh structure, the density gradient characteristics of the fiber mesh are used to achieve the preparation of efficient X-ray protection materials, which solves the problems of difficulty in dispersion and heavy weight in the existing technology, and achieves lightweight and efficient protection effects and simplicity. process flow.

CN119017786AActive Publication Date: 2024-11-26DONGHUA UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411038512.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-26
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

During the preparation process, existing X-ray protective materials have problems such as difficulty in dispersion, low dispersion efficiency, easy contamination of chemical raw materials, and heavy material weight, making it difficult to meet the needs of high efficiency, lightweight and lead-free.

Method used

Using a double-layer fiber mesh structure, the low-beam layer consists of low-density fiber mesh and high-Z element particles, and the high-beam layer consists of high-density fiber mesh and high-Z element particles. It can achieve efficient particle dispersion and Loading, forming density gradient design to improve absorption efficiency.

Benefits of technology

It significantly improves the absorption efficiency and breathability of X-ray protective materials. The material is light and has excellent protective effect, meeting the needs of high efficiency, lightweight and lead-free, and is simple and efficient in process, suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119017786A_ABST
    Figure CN119017786A_ABST
Patent Text Reader

Abstract

The invention discloses an X-ray protection material with a double-layer fiber net structure and a preparation method of the X-ray protection material, and relates to the technical field of preparation of protection materials. The X-ray protection material comprises a low-beam layer and a high-beam layer, the low-beam layer comprises a low-density fiber mesh layer and high-Z-element particles adsorbed in the low-density fiber mesh layer, and the high-beam layer comprises a high-density fiber mesh layer and high-Z-element particles adhered in the high-density fiber mesh layer; the lower portion of the low beam layer is attached to the upper portion of the high beam layer. The low-density fiber net layer is prepared from fibers 1 and fibers 2, and the fibers 2 adsorb high-Z-element particles under the action of surface molecules in a water-based environment; the preparation raw material of the high-density fiber net layer is double-component fiber, the double-component fiber comprises core layer fiber and skin layer fiber, and the skin layer fiber is used for adhering the high-Z-element particles after being melted. According to the preparation method for loading the high-Z-element particles with the fiber net, the high-Z-element particles are fully mixed, and the X-ray protection effect is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of X-ray protection materials, and in particular relates to an X-ray protection material with a double-layer fiber mesh structure and a preparation method thereof. Background Art

[0002] As a high-energy electromagnetic radiation with strong penetrating power, X-rays have played an important role in many fields such as medical diagnosis, scientific research, and industrial flaw detection. However, long-term or excessive exposure to X-ray radiation can cause a series of hazards to the human body, including cell damage, gene mutations, and even health risks such as leukemia and thyroid disease. Especially for sensitive groups such as pregnant women and children, the potential threat of X-rays is more prominent. With the continuous expansion of X-ray application fields, its usage scenarios are becoming more and more complex. Therefore, in order to meet the protection needs of X-rays in different environments, it is very important to develop efficient and lightweight X-ray protection materials. X-ray protection is not only of great significance for protecting human health, but also ensures the accuracy and safety of medical diagnosis, providing strong guarantees for scientific research and industrial development.

[0003] At present, the core shielding material of most X-ray protection materials on the market is lead-containing rubber, but lead is a very clear carcinogen and is heavy. As shown in the patent with publication number CN113929356A, the preparation method proposes to add a variety of chemical substances such as vulcanizing agents and adhesives, but the refining process of this method is cumbersome, costly, and energy-intensive, and the quality of the X-ray protection material produced is relatively large when the protection requirements are met. Therefore, the current research direction is mainly to make the protection material lead-free, lightweight, and efficient.

[0004] Currently, the preparation methods of X-ray protection materials under research mostly use non-lead high-Z element particles blended with polymer materials. In order to enhance the material's absorption performance of photons, improving the dispersion uniformity of high-Z element particles in the material is a proven effective method. The method of modifying BI2O3 and EU2O3 using silane coupling agents described in the invention with publication number CN115910407A, in which the particle modification process is time-consuming, resulting in low efficiency in actual production, and the modification environment requirements are high, making it difficult to ensure uniform dispersion of particles, increasing the complexity and difficulty of the operation, which is not conducive to large-scale application.

