High-bonding-strength oxidation-ablation-resistant composite coating for ceramic-based composite material and preparation method of high-bonding-strength oxidation-ablation-resistant composite coating

By using low-pressure plasma spraying method on the surface of the ceramic matrix composite material to prepare a ceramic coating reinforced with chopped carbon fiber and chopped silicon carbide fiber, the bonding strength and resistance of ceramic matrix composite materials in high-temperature oxidation and ablation environment is solved. Ablation performance issues achieve efficient protection effect.

CN119019179AActive Publication Date: 2024-11-26AEROSPACE INST OF ADVANCED MATERIALS & PROCESSING TECH

Patent Information

Application Number
CN202411161053.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

Ceramic matrix composites are prone to oxidation and have poor ablation resistance under high-temperature oxidation and ablation properties. The existing coatings have low bonding strength with the substrate, which leads to the coatings being easily shedded during thermal shock and cannot effectively protect the substrate.

Method used

Low-pressure plasma spraying method is used to prepare a layer shell coated with chopped carbon fiber reinforced ultra-high temperature ceramic bottom layer and a layer shell coated with chopped silicon carbide fiber reinforced ultra-high temperature ceramic surface layer to form a high binding strength anti-oxidation burning The composite coating is etched, and the weak interface deflection cracks are used between the shell and the fiber, thereby improving the bonding strength between the coating and the substrate and resisting high-temperature oxidation and ablation.

Benefits of technology

It significantly improves the resistance to high-temperature oxidation ablation and service life of ceramic matrix composites, realizes a coating with high binding strength and density, and reduces the risk of peeling of the coating in high-temperature environments and the possibility of interface failure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019179A_ABST
    Figure CN119019179A_ABST
Patent Text Reader

Abstract

The invention relates to a high-bonding-strength oxidation-ablation-resistant composite coating for a ceramic-based composite material and a preparation method of the high-bonding-strength oxidation-ablation-resistant composite coating. The high-bonding-strength oxidation-ablation-resistant composite coating sequentially comprises a superhigh-temperature ceramic bottom layer coating reinforced by a layer shell coated chopped carbon fiber and a superhigh-temperature ceramic surface layer coating reinforced by a layer shell coated chopped silicon carbide fiber from the ceramic-based composite material to the outside. The method comprises the following steps: pretreating the ceramic-based composite material; the preparation method comprises the following steps: sequentially preparing a shell-coated short carbon fiber reinforced superhigh-temperature ceramic bottom layer coating and a shell-coated short silicon carbide fiber reinforced superhigh-temperature ceramic surface layer coating on the surface of a pretreated ceramic-based composite material through a low-pressure plasma spraying method, so as to prepare the high-bonding-strength oxidation-ablation-resistant composite coating. The prepared composite coating is low in porosity, high in bonding strength and excellent in high-temperature oxidation ablation resistance, and the high-temperature protective coating for the ceramic-based composite material can be prepared with high efficiency and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of protective coatings, and in particular relates to a high-bonding-strength anti-oxidation and ablation composite coating for ceramic-based composite materials and a preparation method thereof. Background Art

[0002] Carbon fiber-reinforced ceramic matrix composites combine the high strength and high oxidation resistance of ceramics with the excellent mechanical properties of carbon fiber, and have broad application prospects in the aerospace field. However, the continuous increase in the working temperature of ceramic matrix composites and the need for long-term service in high temperature, oxidation and ablation environments face the problem that carbon fiber is easily oxidized at high temperatures and has poor ablation resistance. It is difficult to meet the performance requirements by relying solely on the ceramic matrix composite matrix.

[0003] In order to improve the high-temperature oxidation and ablation resistance of ceramic-based composite materials, ceramic coatings are often prepared on their surfaces to isolate them from air. Although traditional coating preparation methods, such as chemical vapor deposition, brush coating, plasma spraying, etc., have their own advantages, they generally have the problem of low bonding strength between the coating and the substrate, which causes the coating to easily fall off when experiencing thermal shock and cannot effectively protect the substrate.

[0004] Chinese patent application CN201610172208.0 discloses a ceramic fiber / whisker reinforced composite thermal barrier coating and a preparation method thereof, which uses a plasma spraying or laser cladding method to prepare a ceramic fiber / whisker reinforced oxide coating on the surface of an alloy substrate. Although ceramic fibers / whiskers can improve the fracture toughness of the oxide coating, the thermal expansion coefficient of the oxide coating is quite different from that of the carbon fiber-toughened ceramic-based composite material matrix in the present invention, which will lead to a large thermal mismatch stress between the coating and the ceramic-based composite material matrix, which will reduce the coating bonding strength and thermal shock life, thereby reducing the protective effect of the coating.

[0005] Chinese patent application CN202410645601.1 discloses a method for preparing a TaC ceramic coating. The method first grows silicon carbide nanowires on the surface of a substrate by chemical vapor deposition, and then deposits a TaC ceramic coating on the surface of the substrate by chemical vapor deposition to form a TaC coating toughened by silicon carbide nanowires. However, this method has certain limitations. Repeated heating and cooling will cause cracks in the TaC coating, affecting the quality of the coating. In addition, the efficiency of preparing the coating by the chemical vapor deposition method is low and the cost is high.

[0006] Chinese patent application CN202210003897.8 discloses a thermal protection coating prepared using a silicone rubber matrix, hollow ceramic powder and an auxiliary reinforcing agent and a preparation method thereof. Since the silicone rubber matrix will accelerate aging, cracking and powdering at high temperatures, the slurry in this method is not suitable for preparing the coating by thermal spraying; in addition, the coating mainly relies on hollow ceramic powder to provide thermal protection. In an environment with higher temperature and higher speed air flow, the bonding strength between the hollow ceramic powders is insufficient, the coating is very easy to peel off, and the coating has poor ablation resistance, so it is not suitable for ablation environments exceeding 1800°C.

[0007] Therefore, there is an urgent need to provide a high bonding strength anti-oxidation and ablation coating suitable for ceramic-based composites and a preparation method thereof, so as to significantly improve the anti-oxidation and ablation performance and service life of ceramic-based composites in extreme environments. Summary of the invention

[0008] In order to solve one or more technical problems existing in the prior art, the present invention provides a high-bonding-strength anti-oxidation-ablation composite coating for ceramic-based composite materials and a preparation method thereof. The high-bonding-strength anti-oxidation-ablation composite coating prepared by the present invention has low porosity, high bonding strength, and excellent resistance to high-temperature oxidation and ablation. The present invention can prepare a high-temperature protective coating for ceramic-based composite materials with high efficiency and low cost.

[0009] In the first aspect, the present invention provides a high bonding strength, anti-oxidation and ablation composite coating for ceramic-based composite materials, wherein the high bonding strength, anti-oxidation and ablation composite coating comprises, from the ceramic-based composite material outward, a layer shell-coated short carbon fiber reinforced ultra-high temperature ceramic bottom coating and a layer shell-coated short silicon carbide fiber reinforced ultra-high temperature ceramic surface coating.

[0010] In a second aspect, the present invention provides a method for preparing the high bonding strength anti-oxidation and ablation composite coating for ceramic matrix composite materials according to the first aspect of the present invention, the method comprising the following steps:

[0011] (1) grinding, cleaning and drying the ceramic-based composite material to obtain a pretreated ceramic-based composite material;

[0012] (2) A shell-coated short carbon fiber reinforced ultra-high temperature ceramic base coating and a shell-coated short silicon carbide fiber reinforced ultra-high temperature ceramic surface coating are sequentially prepared on the surface of the pretreated ceramic-based composite material by a low-pressure plasma spraying method, thereby obtaining the high bonding strength and anti-oxidation and ablation composite coating on the surface of the ceramic-based composite material.

[0013] The present invention in a third aspect provides a high bonding strength anti-oxidation and ablation composite coating for ceramic-based composite materials, which is prepared by the preparation method described in the second aspect of the present invention.

[0014] Compared with the prior art, the present invention has at least the following beneficial effects:

[0015] (1) The prior art, for example, Chinese patent application CN201610172208.0 discloses a fiber-reinforced oxide coating suitable for alloy surfaces and a preparation method thereof. However, the coating has a single structure, limited functions, and relatively poor bonding strength, and the coating is not suitable for ceramic-based composite substrates with higher operating temperatures. The present invention designs an anti-oxidation and ablation composite coating with high bonding strength, wherein the bottom layer of the composite coating is an ultra-high temperature ceramic coating reinforced with chopped carbon fibers coated with a shell. The role of the chopped carbon fibers coated with the shell in the coating is to effectively improve the fracture toughness of the coating, reduce the thermal expansion coefficient of the coating, and deflect the crack propagation path in the coating. Therefore, the bottom layer is designed to alleviate the mismatch in thermal expansion coefficients between the coating and the ceramic-based composite substrate, reduce the thermal mismatch stress between the coating and the substrate, and improve the bonding strength of the coating. , thereby extending the thermal shock life of the coating; the surface layer of the composite coating is an ultra-high temperature ceramic coating reinforced by chopped silicon carbide fibers coated with a layer shell. The role of the chopped silicon carbide fibers in the coating is to improve the fracture toughness of the coating. Its oxidation product, silicon oxide, can enhance the self-healing effect of the coating under high-temperature oxidation and ablation conditions. Therefore, the surface layer is designed to improve the coating's resistance to high-temperature oxidation and high-temperature ablation. In addition, the present invention finds that the interface between the layer shell and the chopped fibers (chopped carbon fibers and chopped silicon carbide fibers) deflects the crack propagation path, which can further avoid peeling of the coating in an ablation environment, which is beneficial to enhancing the bonding strength between the coating and the substrate, and improving the high-temperature ablation and oxidation resistance of the composite coating. The composite coating designed by the present invention can give full play to the synergistic effect, further ensuring that the coating has both high bonding strength and excellent anti-oxidation and ablation thermal properties.

[0016] (2) The prior art, for example, Chinese patent application CN202410645601.1 discloses a method for preparing a TaC ceramic coating, but the preparation cost is relatively high and the coating preparation efficiency is low. The present invention prepares the high bonding strength and anti-oxidation and ablation composite coating for the first time by a low-pressure plasma spraying method. In the low-pressure plasma spraying preparation method, under a low-pressure and inert gas environment, the low-pressure plasma spraying method has the advantages of high spraying power, high jet temperature and fast speed, and has the advantages of high deposition efficiency and low cost. In addition, the spraying powder is melted more fully under the action of the high-energy plasma beam, and the coating porosity is lower, thereby avoiding the generation of internal defects in the coating and reducing the risk of peeling of the coating along the defective position under a high-temperature ablation environment. At the same time, it also reduces the possibility of failure along the interface between the coating and the ceramic-based composite material substrate, thereby more effectively ensuring that the composite coating has high bonding strength and excellent anti-oxidation and ablation performance. The method of the present invention has the advantages of high deposition efficiency, low cost and high coating density, and can realize the integrated preparation of the composite coating.

[0017] (3) The prior art, for example, Chinese patent application CN202210003897.8 discloses a method for preparing a thermal protective coating on a substrate by using a slurry prepared using a silicone rubber matrix, hollow ceramic powder and an auxiliary reinforcing agent; however, due to the high viscosity of the silicone rubber matrix, it will accelerate aging, cracking and powdering at high temperatures. Therefore, the slurry in this method is not suitable for preparing a coating with high bonding strength by a thermal spraying method, and the coating prepared by the brushing method suitable for the slurry has a low bonding strength; in addition, the coating mainly relies on hollow ceramic powder to provide thermal protection. In a more severe high-temperature erosion environment, the erosion resistance of the hollow ceramic powder is much lower than that of the solid ceramic powder. Therefore, the coating of this method is very easy to peel off under higher temperatures and more severe erosion environments, and the coating has poor ablation resistance. Compared with this, the present invention uses a spray granulation powder that is more suitable for spraying for low-pressure plasma spraying, the coating has high bonding strength, the obtained coating is denser, and the resistance to high-temperature erosion is better, and it can provide excellent protection in a more severe high-temperature erosion environment.

[0018] Instruction Manual

[0019] The drawings of the present invention are provided for illustrative purposes only, and the proportions and sizes of the layers in the drawings may not necessarily be consistent with the actual products.

[0020] Figure 1 It is a schematic structural diagram of the high bonding strength anti-oxidation and ablation composite coating prepared on the surface of the ceramic-based composite material in some specific embodiments of the present invention;

[0021] In the figure: 1: Ceramic matrix composite material; 2: Ultra-high temperature ceramic base coating reinforced by chopped carbon fiber coated with a shell; 3: Ultra-high temperature ceramic surface coating reinforced by chopped silicon carbide fiber coated with a shell. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0023] In a first aspect, the present invention provides a high bonding strength anti-oxidation ablation composite coating for ceramic matrix composite materials (abbreviated as high bonding strength anti-oxidation ablation composite coating), for example, Figure 1As shown; the high bonding strength and anti-oxidation and ablation composite coating includes, from the ceramic-based composite material (ceramic-based composite material matrix) 1 to the outside, a layer shell-coated short carbon fiber reinforced ultra-high temperature ceramic bottom coating (abbreviated as bottom coating) 2 and a layer shell-coated short silicon carbide fiber reinforced ultra-high temperature ceramic surface coating (abbreviated as surface coating) 3.

[0024] The present invention takes into account the large difference in thermal expansion coefficients between ultra-high temperature ceramics and ceramic-based composite materials. In the prior art, ultra-high temperature ceramic coatings prepared on the surface of ceramic-based composite materials all fail prematurely at the interface of the coating / ceramic-based composite materials during service due to the large difference in thermal expansion coefficients; however, the thermal expansion coefficients of carbon fibers are close to those of ultra-high temperature ceramic-based composite materials. Based on this, the present invention designs an ultra-high temperature ceramic coating reinforced with chopped carbon fibers coated with a layer shell as the bottom layer. The layer shell coated with chopped carbon fibers can improve the fracture toughness of the ultra-high temperature ceramic coating while alleviating the thermal expansion coefficient between the ultra-high temperature ceramic coating and the ceramic-based composite matrix, reducing the thermal mismatch stress between the interface of the ultra-high temperature ceramic coating and the ceramic-based composite material, effectively avoiding premature peeling of the interface of the coating / ceramic-based composite material, and effectively improving the bonding strength between the coating and the ceramic-based composite matrix. In addition, the present invention uses the layer shell coated with chopped carbon fibers instead of directly using chopped carbon fibers to enhance the ultra-high temperature ceramic coating. This is because the present invention finds that the weak interface between the layer shell and the chopped carbon fibers can deflect the cracks in the coating, further enhancing the bonding strength between the coating and the matrix. In addition, in order to further improve the high-temperature oxidation and ablation resistance of the ultra-high temperature ceramic coating, the present invention uses a layer shell coated with short-cut silicon carbide fibers reinforced ultra-high temperature ceramic coating as a surface layer. The present invention finds that while the layer shell coated with short-cut silicon carbide fibers improves the fracture toughness of the ultra-high temperature ceramic material, the silicon oxide formed by its oxidation is liquid or semi-liquid at high temperatures. This fluidity enables it to fill cracks or holes in the coating, further improving its high-temperature oxidation and ablation resistance. The interface between the layer shell and the short-cut silicon carbide fibers can also deflect the crack propagation path, which can further avoid peeling of the coating in an ablation environment. Compared with directly using short-cut silicon carbide fibers for reinforcement, it is more conducive to significantly improving the high-temperature ablation resistance and oxidation resistance of the composite coating.