[0005] The above-mentioned preparation method of high-Z element particle shielding material has problems such as difficulty in uniform dispersion, low dispersion efficiency, easy contamination of chemical raw materials, and heavy weight of the finished material. The present invention is based on the structural characteristics of the fiber mesh and uses fibers with different surface characteristics as an auxiliary to provide an efficient and convenient particle dispersion and loading method to prepare efficient and lightweight X-ray shielding materials. Summary of the invention

[0006] The purpose of the present invention is to provide an X-ray shielding material with a double-layer fiber mesh structure and a method for preparing the same, so as to solve the problems in the prior art of preparing X-ray shielding materials proposed in the above background technology, such as difficulty in uniform dispersion, low dispersion efficiency, easy contamination of chemical raw materials, heavy weight of the manufactured material, etc.

[0007] To achieve the above object, the present invention adopts the following technical solutions:

[0008] The first aspect of the present invention provides an X-ray shielding material with a double-layer fiber mesh structure, comprising a low-light layer and a high-light layer, wherein the low-light layer comprises a low-density fiber mesh layer and high-Z element particles adsorbed in the low-density fiber mesh layer, and the high-light layer comprises a high-density fiber mesh layer and high-Z element particles adhered in the high-density fiber mesh layer; the lower side of the low-light layer is attached to the upper side of the high-light layer;

[0009] The raw materials for preparing the low-density fiber mesh layer include fiber 1 and fiber 2, the modulus range of fiber 1 is 80-600 GPa, fiber 2 is a natural fiber with rich hydroxyl groups on the fiber surface, and fiber 2 is used to adsorb high-Z element particles;

[0010] The raw material for preparing the high-density fiber mesh layer is bicomponent fiber, which includes core fiber and skin fiber. The melting point of the skin fiber is lower than that of the core fiber. The skin fiber is used to adhere to the high-Z element particles after melting.

[0011] Preferably, the high-Z element particles include one or more elements with an atomic number Z of 56 to 83, wherein the element is in the form of oxide, simple substance or inorganic salt.

[0012] In the present invention, the near light layer uses the property of bamboo fiber in an aqueous environment where the surface intermolecular force is strengthened to achieve a dispersion method for high-Z element particles to be efficiently adsorbed, and the structure of this layer of material is a fiber mesh layer with a low density. The far light layer uses the property of different melting points of the inner and outer materials of the bicomponent fiber to uniformly adhere the high-Z element particles under the condition of controlling the hot pressing temperature, and because the inner layer has a higher melting point, the fiber mesh structure is still maintained, and finally a fiber mesh layer with a higher density is formed. The present invention realizes a preparation method for loading high-Z element particles with a fiber mesh, fully mixes the high-Z particles, and improves the X-ray protection effect.

[0013] The second aspect of the present invention provides a method for preparing an X-ray shielding material with a double-layer fiber mesh structure, comprising the following steps:

[0014] S1. Preparation of near light layer;

[0015] Add fiber 1, fiber 2 and deionized water to a cutting and stirring device, cut and stir at room temperature, and preliminarily mix fiber 1 and fiber 2, and the stirring time of the preliminary mixing is 3 to 30 seconds; then add high-Z element particles to the cutting and stirring device, cut and stir for 10 to 100 seconds to obtain a mixture of fiber 1 / fiber 2 / high-Z element particles / deionized water; treat the mixture to completely remove the deionized water, and after drying, obtain a low-density mixture of fiber 1 / fiber 2 / high-Z element particles, i.e., a near-light layer;

[0016] S2, preparation of the far light layer;

[0017] The two-component fiber is opened, and then combed into a web by a carding machine to obtain a fiber web, and the fiber web is processed by a needle combing machine to obtain a needle-punched cloth; high-Z element particles are evenly sprayed on the needle-punched cloth by a granulator, and then the high-Z element particles are needle-punched between the fibers; the needle-punched cloth mixed with high-Z element particles is placed in a mold, and then hot-pressed, the hot-pressing time is 4 to 100 minutes, and the hot-pressing temperature is 160 to 220° C. After hot-pressing, a high-density needle-punched fiber material, i.e., a high-light layer, is obtained;

[0018] S3. Preparation of X-ray protection material with double-layer fiber mesh structure;

[0019] The high beam layer is spread flat on the bottom of the mold, and the low beam layer is completely attached to the high beam layer. Water-based polyurethane is poured into the mold to immerse the low beam layer in the water-based polyurethane. The superimposed low beam layer and high beam layer are then taken out, and after drying, a double-layer fiber mesh structure X-ray protection material is obtained.

[0020] Preferably, the fiber 1 is made of carbon fiber or hemp fiber.

[0021] Furthermore, the fiber 1 added by the cutting and stirring device in S1 has a fiber length ranging from 0.1 to 10.0 cm, preferably from 0.5 to 2.0 cm. If the fiber 1 is too long, it is not conducive to cutting and stirring, and if it is too short, the shear force provided during rotation is reduced, which is not conducive to particle dispersion.

[0022] Preferably, the fiber 2 is wood pulp fiber.

[0023] Furthermore, the fiber 2 is made of cotton fiber, bamboo fiber or hemp fiber.

[0024] Preferably, the core layer / skin layer of the bicomponent fiber is PET / PAN, PET / PP or PET / PA. The melting point of PET (polyethylene terephthalate) is higher than the hot pressing temperature of 160-220°C; the melting points of PAN, PP and PA are lower than the hot pressing temperature of 160-220°C, and they melt after hot pressing to adhere to the high-Z element particles.

[0025] Preferably, the high-Z element particles are bismuth oxide particles.

[0026] Furthermore, the diameter of the high-Z element particles in S1 ranges from 30 to 500 nanometers.

[0027] Furthermore, the diameter of the high-Z element particles in S2 ranges from 0.5 to 100 microns, preferably from 5 to 40 microns.

[0028] Preferably, the weight of the fiber 2 in S1 is 10% to 200% of the weight of the fiber 1 , and the weight of the deionized water is 20 to 80 times the total weight of the fiber 1 and the fiber 2 .

[0029] Preferably, the mixture is treated in S1 to completely remove the deionized water, specifically: the mixture is filtered, and then squeezed to dry or directly dried to completely remove the deionized water.

[0030] Further, pour the fiber 1 / fiber 2 / high-Z element particles / deionized water mixture into a filter dish to filter out the flowing deionized water; place a pressure cap on the mixture, adjust the weight of the pressure cap according to the diameter of the filter dish so that the pressure range of the pressure cap on the mixture is 20 to 300N, and then let it stand to dry to completely remove the deionized water; or remove the deionized water by drying, place the mixture together with the filter dish in an oven to dry and form, and the drying temperature is preferably not to affect the properties of the fibers used. After complete drying, a fluffy and porous fiber 1 / fiber 2 / high-Z element particle mixture is obtained.

[0031] Preferably, the needle-punched fabric in S2 is specifically processed as follows: first, the bicomponent fibers are opened to obtain loose single fibers or small fiber bundles; and then the fibers are combed into a web by a carding machine, and the obtained fiber web has a thickness ranging from 100 to 600 g / m 2 , preferably 210~300g / m 2 The fiber web is passed through a needle combing machine, and the needle combing machine needle punching frequency range is set to 30 to 500 punctures / minute, preferably 100 to 200 punctures / minute.

[0032] Preferably, the hot pressing in S2 is specifically as follows: placing the needle-punched cloth doped with high-Z element particles into a mold with a thickness of 0.5 to 4 mm, followed by hot pressing (hot pressing pressure range 1.5 to 4 MPa), hot pressing time 4 to 100 min, and hot pressing temperature 160 to 220°C.

[0033] Preferably, the low beam layer in S3 is immersed in waterborne polyurethane, specifically: the solid content of the waterborne polyurethane is 5% to 40% to ensure sufficient fluidity; the solid content of the waterborne polyurethane is 15% to 20% of the weight of the added high-Z element particles.

[0034] Preferably, after drying in S3, an X-ray protective material with a double-layer fiber mesh structure is obtained, specifically: it is dried by standing still or in an oven. If drying in an oven is adopted, the drying temperature cannot be higher than 60°C, and the drying time can be adjusted with the temperature, and finally an X-ray protective material with a double-layer fiber mesh structure is obtained.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] (1) The X-ray protection material with a double-layer fiber mesh structure in the present invention has a low-light layer prepared by mixing-stacking-adsorption. The material is rich in holes and has a low density, so that more photons can penetrate into the material. The high-light layer uses a high-density needle-punched cloth material that has been heat-pressed to form a tightly arranged "micro-chamber" structure. This double-layer density gradient design material can reduce scattering on the one hand: the low-density design of the low-light layer helps to reduce the scattering of photons on the surface of the material, thereby reducing the impact of scattered radiation on the environment; the high density of the high-light layer helps to capture the photons that penetrate the low-light layer, further reducing scattering. On the other hand, it can improve the absorption efficiency of the material: the porous structure of the low-light layer allows photons to penetrate into the material and collide with high-Z particles multiple times, thereby improving the absorption efficiency; the compact structure of the high-light layer ensures that the remaining photons are effectively absorbed. This design significantly enhances the scattering and absorption effect of photons between fiber layers, thereby improving the overall protection ability of the material against radiation. In addition, this X-ray material with a fiber mesh structure can achieve a certain air permeability while maintaining X-ray protection ability.