[0025] According to some preferred embodiments, the shell material in the shell-coated chopped carbon fiber and / or the shell-coated chopped silicon carbide fiber is one or more of pyrolytic carbon (PyC), silicon carbide (SiC) and boron nitride (BN); of course, in the present invention, the shell material may not be limited to one or more of pyrolytic carbon (PyC), silicon carbide (SiC) and boron nitride (BN); in the present invention, the shell coating the chopped carbon fiber and the chopped silicon carbide fiber is prepared, for example, by chemical vapor deposition (CVD), and the thickness of the shell is, for example, 100 to 500 nm (for example, 100, 150, 200, 250, 300, 350, 400, 450 or 500 nm).

[0026] According to some preferred embodiments, the preparation of the shell-coated chopped carbon fiber is as follows: a shell with a thickness of 100 to 500 nm is deposited on the surface of the carbon fiber by chemical vapor deposition to obtain a shell-coated carbon fiber, and then the shell-coated carbon fiber is cut; the preparation of the shell-coated chopped silicon carbide fiber is as follows: a shell with a thickness of 100 to 500 nm is deposited on the surface of the silicon carbide fiber by chemical vapor deposition to obtain a shell-coated silicon carbide fiber, and then the shell-coated silicon carbide fiber is cut; in the present invention, for example, mechanical or water jet cutting equipment can be used to cut the shell-coated carbon fiber and the shell-coated silicon carbide fiber; the present invention does not specifically limit the process conditions for preparing the shell by chemical vapor deposition, and those skilled in the art can select as needed, as long as the shell can reach the target thickness.

[0027] According to some preferred embodiments, the length of the shell-coated chopped carbon fiber and / or the shell-coated chopped silicon carbide fiber is 1 μm to 10 μm (for example, 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 μm) and the diameter is 0.2 μm to 2 μm (for example, 0.2, 0.4, 0.6, 0.8, 1, 1.2, 1.4, 1.6, 1.8 or 2 μm).

[0028] According to some preferred embodiments, the ultra-high temperature ceramic in the ultra-high temperature ceramic base coating and / or the ultra-high temperature ceramic surface coating is one or more of high melting point carbides, borides and nitrides; preferably, the carbide is one or more of silicon carbide, zirconium carbide, hafnium carbide, tantalum carbide, titanium carbide and niobium carbide, the boride is one or more of zirconium boride, hafnium boride, tantalum boride, titanium boride and niobium boride, and the nitride is one or more of zirconium nitride, hafnium nitride, tantalum nitride, titanium nitride and niobium nitride.

[0029] According to some preferred embodiments, the shell-coated chopped carbon fiber reinforced ultra-high temperature ceramic bottom layer coating and the shell-coated chopped silicon carbide fiber reinforced ultra-high temperature ceramic surface layer coating are respectively formed on the surface of the ceramic-based composite material by low-pressure plasma spraying using shell-coated chopped carbon fiber reinforced ultra-high temperature ceramic powder and shell-coated chopped silicon carbide fiber reinforced ultra-high temperature ceramic powder as spraying materials; the shell-coated chopped carbon fiber reinforced ultra-high temperature ceramic powder is composited by shell-coated chopped carbon fiber and ultra-high temperature ceramic powder by spray granulation; The shell-coated chopped silicon carbide fiber reinforced ultra-high temperature ceramic powder is formed by compounding shell-coated chopped silicon carbide fibers and ultra-high temperature ceramic powder through spray granulation; the present invention does not specifically limit the spray granulation method, and technical personnel in this field can make a conventional selection; in the present invention, the shell-coated chopped carbon fibers and the shell-coated chopped silicon carbide fibers are respectively compounded with ultra-high temperature ceramic powder through a spray granulation method to form shell-coated chopped carbon fiber reinforced ultra-high temperature ceramic powder suitable for low-pressure plasma spraying and shell-coated chopped silicon carbide fiber reinforced ultra-high temperature ceramic powder.

[0030] According to some preferred embodiments, the median particle size D50 of the shell-coated chopped carbon fiber reinforced ultra-high temperature ceramic powder and / or the shell-coated chopped silicon carbide fiber reinforced ultra-high temperature ceramic powder is 5 to 50 μm (for example, 5, 10, 15, 20, 25, 30, 35, 40, 45 or 50 μm).

[0031] According to some preferred embodiments, in the layer shell coated short carbon fiber reinforced ultra-high temperature ceramic bottom layer coating, the mass ratio of the layer shell coated short carbon fiber to the ultra-high temperature ceramic is (0.2-9):1; in the layer shell coated short silicon carbide fiber reinforced ultra-high temperature ceramic surface layer coating, the mass ratio of the layer shell coated short silicon carbide fiber to the ultra-high temperature ceramic is (0.2-9):1; specifically, in the layer shell coated short carbon fiber reinforced ultra-high temperature ceramic powder and the layer shell coated short silicon carbide fiber reinforced ultra-high temperature ceramic powder of the present invention, the mass ratio of the layer shell coated short carbon fiber to the ultra-high temperature ceramic powder is 1: 5 to 9:1 (e.g., 1:5, 1:4, 1:3, 1:2, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1 or 9:1) to suit ceramic matrix composites with different thermal expansion coefficients, the mass ratio of the shell-coated chopped silicon carbide fibers to the ultra-high temperature ceramic powder is 1:5 to 9:1 (e.g., 1:5, 1:4, 1:3, 1:2, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1 or 9:1) to match the anti-oxidation and ablation properties at different service temperatures, thereby enhancing the mechanical properties and anti-ablation properties of the coating.

[0032] According to some preferred embodiments, the thickness of the layer shell coated with chopped carbon fiber reinforced ultra-high temperature ceramic bottom layer coating and / or the layer shell coated with chopped silicon carbide fiber reinforced ultra-high temperature ceramic surface layer coating is 50 to 500 μm (for example, 50, 100, 150, 200, 250, 300, 350, 400, 450 or 500 μm); specifically, in order to ensure that the layer shell coated with chopped carbon fiber reinforced ultra-high temperature ceramic bottom layer coating can minimize the mismatch of thermal expansion coefficients between ultra-high temperature ceramics and ceramic-based composite materials, it is preferred that the layer shell coated with chopped carbon fiber reinforced ultra-high temperature ceramic bottom layer The thickness of the coating is 50 to 500 μm (for example, 50, 100, 150, 200, 250, 300, 350, 400, 450 or 500 μm); to ensure that the shell-coated short-cut silicon carbide fiber reinforced ultra-high temperature ceramic surface coating has excellent anti-oxidation and ablation properties and prevent the oxidation and ablation failure of the ceramic-based composite material under high temperature, preferably, the thickness of the shell-coated short-cut silicon carbide fiber reinforced ultra-high temperature ceramic surface coating is 50 to 500 μm (for example, 50, 100, 150, 200, 250, 300, 350, 400, 450 or 500 μm).