[0037] (2) The present invention designs a near-light layer, and the high modulus fiber has good shape stability. During the stacking process, a three-dimensional network structure is constructed, which effectively physically separates the bismuth oxide particles and provides more paths for X-ray scattering and absorption. The physical properties of high-strength fibers generate shear force and impact force during the stirring process, improve the agglomeration of nanoparticles, increase the specific surface area, and thus increase the probability of the photoelectric effect, thereby achieving the effect of improving the X-ray protection ability of the material. In addition, wood pulp fibers have higher surface energy and polarity due to the hydroxyl groups they contain, which makes them easier to adsorb polar particles, such as nano bismuth oxide particles. The material structure allows the bismuth oxide particles to be evenly and firmly dispersed between the fibers, forming a compact photon absorption space, reducing photon escape, and improving the efficiency of the photoelectric effect. Photons collide multiple times between fibers, extending the free path, reducing the energy to complete absorption, and achieving an X-ray protection effect. This design significantly improves the probability of photon scattering and transmission distance, so that the finished product has excellent X-ray protection performance.

[0038] (3) The present invention designs a far-beam layer, adheres particles to the fiber net, and has certain pores in the material, so that the material can have certain air permeability while ensuring the X-ray protection effect. However, most X-ray protection materials on the market use polymers and high-Z particles directly mixed together, and the air permeability is basically zero.

[0039] (4) The X-ray protective material with a double-layer fiber mesh structure in the present invention is light in material and has good protective effect while ensuring the protective effect. Compared with the traditional lead rubber material, the lightweight and efficient X-ray protective material prepared by the present invention can achieve an effect of 0.35mmpb when the mass is 25.6g (a disc with a diameter of 9cm) under a tube voltage of 80KV, which exceeds the national standard (0.25mmpb). And the lead rubber material with a 0.35mmpb effect purchased on the market (cut into a disc with a diameter of 9cm) has a mass of 32.17g. Compared with the materials used in the market, the weight of the X-ray protective material prepared by this method is reduced by 20%. And when the addition amount of high-Z particles of this material is 12, 16, 20, 24, and 28g, its protective effect at 80KV is significantly improved, and it can be used to prepare lightweight and efficient X-ray protective materials.

[0040] (5) The present invention designs an extremely simple and highly efficient method for reducing the agglomeration of nanoparticles and promoting the uniform dispersion of nanoparticles in polymers. Only a very small amount of auxiliary fibers need to be added to achieve the dispersion of agglomerated particles. This method can be applied not only to the field of X-ray protection, but also to other functional fields that require uniform dispersion of nanoparticles, and has extremely strong potential application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is a flow chart of a method for preparing an X-ray shielding material with a double-layer fiber mesh structure in the present invention;

[0042] Figure 2 A schematic diagram of an X-ray source irradiating an X-ray shielding material in the present invention;

[0043] Figure 3 This is an electron microscope image of the near-light layer of the X-ray protection material of the present invention;

[0044] Figure 4 This is an electron microscope image of a fiber of the X-ray shielding material of the present invention that has adsorbed high-Z element particles;

[0045] Figure 5 It is an electron microscope image of the far-light layer of the X-ray protection material of the present invention;

[0046] Figure 6 This is a graph showing the air permeability test results of the X-ray shielding material prepared in Example 1 of the present invention;

[0047] Figure 7 This is a comparison chart of the effects of the X-ray shielding material prepared in Example 1 of the present invention and materials on the market;

[0048] Figure 8 This is a comparison chart of the protective effects of protective materials with and without added fiber mesh structure. DETAILED DESCRIPTION

[0049] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0050] Embodiment 1:

[0051] like Figure 1 As shown, the preparation method of the X-ray protection material with a double-layer fiber mesh structure is as follows:

[0052] S1. Weigh 0.6g of carbon fiber and cut it to 1.5cm, then mix it with 0.2g of bamboo fiber and 50g of deionized water in a cutting agitator, start the cutting agitator, and stir for 5S at room temperature for preliminary mixing. Then weigh 12g of bismuth oxide particles, add them to the cutting agitator containing the preliminary mixture of carbon fiber and bamboo fiber, and stir again for 30S to obtain a mixture of carbon fiber, bamboo fiber and bismuth oxide. Pour the mixed solution into a filter dish with a diameter of 9cm, filter out excess deionized water, and then dry it in a 40℃ oven for 24h to form a fluffy porous mixture.

[0053] S2. Open the bicomponent fiber (PET / PP) to obtain loose single fibers or fiber bundles of a certain length. Weigh 50.4g of the opened fibers and evenly spread them on the conveyor belt of the carding machine for combing. Comb twice to obtain a 30cm×80cm fiber web. Take the combed fiber web and lay it flat on the conveyor belt of the needle punching machine, and then perform acupuncture at a frequency of 100-200 punctures / min. After obtaining a uniform pre-needled cloth, cut the needle punched cloth into discs with a diameter of 9cm, and use a granulator to evenly spray 12g of bismuth oxide particles. In order to evenly disperse the particles in the needle punched cloth, perform another acupuncture to needle the particles into the fibers, and then perform hot pressing (hot pressing pressure 2Mpa), the hot pressing time is 10min, and the hot pressing temperature is 160°C. After hot pressing, a second layer of needle punched fiber material with a higher density is obtained.

[0054] S3, the second layer material (needle punch material) is evenly spread on the bottom of the polytetrafluoroethylene mold with a diameter of 9cm, and then the first layer material (fluffy and porous high-strength fiber / bamboo fiber / bismuth oxide mixture) is spread on the first layer material. Pour water-based polyurethane, immerse the high-strength fiber / bamboo fiber / bismuth oxide mixture in the water-based polyurethane, and pour 25g of water-based polyurethane (solid content 15%). Dry it again in an oven at 45°C for 24h, and dry it to obtain a double-layer composite material with 24g of Bi2O3 added.

[0055] The performance test of the double-layer composite material is as follows:

[0056] In this embodiment, the double-layer composite material is a double-layer superimposed structure of a low beam layer and a high beam layer. Figure 2 As shown, the prepared double-layer composite material is irradiated with an X-ray source, the layer close to the X-ray source is the near-light layer, and the layer far from the X-ray source is the far-light layer. The electron microscope image of the near-light layer of the sample of Example 1 is shown in FIG. Figure 3 , Figure 4 As shown in Figure 1, nano-bismuth oxide forms a covering layer on the surface of bamboo fibers. Figure 5 As shown, it can be seen that micron-sized bismuth oxide is evenly dispersed inside the fiber mesh. Due to the different melting points of the two-component fibers, the skin layer adheres to the bismuth oxide particles after melting, but the material still retains the fiber mesh structure.

[0057] In this embodiment, the air permeability of the prepared X-ray protection composite material was tested according to GB 5453-1997 "Determination of air permeability of textile fabrics". According to the standard, the test pressure was set to 200Pa, and the air permeability effect was measured as follows: Figure 6 As shown. However, the lead rubber material purchased on the market has basically no air permeability effect.

[0058] In this embodiment, the sample obtained according to the preparation method has a mass of 25.6 g and a lead equivalent effect of 0.35 mmpb when the amount of bismuth oxide added is 24 g. Compared with the lead rubber with the same shielding effect on the market (cut into a 9 cm diameter disc), the mass is 32.17 g. Under the same effect, the weight reduction effect can be improved by 20%. The comparison effect is as follows Figure 7 shown.

[0059] Embodiment 2:

[0060] The preparation method of the X-ray protection material with a double-layer fiber mesh structure is as follows:

[0061] S1. Weigh 0.6g of carbon fiber and cut it to 1.5cm, then mix it with 0.2g of cotton fiber and 50g of deionized water in a cutting blender, start the cutting blender, and stir for 40S at room temperature for preliminary mixing. Then weigh 12g of bismuth oxide particles, add them to the cutting blender containing the preliminary mixture of carbon fiber and cotton fiber, and stir again for 30S to obtain a mixture of carbon fiber, cotton fiber and bismuth oxide. Pour the mixture into a filter dish with a diameter of 9cm, filter out excess deionized water, and then dry it in a 40℃ oven for 24h to form a fluffy porous mixture.