[0033] According to some preferred embodiments, the ultra-high temperature ceramic base coating and / or the ultra-high temperature ceramic surface coating further comprises yttrium aluminum garnet powder, and the volume fraction of yttrium aluminum garnet powder in the ultra-high temperature ceramic base coating and / or the ultra-high temperature ceramic surface coating is 4-8% (for example, 4%, 5%, 6%, 7% or 8%); in the present invention, preferably, the particle size of the yttrium aluminum garnet powder is 1-3 μm; the present invention finds that adding small-particle yttrium aluminum garnet powder during the spraying process of the ultra-high temperature ceramic base coating and / or the ultra-high temperature ceramic surface coating can better fill the ultra-high temperature ceramic and layer shell. The pores and defects between the coated chopped fibers are improved to improve the density and bonding strength of the coating; on the other hand, since the position of oxygen ions in the yttrium aluminum garnet lattice is relatively fixed and the yttrium aluminum garnet has poor ability to transport oxygen ions, it can avoid the transmission of oxygen from the defect position of the coating to the interior of the coating, thereby optimizing the coating's antioxidant properties; in addition, since the melting point of yttrium aluminum garnet is about 1950°C, when used at temperatures exceeding 2000°C, the molten yttrium aluminum garnet can further fill microcracks and prevent further crack expansion, which enables the coating to maintain stable anti-ablation properties in extremely high temperature environments, thereby further improving the service life and reliability of the material.

[0034] In the present invention, preferably, the volume fraction of yttrium aluminum garnet powder contained in the ultra-high temperature ceramic base coating and / or the ultra-high temperature ceramic surface coating is 4-8%. The present invention finds that although adding yttrium aluminum garnet powder to the ultra-high temperature ceramic base coating and / or the ultra-high temperature ceramic surface coating is beneficial to further improve the high temperature oxidation and ablation resistance and bonding strength of the high bonding strength anti-oxidation and ablation composite coating, the control of the amount of yttrium aluminum garnet powder is very important. The possible reason is that the addition of an appropriate amount of yttrium aluminum garnet powder further blocks the diffusion of oxygen, thereby improving the oxidation resistance of the coating and extending the service life of the coating at high temperatures. If the volume fraction of yttrium aluminum garnet powder is low, the effect of improving the oxidation resistance and healing microcracks of the coating is not obvious. If the volume fraction of yttrium aluminum garnet is too high, the brittleness of the coating will increase. The large difference in thermal expansion coefficient between yttrium aluminum garnet and ultra-high temperature ceramics will lead to excessive thermal mismatch stress, thereby reducing the bonding strength and impact resistance of the coating, which will lead to degradation of the coating performance.

[0035] In the present invention, a shell-coated ultra-high temperature ceramic bottom layer coating reinforced with chopped carbon fibers and a shell-coated ultra-high temperature ceramic top layer coating reinforced with chopped silicon carbide fibers are obtained for the first time by a low-pressure plasma spraying method; in the low-pressure plasma spraying preparation method, the low-pressure plasma spraying method has the advantages of large spraying power, high jet temperature, and fast speed, and has the advantages of high deposition efficiency and low cost; the low-pressure, inert gas coating preparation environment can effectively avoid oxidation of the sprayed powder and improve the purity of the coating; in addition, the powder melts more fully under the action of the high-energy plasma beam, and the coating porosity is lower, which avoids the generation of internal defects in the coating and reduces the risk of peeling of the coating along the defect position in a high-temperature ablation environment. At the same time, it also reduces the possibility of failure along the interface between the coating and the ceramic-based composite material matrix, and more effectively ensures that the composite coating has high bonding strength and excellent anti-oxidation and ablation properties.

[0036] Therefore, the present invention provides in a second aspect a method for preparing the high bonding strength anti-oxidation and ablation composite coating for ceramic matrix composite materials according to the first aspect of the present invention, the method comprising the following steps:

[0037] (1) grinding, cleaning and drying the ceramic-based composite material (ceramic-based composite material matrix) to obtain a pretreated ceramic-based composite material; specifically, pretreating the ceramic-based composite material: after grinding the ceramic-based composite material, ultrasonically cleaning it in an organic solvent for 10 to 15 minutes, and then drying it in an oven to obtain a pretreated ceramic-based composite material;

[0038] (2) A layer of shell-coated short carbon fiber reinforced ultra-high temperature ceramic base coating and a layer of shell-coated short silicon carbide fiber reinforced ultra-high temperature ceramic surface coating are sequentially prepared on the surface of the pretreated ceramic-based composite material by low-pressure plasma spraying, thereby obtaining the high bonding strength anti-oxidation and ablation composite coating (abbreviated as high bonding strength anti-oxidation and ablation composite coating) on ​​the surface of the ceramic-based composite material; in the present invention, specifically, the pretreated ceramic-based composite substrate is fixed on a workbench in a vacuum chamber of a low-pressure plasma spraying device; a layer of shell-coated short carbon fiber reinforced ultra-high temperature ceramic base coating is first prepared on the surface of the pretreated ceramic-based composite material by low-pressure plasma spraying technology to improve the fracture toughness of the coating and reduce the thermal expansion coefficient, thereby improving the bonding strength between the coating and the substrate; on top of the ultra-high temperature ceramic base coating, a layer of shell-coated short silicon carbide fiber reinforced ultra-high temperature ceramic surface coating is continuously prepared by low-pressure plasma spraying technology to further enhance the coating's resistance to high-temperature ablation and long-term oxidation, thereby obtaining the high bonding strength anti-oxidation and ablation composite coating on the surface of the ceramic-based composite material.

[0039] The high bonding strength and anti-oxidation and ablation composite coating described in the present invention adopts ultra-high temperature ceramic powder reinforced by shell-coated short-cut carbon fiber and shell-coated short-cut silicon carbide fiber as spraying materials, and utilizes low-pressure plasma spraying technology to sequentially prepare a base layer and a surface layer on the surface of the ceramic-based composite material, which significantly improves the high-temperature ablation resistance and oxidation resistance of the coating, while utilizing the weak interface between the shell layer and the fiber to deflect cracks in the coating, further enhancing the bonding strength between the coating and the substrate, and further improving the high-temperature oxidation and ablation resistance of the coating; the method of the present invention has the advantages of high deposition efficiency, low cost, and high coating density, and can realize the integrated preparation of high-bonding strength and anti-oxidation and ablation composite coatings.

[0040] According to some preferred embodiments, the ceramic matrix composite material is a carbon fiber reinforced silicon carbide ceramic matrix composite material (C / SiC ceramic matrix composite material) or a carbon fiber reinforced ultra-high temperature ceramic matrix composite material; the density of the ceramic matrix composite material is 1.8 to 5.0 g / cm 3 (e.g., 1.8, 2.0, 2.2, 2.4, 2.6, 2.8, 3.0, 3.2, 3.4, 3.6, 3.8, 4.0, 4.2, 4.4, 4.6, 4.8, or 5.0 g / cm 3 ); the polishing is performed using sandpaper; the cleaning is ultrasonic cleaning in acetone and / or ethanol for 10 to 15 minutes; and / or the drying temperature is 100 to 150°C.

[0041] According to some specific embodiments, the ceramic-based composite material is pretreated before spraying, and the pretreatment steps are: first, the surface of the ceramic-based composite material is polished, and then the polished ceramic-based composite material is cleaned in an organic solvent, and then placed in an oven for drying, which is beneficial to remove impurities on the surface of the ceramic-based composite material and improve the bonding force between the coating and the substrate; preferably, the surface of the ceramic-based composite material is polished with 400#, 800#, and 1000# sandpaper in sequence, and then ultrasonically cleaned in an organic solvent such as acetone or ethanol for 10 to 15 minutes (for example, 10, 11, 12, 13, 14 or 15 minutes), and then dried in an oven at 100 to 150°C (for example, 100, 110, 120, 130, 140 or 150°C).

[0042] According to some preferred embodiments, during the low-pressure plasma spraying process, plasma jet heating is used to make the surface temperature of the pretreated ceramic-based composite material reach 600-1000°C (for example, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C or 1000°C) to increase the spreading range of the droplets after the powder melts on the substrate, improve the bonding strength between the coating and the substrate, and reduce the porosity and defects of the coating.