[0062] S2. Open the bicomponent fiber (PET / PP) to obtain loose single fibers or fiber bundles of a certain length. Weigh 50.4g of the opened fibers and evenly spread them on the conveyor belt of the carding machine for combing. Comb twice to obtain a 30cm×80cm fiber web. Take the combed fiber web and lay it flat on the conveyor belt of the needle punching machine, and then perform acupuncture at a frequency of 100-200 punctures / min. After obtaining a uniform pre-needled cloth, cut the needle punched cloth into discs with a diameter of 9cm, and use a granulator to evenly spray 12g of bismuth oxide particles. In order to evenly disperse the particles in the needle punched cloth, perform another acupuncture to needle the particles into the fibers, and then perform hot pressing (hot pressing pressure 2Mpa), the hot pressing time is 10min, and the hot pressing temperature is 160°C. After hot pressing, a second layer of needle punched fiber material with a higher density is obtained.

[0063] S3. Lay the second layer of material (needle punched material) evenly on the bottom of a 9cm diameter polytetrafluoroethylene mold, and then lay the first layer of material (fluffy porous high-strength fiber / cotton fiber / bismuth oxide mixture) on the first layer of material. Pour water-based polyurethane, immerse the high-strength fiber / cotton fiber / bismuth oxide mixture in the water-based polyurethane, and pour 25g of water-based polyurethane (solid content 15%). Dry in an oven at 45°C for 24h, and dry to obtain a sample obtained by the adsorption of cotton fibers in the near-light layer.

[0064] Example 2 successfully used cotton fibers to adsorb high-Z element particles in the near-light layer, once again proving the adsorption effect of natural fibers on nanoparticles in an aqueous environment.

[0065] Embodiment 3:

[0066] The preparation method of the X-ray protection material with a double-layer fiber mesh structure is as follows:

[0067] S1. Weigh 0.6g of carbon fiber and cut it to 1.5cm, then mix it with 0.2g of bamboo fiber and 50g of deionized water in a cutting agitator, start the cutting agitator, and stir for 40S at room temperature for preliminary mixing. Then weigh 12g of bismuth oxide particles, add them to the cutting agitator containing the preliminary mixture of carbon fiber and bamboo fiber, and stir again for 30S to obtain a mixture of carbon fiber, bamboo fiber and bismuth oxide. Pour the mixed solution into a filter dish with a diameter of 9cm, filter out excess deionized water, and then dry it in a 40℃ oven for 24h to form a fluffy porous mixture.

[0068] S2. Open the bicomponent fiber (PET / PAN) to obtain loose single fibers or fiber bundles of a certain length. Weigh 50.4g of the opened fibers and evenly spread them on the conveyor belt of the carding machine for combing. Comb twice to obtain a 30cm×80cm fiber web. Take the combed fiber web and lay it flat on the conveyor belt of the needle punching machine, and then perform acupuncture at a frequency of 100-200 punctures / min. After obtaining a uniform pre-needled cloth, cut the needle punched cloth into discs with a diameter of 9cm, and use a granulator to evenly spray 12g of bismuth oxide particles. In order to evenly disperse the particles in the needle punched cloth, perform another acupuncture to needle the particles into the fibers, and then perform hot pressing (hot pressing pressure 2Mpa), the hot pressing time is 10min, and the hot pressing temperature is 160°C. After hot pressing, a second layer of needle punched fiber material with a higher density is obtained.

[0069] S3. The second layer of material (needle punched material) is evenly laid on the bottom of a 9 cm diameter polytetrafluoroethylene mold, and then the first layer of material (fluffy porous high-strength fiber / bamboo fiber / bismuth oxide mixture) is laid on the first layer of material. Pour water-based polyurethane, immerse the high-strength fiber / bamboo fiber / bismuth oxide mixture in the water-based polyurethane, and pour 25g of water-based polyurethane (solid content 15%). Dry in an oven at 45°C for 24h, and dry to obtain a sample obtained by the adhesion of the far-light layer by the two-component fiber (PET / PAN).

[0070] Example 3 uses a two-component fiber (PET / PAN), in which the skin layer is polyacrylonitrile with a lower melting point, and the core layer is polyethylene terephthalate with a higher melting point. After hot pressing, the fiber material completely adheres to the 12g bismuth oxide particles added to the high-beam layer.

[0071] Embodiment 4:

[0072] The preparation method of the X-ray protection material with a double-layer fiber mesh structure is as follows:

[0073] S1. Weigh 1.2g of carbon fiber and cut it to 1.5cm, then mix it with 0.2g of bamboo fiber and 50g of deionized water in a cutting agitator, start the cutting agitator, and stir for 40S at room temperature for preliminary mixing. Then weigh 12g of bismuth oxide particles, add it to the cutting agitator containing the preliminary mixture of carbon fiber and bamboo fiber, and stir again for 30S to obtain a mixture of carbon fiber, bamboo fiber and bismuth oxide. Pour the mixed solution into a filter dish with a diameter of 9cm, filter out excess deionized water, and then dry it in a 40℃ oven for 24h to form a fluffy porous mixture.

[0074] S2. Open the bicomponent fiber (PET / PAN) to obtain loose single fibers or fiber bundles of a certain length. Weigh 50.4g of the opened fibers and evenly spread them on the conveyor belt of the carding machine for combing. Comb twice to obtain a 30cm×80cm fiber web. Take the combed fiber web and lay it flat on the conveyor belt of the needle punching machine, and then perform acupuncture at a frequency of 100-200 punctures / min. After obtaining a uniform pre-needled cloth, cut the needle punched cloth into discs with a diameter of 9cm, and use a granulator to evenly spray 12g of bismuth oxide particles. In order to evenly disperse the particles in the needle punched cloth, perform another acupuncture to needle the particles into the fibers, and then perform hot pressing (hot pressing pressure 2Mpa), the hot pressing time is 10min, and the hot pressing temperature is 160°C. After hot pressing, a second layer of needle punched fiber material with a higher density is obtained.

[0075] S3. The second layer of material (needle punched material) is evenly laid on the bottom of a 9 cm diameter polytetrafluoroethylene mold, and then the first layer of material (fluffy porous high-strength fiber / bamboo fiber / bismuth oxide mixture) is laid on the first layer of material. Pour water-based polyurethane, immerse the high-strength fiber / bamboo fiber / bismuth oxide mixture in the water-based polyurethane, and pour 25g of water-based polyurethane (solid content 15%). Dry in an oven at 45°C for 24h, and dry to obtain a sample obtained by the adsorption of bamboo fiber in the near light layer.

[0076] The sample prepared according to the method of Example 4 only changed the amount of carbon fiber added compared to Example 1, but the lead equivalent of Example 4 was 0.37 mmpb, which was improved compared to the lead equivalent effect of 0.35 mmpb of the sample in Example 1, further proving that carbon fiber helps to improve the X-ray protection performance of the material.

[0077] Comparative Example 1:

[0078] S1. Weigh different masses of nano bismuth oxide particles (12g, 16g, 20g, 24g, 28g) and place them in a beaker. According to the weighed bismuth oxide particles, accurately weigh 1 / 2 of the mass of the water-based polyurethane (solid content of 38%) of the bismuth oxide particles. Pour it into the beaker containing bismuth oxide particles. Place the beaker containing bismuth oxide and water-based polyurethane on a magnetic stirrer. Stir for 12 minutes at room temperature using a magnetic stirrer with a rotation speed of 1000 revolutions per minute.

[0079] S2. After stirring, quickly pour the mixture into a 9 cm diameter tetrafluoroethylene mold. Manually shake to spread evenly, and then put it into a 40°C oven for drying for 24 hours. Then demold and take it out to obtain a comparison sample.

[0080] The protective material was prepared by using the preparation method in Example 1, and five different contents of bismuth oxide particles were added, 12g, 16g, 20g, 24g, and 28g, respectively. The comparative sample was prepared using the same bismuth oxide particles and waterborne polyurethane as in Example 1, and five different contents of bismuth oxide particles were added, 12g, 16g, 20g, 24g, and 28g, respectively. The protective effect was compared with that of Example 1. Figure 8 It can be seen that the X-ray protection effect of the protective material with added fiber mesh structure is significantly improved at different addition amounts.

[0081] The above description is only used to help understand the method of the present invention and its core essence, but the protection scope of the present invention is not limited thereto. For those skilled in the art in the art, equivalent replacement or change according to the technical solution and inventive concept of the present invention within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. An X-ray protection material with a double-layer fiber mesh structure, characterized in that: It comprises a low beam layer and a high beam layer, wherein the low beam layer comprises a low-density fiber mesh layer and high-Z element particles adsorbed in the low-density fiber mesh layer, and the high beam layer comprises a high-density fiber mesh layer and high-Z element particles adhered in the high-density fiber mesh layer; the lower part of the low beam layer is attached to the upper part of the high beam layer; The low-density fiber mesh layer is prepared from fibers 1 and 2. The modulus of fiber 1 is in the range of 80 to 600 GPa. Fiber 2 is a natural fiber with a rich hydroxyl group on the fiber surface. Fiber 2 uses the surface intermolecular interaction in an aqueous environment to adsorb high-Z element particles. The raw material for preparing the high-density fiber mesh layer is bicomponent fiber, which includes core fiber and skin fiber. The melting point of the skin fiber is lower than that of the core fiber. The skin fiber is used to adhere to the high-Z element particles after melting.