[0043] According to some preferred embodiments, during the low-pressure plasma spraying process, the absolute pressure in the spraying chamber (vacuum chamber of the spraying equipment) is 1×10 2 ~2×10 3 Specifically, in the process of preparing the coating by low-pressure plasma spraying, the pressure in the vacuum chamber of the spraying equipment is first reduced to 1-10Pa (e.g., 1, 2, 4, 6, 8 or 10Pa), and then argon is filled into the vacuum chamber to make the absolute pressure in the vacuum chamber 1×10 2 ~2×10 3 Pa (e.g. 1×10 2 , 4×10 2 , 8×10 2 , 1.2×10 3 , 1.6×10 3 or 2×10 3 Pa).

[0044] According to some preferred embodiments, in the process of preparing the layer shell coated short carbon fiber reinforced ultra-high temperature ceramic bottom layer coating and / or the layer shell coated short silicon carbide fiber reinforced ultra-high temperature ceramic surface layer coating, argon and helium are used as plasma gases, the flow rate of argon is 20 to 50 L / min (for example, 20, 25, 30, 35, 40, 45 or 50 L / min), the flow rate of helium is 10 to 40 L / min (for example, 10, 15, 20, 25, 30, 35 or 40 L / min), the spraying distance is 400 to 1000 mm (for example, 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950 or 1000 mm), and the speed of the rotating table is The arc voltage of the low-pressure plasma spraying equipment is 20-40V (20, 25, 30, 35 or 40V), and the arc current is 800-1600A (e.g., 800, 900, 1000, 1100, 1200, 1300, 1400, 1500 or 1600A). The powder feeding rate of the shell-coated chopped carbon fiber reinforced ultrahigh temperature ceramic powder and / or the shell-coated chopped silicon carbide fiber reinforced ultrahigh temperature ceramic powder is 10-20g / min (e.g., 10, 12, 14, 16, 18 or 20g / min). In the present invention, argon is used as the powder feeding carrier gas during powder feeding.

[0045] According to some specific embodiments, the method for preparing the high bonding strength anti-oxidation ablation composite coating of the present invention comprises the following steps:

[0046] (a) Pretreatment of the surface of the ceramic matrix composite material substrate: The surface of the ceramic matrix composite material substrate is polished using 400, 800, and 1000 sandpapers in sequence, ultrasonically cleaned in an organic solvent such as acetone or ethanol for 10 to 15 minutes, and then dried in an oven at 100 to 150° C. to obtain a pretreated ceramic matrix composite material.

[0047] (b) fixing the pretreated ceramic matrix composite material on a rotating table in a vacuum chamber of a low-pressure plasma spraying device; before spraying, the vacuum chamber of the low-pressure plasma spraying device is first evacuated to 1-10 Pa, and then filled with argon gas to 1×10 2 ~2×10 3 Pa.

[0048] (c) The surface of the ceramic matrix composite material substrate pretreated by plasma jet heating is heated to 600-1000°C.

[0049] (d) First, a shell-coated short carbon fiber reinforced ultra-high temperature ceramic powder with a median particle size (D50) of 5 to 50 μm is loaded into a powder feeder of a low-pressure plasma spraying device, and deposited onto the surface of a ceramic-based composite material matrix by a low-pressure plasma spraying method to prepare a shell-coated short carbon fiber reinforced ultra-high temperature ceramic base coating with a thickness of about 50 to 500 μm.

[0050] (e) Subsequently, the shell-coated short-cut silicon carbide fiber reinforced ultra-high temperature ceramic powder with a median particle size (D50) of 5 to 50 μm is loaded into the powder feeder of the low-pressure plasma spraying equipment, and is deposited on the shell-coated short-cut carbon fiber reinforced ultra-high temperature ceramic base coating of the ceramic-based composite material substrate by a low-pressure plasma spraying method to prepare a shell-coated short-cut silicon carbide fiber reinforced ultra-high temperature ceramic top coating with a thickness of about 50 to 500 μm, and the spraying is terminated to obtain the high bonding strength and anti-oxidation and ablation composite coating on the surface of the ceramic-based composite material.

[0051] (f) After the ceramic-based composite substrate and its coating are cooled to below 400° C., the vacuum chamber pressure is restored to atmospheric pressure, and finally the ceramic-based composite material on which the high-bonding-strength anti-oxidation and ablation composite coating is deposited is taken out.

[0052] The present invention in a third aspect provides a high bonding strength anti-oxidation and ablation composite coating for ceramic-based composite materials, which is prepared by the preparation method described in the second aspect of the present invention.

[0053] According to some preferred embodiments, the bonding strength of the high bonding strength anti-oxidation ablation composite coating is not less than 50 MPa; the porosity of the high bonding strength anti-oxidation ablation composite coating is less than 10%; the linear ablation rate of the high bonding strength anti-oxidation ablation composite coating in the oxyacetylene ablation test at a coating surface temperature of 2000°C is less than 1×10 -3 mm / s.

[0054] The present invention will be further described below by way of examples, but the protection scope of the present invention is not limited to these embodiments. The present invention may also have other various embodiments, and those skilled in the art may make various corresponding changes and deformations according to the present invention without departing from the spirit and essence of the present invention, but these corresponding changes and deformations shall all belong to the protection scope of the claims attached to the present invention.

[0055] Example 1

[0056] ① Pretreated ceramic matrix composite material: the size is 30mm (diameter) × 5mm (thickness), and the density is 1.88g / cm 3A carbon fiber reinforced silicon carbide ceramic matrix composite material (C / SiC) was used as a matrix, and the surface of the matrix was polished with 400#, 800#, and 1000# sandpapers in sequence, then ultrasonically cleaned in acetone for 10 minutes, and finally dried in an oven at 120°C to obtain a pretreated ceramic matrix composite material.

[0057] ②Prepare the spraying material: Use the CVD method to prepare a PyC layer shell with a thickness of 300nm on the surface of the carbon fiber to obtain a PyC layer shell coated carbon fiber, and prepare a SiC layer shell with a thickness of 300nm on the surface of the silicon carbide fiber to obtain a SiC layer shell coated silicon carbide fiber; then use a mechanical cutting device to cut the PyC layer shell coated carbon fiber and the SiC layer shell coated silicon carbide fiber to obtain a PyC layer shell coated short carbon fiber with a length of 5μm and a diameter of 0.8μm, and obtain a SiC layer shell coated short silicon carbide fiber with a length of 8μm and a diameter of 1μm. The PyC layer shell coated short carbon fiber reinforced hafnium carbide (HfC) ultra-high temperature ceramic powder is obtained by a spray granulation method, wherein the mass ratio of the PyC layer shell coated short carbon fiber to the HfC ultra-high temperature ceramic powder is 1:3, and the median particle size (D50) of the powder is 20μm. The HfC ultra-high temperature ceramic powder reinforced with SiC layer shell coated chopped silicon carbide fibers was obtained by a spray granulation method, wherein the mass ratio of SiC layer shell coated chopped silicon carbide fibers to HfC ultra-high temperature ceramic powder was 1:4, and the median particle size (D50) of the powder was 25 μm.