2. The X-ray shielding material with a double-layer fiber mesh structure according to claim 1, characterized in that: The high-Z element particles include one or more elements with an atomic number Z of 56 to 83, wherein the element is in the form of oxide, simple substance or inorganic salt.

3. A method for preparing an X-ray protective material with a double-layer fiber mesh structure as claimed in claim 1 or 2, characterized in that: The steps include: S1. Preparation of near light layer; Add fiber 1, fiber 2 and deionized water into a cutting and stirring device, cut and stir at room temperature to preliminarily mix fiber 1 and fiber 2, and the stirring time for the preliminary mixing is 3 to 30 seconds; Then, high-Z element particles are added to the cutting and stirring device, and the mixture is cut and stirred for 10 to 100 seconds to obtain a mixture of fiber 1 / fiber 2 / high-Z element particles / deionized water; the mixture is treated to completely remove the deionized water, and after drying, a low-density mixture of fiber 1 / fiber 2 / high-Z element particles is obtained, namely, a near-light layer; S2, preparation of the far light layer; The two-component fiber is opened, and then combed into a web by a carding machine to obtain a fiber web, and the fiber web is processed by a needle combing machine to obtain a needle-punched cloth; high-Z element particles are evenly sprayed on the needle-punched cloth by a granulator, and then the high-Z element particles are needle-punched between the fibers; the needle-punched cloth mixed with high-Z element particles is placed in a mold, and then hot-pressed, the hot-pressing time is 4 to 100 minutes, and the hot-pressing temperature is 160 to 220° C. After hot-pressing, a high-density needle-punched fiber material, i.e., a high-light layer, is obtained; S3. Preparation of X-ray protection material with double-layer fiber mesh structure; The high beam layer is spread flat on the bottom of the mold, and the low beam layer is completely attached to the high beam layer. Water-based polyurethane is poured into the mold to immerse the low beam layer in the water-based polyurethane. The superimposed low beam layer and high beam layer are then taken out, and after drying, a double-layer fiber mesh structure X-ray protection material is obtained.

4. The method for preparing a double-layer fiber mesh structure X-ray protection material according to claim 3, characterized in that: The fiber 1 is made of carbon fiber or hemp fiber.

5. The method for preparing a double-layer fiber mesh structure X-ray protection material according to claim 3, characterized in that: The fiber 2 is wood pulp fiber.

6. The method for preparing a double-layer fiber mesh structure X-ray protection material according to claim 5, characterized in that: The fiber 2 is made of cotton fiber, bamboo fiber or hemp fiber.

7. The method for preparing a double-layer fiber mesh structure X-ray protection material according to claim 3, characterized in that: The bicomponent fiber adopts core layer / skin layer of PET / PAN, PET / PP or PET / PA.

8. The method for preparing a double-layer fiber mesh structure X-ray protection material according to claim 3, characterized in that: The diameter of the high-Z element particles in S1 ranges from 30 to 500 nanometers; the diameter of the high-Z element particles in S2 ranges from 0.5 to 100 micrometers.

9. The method for preparing a double-layer fiber mesh structure X-ray protection material according to claim 8, characterized in that: The high-Z element particles are bismuth oxide particles.

10. The method for preparing a double-layer fiber mesh structure X-ray protection material according to claim 3, characterized in that: The weight of the fiber 2 in the S1 is 10% to 200% of the weight of the fiber 1 , and the weight of the deionized water is 20 to 80 times the total weight of the fiber 1 and the fiber 2 .

Citation Information

Patent Citations

  • Double-layer adsorption and protection fabric

    CN103753876A

  • Element gradient combined anti-radiation rubber product and preparation method thereof

    CN106009944A

  • Flexible material with nuclear radiation protection and electromagnetic shielding functions, and preparation method and application thereof

    CN111572133A

  • X-ray attenuation fiber, and fabric and clothing using the fiber

    JP2014070324A