[0058] ③Preparation of bottom coating by low-pressure plasma spraying: The pretreated ceramic matrix composite substrate obtained in step ① is fixed on the rotating table of the vacuum chamber of the low-pressure plasma spraying equipment; before spraying, the vacuum chamber is evacuated to 5Pa, and then filled with argon gas to an absolute pressure of 8×10 2 Pa. The surface of the ceramic matrix composite material substrate pretreated by plasma jet heating was heated to 800°C. Argon and helium were used as plasma gases (argon flow rate 30L / min, helium flow rate 20L / min), the spraying distance was 600mm, the rotating table speed was 10r / min, the arc voltage was 30V, the arc current was 1000A, and after the plasma beam was stable, the powder feeder containing the PyC layer shell coated short carbon fiber reinforced HfC ultra-high temperature ceramic powder obtained in step ② was turned on, the powder feeding rate was 12g / min, the deposition time was 2min, and a PyC layer shell coated short carbon fiber reinforced HfC ultra-high temperature ceramic bottom coating with a thickness of 200μm was prepared.

[0059] ④ Preparation of the surface coating by low-pressure plasma spraying: keeping the absolute pressure in the vacuum chamber unchanged, the surface coating is prepared with the same plasma gas ratio, spraying distance and turntable speed as in step ③, arc voltage of 30V, arc current of 1100A, and after the plasma beam is stable, the powder feeder containing the SiC layer shell coated short-cut silicon carbide fiber reinforced HfC ultra-high temperature ceramic powder obtained in step ③ is turned on, the powder feeding rate is 15g / min, the deposition time is 1.5min, and a SiC layer shell coated short-cut silicon carbide fiber reinforced HfC ultra-high temperature ceramic bottom coating with a thickness of 150μm is prepared on the basis of the PyC layer shell coated short-cut carbon fiber reinforced HfC ultra-high temperature ceramic top layer coating, thereby obtaining the high bonding strength and anti-oxidation and ablation composite coating on the surface of the C / SiC ceramic-based composite material.

[0060] ⑤ Cooling and taking out: After the vacuum chamber is cooled to room temperature, the atmospheric pressure is restored and the C / SiC ceramic-based composite material with the high bonding strength anti-oxidation and ablation composite coating is taken out.

[0061] Performance test: The present invention uses an electronic universal material testing machine to test the bonding strength of the high bonding strength anti-oxidation ablation composite coating described in this embodiment, and the result is 60MPa. The overall porosity of the high bonding strength anti-oxidation ablation composite coating in this embodiment is calculated by image method based on the cross-sectional micromorphology of the coating, and is 8%; the C / SiC ceramic-based composite material with the high bonding strength anti-oxidation ablation composite coating is subjected to oxyacetylene ablation test according to GJB 323 standard, the coating surface temperature is 2000℃, the test time is 600s, and the linear ablation rate of the high bonding strength anti-oxidation ablation composite coating is measured to be 0.8×10 -3 mm / s.

[0062] Example 2

[0063] Embodiment 2 is substantially the same as Embodiment 1, except that:

[0064] In step ③, the arc voltage is 35 V, the arc current is 1200 A, and the other process parameters are the same, and a PyC layer shell with a thickness of 190 μm and a short carbon fiber reinforced HfC ultra-high temperature ceramic base coating is prepared.

[0065] In step ④, the arc voltage is 35 V, the arc current is 1300 A, and the other process parameters are the same, and a SiC layer shell with a thickness of 140 μm and short-cut silicon carbide fiber reinforced HfC ultra-high temperature ceramic surface coating is prepared.

[0066] The bonding strength, porosity and anti-ablation performance of the high bonding strength anti-oxidation and ablation composite coating prepared in this embodiment were tested using the same testing method as in Example 1. The performance test results are shown in Table 1.

[0067] Example 3

[0068] Embodiment 3 is substantially the same as Embodiment 1, except that:

[0069] In step ③, the same process parameters were used and the deposition time was 3 min to prepare a 300 μm thick PyC layer shell-coated chopped carbon fiber reinforced HfC ultra-high temperature ceramic base coating.

[0070] In step ④, using the same process parameters and a deposition time of 3 min, a 300 μm thick SiC layer shell-coated chopped silicon carbide fiber-reinforced HfC ultra-high temperature ceramic surface coating was prepared.

[0071] The bonding strength, porosity and anti-ablation performance of the high bonding strength anti-oxidation and ablation composite coating prepared in this embodiment were tested using the same testing method as in Example 1. The performance test results are shown in Table 1.

[0072] Example 4

[0073] Embodiment 4 is substantially the same as Embodiment 1, except that:

[0074] In step ②, a spray granulation method is used to obtain a PyC layer shell coated short carbon fiber reinforced zirconium carbide (ZrC) ultra-high temperature ceramic powder, wherein the length of the PyC layer shell coated short carbon fiber is 6μm and the diameter is 1μm, the mass ratio of the PyC layer shell coated short carbon fiber to the ZrC ultra-high temperature ceramic powder is 1:3, and the median particle size (D50) of the powder is 22μm. A SiC layer shell coated short silicon carbide fiber reinforced zirconium boride (ZrB2) ultra-high temperature ceramic powder is obtained by a spray granulation method, wherein the length of the SiC layer shell coated short silicon carbide fiber is 8μm and the diameter is 1.2μm, the mass ratio of the SiC layer shell coated short silicon carbide fiber to the ZrB2 ultra-high temperature ceramic powder is 1:4, and the median particle size (D50) of the powder is 27μm.

[0075] In step ③, the same process parameters were used and the deposition time was 2 min to prepare a 180 μm thick PyC layer shell-coated short carbon fiber reinforced ZrC ultra-high temperature ceramic base coating.

[0076] In step ④, using the same process parameters and a deposition time of 1.5 min, a SiC layer shell with a thickness of 140 μm and a ZrB2 ultra-high temperature ceramic surface coating reinforced with chopped silicon carbide fibers was prepared.

[0077] The bonding strength, porosity and anti-ablation performance of the high bonding strength anti-oxidation and ablation composite coating prepared in this embodiment were tested using the same testing method as in Example 1. The performance test results are shown in Table 1.

[0078] Example 5

[0079] Example 5 is substantially the same as Example 1, except that:

[0080] In step ①, select the size of 30mm (diameter) × 5mm (thickness) and the density of 2.52g / cm 3 The C / ZrC-SiC carbon fiber reinforced ceramic matrix composite material is used as the matrix, and other pretreatment methods remain unchanged to obtain the pretreated ceramic matrix composite material.

[0081] In step ②, a spray granulation method is used to obtain a tantalum nitride (TaN) ultra-high temperature ceramic powder reinforced with PyC shell-coated short carbon fibers, wherein the length of the PyC shell-coated short carbon fibers is 10 μm and the diameter is 1.0 μm, the mass ratio of the PyC shell-coated short carbon fibers to the TaN ultra-high temperature ceramic powder is 1:1, and the median particle size (D50) of the powder is 25 μm. A SiC shell-coated short silicon carbide fiber-reinforced hafnium boride (HfB2) ultra-high temperature ceramic powder is obtained by a spray granulation method, wherein the length of the SiC shell-coated short silicon carbide fibers is 8 μm and the diameter is 1 μm, the mass ratio of the SiC shell-coated short silicon carbide fibers to the HfB2 ultra-high temperature ceramic powder is 1:1, and the median particle size (D50) of the powder is 30 μm.

[0082] In step ③, the same process parameters were used and the deposition time was 2.2 min to prepare a 180 μm thick PyC layer shell-coated short carbon fiber reinforced TaN ultra-high temperature ceramic base coating.

[0083] In step ④, using the same process parameters and a deposition time of 1.7 min, a SiC layer shell with a thickness of 140 μm and short-cut silicon carbide fiber-reinforced HfB2 ultra-high temperature ceramic surface coating was prepared.

[0084] The bonding strength, porosity and anti-ablation performance of the high bonding strength anti-oxidation and ablation composite coating prepared in this embodiment were tested using the same testing method as in Example 1. The performance test results are shown in Table 1.

[0085] Example 6

[0086] Embodiment 6 is substantially the same as Embodiment 1, except that:

[0087] In step ②: using the CVD method, a boron nitride (BN) layer shell with a thickness of 300nm is prepared on the surface of the carbon fiber to obtain a BN layer shell coated carbon fiber, and a SiC layer shell with a thickness of 300nm is prepared on the surface of the silicon carbide fiber to obtain a SiC layer shell coated silicon carbide fiber; then a mechanical cutting device is used to cut the BN layer shell coated carbon fiber and the SiC layer shell coated silicon carbide fiber to obtain a BN layer shell coated short carbon fiber with a length of 5μm and a diameter of 0.8μm, and a SiC layer shell coated short silicon carbide fiber with a length of 8μm and a diameter of 1μm. The spray granulation method is used to obtain a BN layer shell coated short carbon fiber reinforced hafnium carbide (HfC) ultra-high temperature ceramic powder, wherein the mass ratio of the BN layer shell coated short carbon fiber to the HfC ultra-high temperature ceramic powder is 1:3, and the median particle size (D50) of the powder is 20μm. The HfC ultra-high temperature ceramic powder reinforced with SiC layer shell coated chopped silicon carbide fibers was obtained by a spray granulation method, wherein the mass ratio of SiC layer shell coated chopped silicon carbide fibers to HfC ultra-high temperature ceramic powder was 1:4, and the median particle size (D50) of the powder was 25 μm.

[0088] In step ③: the pretreated ceramic matrix composite substrate obtained in step ① is fixed on the rotating table of the vacuum chamber of the low-pressure plasma spraying equipment; before spraying, the vacuum chamber is evacuated to 5 Pa, and then filled with argon gas to an absolute pressure of 8×10 2 Pa. The surface of the ceramic matrix composite material substrate pretreated by plasma jet heating was heated to 800°C. Argon and helium were used as plasma gases (argon flow rate 30L / min, helium flow rate 20L / min), the spraying distance was 600mm, the rotating table speed was 10r / min, the arc voltage was 30V, the arc current was 1000A, and after the plasma beam was stable, the powder feeder containing the BN layer shell coated short carbon fiber reinforced HfC ultra-high temperature ceramic powder obtained in step ② was turned on, and the powder feeding rate was 12g / min, and a BN layer shell coated short carbon fiber reinforced HfC ultra-high temperature ceramic bottom coating with a thickness of 200μm was prepared.

[0089] In step ④: keep the absolute pressure in the vacuum chamber unchanged, prepare the surface coating with the same plasma gas ratio, spraying distance and turntable speed as in step ③, arc voltage 30V, arc current 1100A, and after the plasma beam is stable, start the powder feeder containing the SiC layer shell coated short silicon carbide fiber reinforced HfC ultra-high temperature ceramic powder obtained in step ③, the powder feeding rate is 15g / min, and prepare a SiC layer shell coated short silicon carbide fiber reinforced HfC ultra-high temperature ceramic surface coating with a thickness of 150μm on the basis of the BN layer shell coated short carbon fiber reinforced HfC ultra-high temperature ceramic bottom coating, thereby obtaining the high bonding strength and anti-oxidation and ablation composite coating on the surface of the C / SiC ceramic-based composite material.

[0090] The bonding strength, porosity and anti-ablation performance of the high bonding strength anti-oxidation and ablation composite coating prepared in this embodiment were tested using the same testing method as in Example 1. The performance test results are shown in Table 1.

[0091] Example 7

[0092] Example 7 is substantially the same as Example 1, except that:

[0093] ② Prepare the spraying material: Use the CVD method to prepare a PyC shell with a thickness of 300 nm on the surface of the carbon fiber to obtain PyC shell-coated carbon fiber, and prepare a SiC shell with a thickness of 300 nm on the surface of the silicon carbide fiber to obtain SiC shell-coated silicon carbide fiber; then use mechanical cutting equipment to cut the PyC shell-coated carbon fiber and the SiC shell-coated silicon carbide fiber to obtain PyC shell-coated chopped carbon fiber with a length of 5 μm and a diameter of 0.8 μm, and obtain SiC shell-coated chopped silicon carbide fiber with a length of 8 μm and a diameter of 1 μm. A spray granulation method is used to compound PyC layer shell coated chopped carbon fibers, hafnium carbide (HfC) ultra-high temperature ceramic powder and yttrium aluminum garnet powder to obtain PyC layer shell coated chopped carbon fibers reinforced with hafnium carbide (HfC) ultra-high temperature ceramic powder, wherein the mass ratio of the PyC layer shell coated chopped carbon fibers to the HfC ultra-high temperature ceramic powder is 1:3, the volume fraction of yttrium aluminum garnet powder in the PyC layer shell coated chopped carbon fibers reinforced with hafnium carbide (HfC) ultra-high temperature ceramic powder is 6%, and the median particle size (D50) of the powder is 17 μm. A spray granulation method is used to compound SiC layer shell coated chopped silicon carbide fibers, hafnium carbide (HfC) ultra-high temperature ceramic powder and yttrium aluminum garnet powder to obtain SiC layer shell coated chopped silicon carbide fiber reinforced HfC ultra-high temperature ceramic powder, wherein the mass ratio of SiC layer shell coated chopped silicon carbide fibers to HfC ultra-high temperature ceramic powder is 1:4, the volume fraction of yttrium aluminum garnet powder in the SiC layer shell coated chopped silicon carbide fiber reinforced HfC ultra-high temperature ceramic powder is 6%, and the median particle size (D50) of the powder is 21μm.

[0094] The bonding strength, porosity and anti-ablation performance of the high bonding strength anti-oxidation and ablation composite coating prepared in this embodiment were tested using the same testing method as in Example 1. The performance test results are shown in Table 1.

[0095] Comparative Example 1

[0096] ① Pretreated ceramic matrix composite material: the size is 30mm (diameter) × 5mm (thickness), and the density is 1.88g / cm 3A carbon fiber reinforced silicon carbide ceramic matrix composite material (C / SiC) was used as a matrix, and the surface of the matrix was polished with 400#, 800#, and 1000# sandpapers in sequence, then ultrasonically cleaned in acetone for 10 minutes, and finally dried in an oven at 120°C to obtain a pretreated ceramic matrix composite material.

[0097] ②Prepare spraying materials: Use a spray granulation method to obtain short carbon fiber reinforced hafnium carbide (HfC) ultra-high temperature ceramic powder, the short carbon fiber length is 5μm, the diameter is 0.8μm, the mass ratio of short carbon fiber to HfC ultra-high temperature ceramic powder is 1:3, and the median particle size (D50) of the powder is 20μm. Use a spray granulation method to obtain short silicon carbide fiber reinforced HfC ultra-high temperature ceramic powder, wherein the short silicon carbide fiber length is 8μm, the diameter is 1μm, the mass ratio of short silicon carbide fiber to HfC ultra-high temperature ceramic powder is 1:4, and the median particle size (D50) of the powder is 25μm.

[0098] ③Preparation of base coating by atmospheric plasma spraying: Fix the pretreated ceramic matrix composite material substrate obtained in step ① on the operating table of the atmospheric plasma spraying equipment; the spraying pressure is atmospheric pressure. During spraying, argon is used as plasma gas, hydrogen is used as auxiliary gas, argon flow rate is 40L / min, hydrogen flow rate is 7.5L / min, spraying distance is 800mm, arc voltage is 40V, arc current is 700A, after the plasma beam is stable, open the powder feeder equipped with the short carbon fiber reinforced HfC ultra-high temperature ceramic powder obtained in step ②, the powder feeding rate is 15g / min, the deposition time is 5min, and a short carbon fiber reinforced HfC ultra-high temperature ceramic base coating with a thickness of 200μm is prepared.

[0099] ④ Preparation of the surface coating by atmospheric plasma spraying: maintaining the same plasma gas flow rate, auxiliary gas flow rate, spraying distance as step ③, arc voltage 42V, arc current 750A to prepare the surface coating, and after the plasma beam is stable, open the powder feeder containing the chopped silicon carbide fiber reinforced HfC ultra-high temperature ceramic powder obtained in step ②, the powder feeding rate is 18g / min, the deposition time is 4min, and a chopped silicon carbide fiber reinforced HfC ultra-high temperature ceramic surface coating with a thickness of 150μm is prepared on the basis of the chopped carbon fiber reinforced HfC ultra-high temperature ceramic base coating, thereby obtaining an antioxidant ablation composite coating on the surface of the C / SiC ceramic-based composite material.

[0100] ⑤ Cooling and taking out: After the coating and the substrate are cooled, the C / SiC ceramic-based composite material with the anti-oxidation and ablation composite coating is taken out from the operating table.

[0101] The bonding strength, porosity and anti-ablation performance of the anti-oxidation ablation composite coating prepared in this comparative example were tested using the same testing method as in Example 1. The performance test results are shown in Table 1.

[0102] Comparative Example 2

[0103] ① Pretreated ceramic matrix composite material: the size is 30mm (diameter) × 5mm (thickness), and the density is 1.88g / cm 3 A carbon fiber reinforced silicon carbide ceramic matrix composite material (C / SiC) was used as a matrix, and the surface of the matrix was polished with 400#, 800#, and 1000# sandpapers in sequence, then ultrasonically cleaned in acetone for 10 minutes, and finally dried in an oven at 120°C to obtain a pretreated ceramic matrix composite material.

[0104] ②Prepare spraying materials: Use HfC ultra-high temperature ceramic powder after spray granulation, with a median particle size (D50) of 20 μm.

[0105] ③ Preparation of coating by low-pressure plasma spraying: The pretreated ceramic matrix composite substrate obtained in step ① is fixed on the rotating table of the vacuum chamber of the low-pressure plasma spraying equipment; before spraying, the vacuum chamber is evacuated to 5Pa, and then filled with argon gas to an absolute pressure of 8×10 2 Pa. The surface of the ceramic matrix composite material substrate pretreated by plasma jet heating was heated to 800°C. Argon and helium were used as plasma gases (argon flow rate 30L / min, helium flow rate 20L / min), the spraying distance was 600mm, the rotating table speed was 10r / min, the arc voltage was 30V, the arc current was 1000A, and after the plasma beam was stable, the powder feeder containing the HfC ultra-high temperature ceramic powder in step ② was turned on, the powder feeding rate was 12g / min, and the deposition time was 3.5min, and a HfC ultra-high temperature ceramic coating with a thickness of 350μm was prepared.

[0106] ④ Cooling and taking out: After the vacuum chamber is cooled to room temperature, the atmospheric pressure is restored and the C / SiC ceramic matrix composite material with the HfC ultra-high temperature ceramic coating is taken out.

[0107] The bonding strength, porosity and ablation resistance of the HfC ultrahigh temperature ceramic coating prepared in this comparative example were tested using the same testing method as in Example 1. The performance test results are shown in Table 1.

[0108] Comparative Example 3

[0109] Comparative Example 3 is substantially the same as Comparative Example 2, except that:

[0110] ② Prepare spraying materials: Use a spray granulation method to obtain short-cut carbon fiber reinforced HfC ultra-high temperature ceramic powder, wherein the length of the short-cut carbon fiber is 5 μm, the diameter is 0.8 μm, the mass ratio of the short-cut carbon fiber to the HfC ceramic powder is 1:3, and the median particle size (D50) of the powder is 20 μm.

[0111] In step ③, the same process parameters are used, except that after the plasma beam is stabilized, the powder feeder containing the HfC ultra-high temperature ceramic powder reinforced with short-cut carbon fiber in step ② is turned on, the deposition time is 3.5 min, and a short-cut carbon fiber reinforced HfC coating with a thickness of 350 μm is prepared.

[0112] The bonding strength, porosity and ablation resistance of the chopped carbon fiber reinforced HfC coating prepared in this comparative example were tested by the same testing method as in Example 1. The performance test results are shown in Table 1.

[0113] Comparative Example 4

[0114] Comparative Example 4 is substantially the same as Comparative Example 2, except that:

[0115] ② Prepare spraying materials: Use a spray granulation method to obtain short-cut silicon carbide fiber reinforced HfC ultra-high temperature ceramic powder, wherein the short-cut silicon carbide fiber has a length of 8 μm and a diameter of 1 μm, the mass ratio of the short-cut silicon carbide fiber to the HfC ceramic powder is 1:4, and the median particle size (D50) of the powder is 25 μm.

[0116] In step ③, the same process parameters are used, except that after the plasma beam is stabilized, the powder feeder containing the HfC ultra-high temperature ceramic powder reinforced with short-cut silicon carbide fibers in step ② is turned on to prepare a 350 μm thick short-cut silicon carbide fiber reinforced HfC coating.

[0117] The bonding strength, porosity and ablation resistance of the chopped silicon carbide fiber reinforced HfC coating prepared in this comparative example were tested using the same test method as in Example 1. The performance test results are shown in Table 1.

[0118] Comparative Example 5

[0119] Comparative Example 5 is substantially the same as Comparative Example 2, except that:

[0120] In step ①, select the size of 30mm (diameter) × 5mm (thickness) and the density of 2.52g / cm 3 The C / ZrC-SiC carbon fiber reinforced ceramic matrix composite material is used as the matrix, and other pretreatment methods remain unchanged to obtain the pretreated ceramic matrix composite material.

[0121] In step ②, a spray granulation method is used to obtain chopped carbon fiber reinforced hafnium boride (HfB2) ultra-high temperature ceramic powder, wherein the length of the chopped carbon fiber is 8 μm, the diameter is 1 μm, the mass ratio of the chopped carbon fiber to the HfB2 ultra-high temperature ceramic powder is 1:1, and the median particle size (D50) of the powder is 30 μm.

[0122] In step ③, the same process parameters are used, except that after the plasma beam is stabilized, the powder feeder containing the ultra-high temperature ceramic powder of hafnium boride (HfB2) reinforced with short-cut carbon fiber in step ② is turned on, and the deposition time is 4 minutes to prepare a short-cut carbon fiber reinforced HfB2 coating with a thickness of 370 μm.

[0123] The bonding strength, porosity and ablation resistance of the chopped silicon carbide fiber reinforced HfB2 coating prepared in this comparative example were tested using the same test method as in Example 1. The performance test results are shown in Table 1.

[0124] Comparative Example 6

[0125] ① Pretreated ceramic matrix composite material: the size is 30mm (diameter) × 5mm (thickness), and the density is 1.88g / cm 3 A carbon fiber reinforced silicon carbide ceramic matrix composite material (C / SiC) was used as a matrix, and the surface of the matrix was polished with 400#, 800#, and 1000# sandpapers in sequence, then ultrasonically cleaned in acetone for 10 minutes, and finally dried in an oven at 120°C to obtain a pretreated ceramic matrix composite material.

[0126] ②Prepare spraying materials: Use a spray granulation method to obtain short carbon fiber reinforced hafnium carbide (HfC) ultra-high temperature ceramic powder, the short carbon fiber length is 5μm, the diameter is 0.8μm, the mass ratio of short carbon fiber to HfC ultra-high temperature ceramic powder is 1:3, and the median particle size (D50) of the powder is 20μm. Use a spray granulation method to obtain short silicon carbide fiber reinforced HfC ultra-high temperature ceramic powder, wherein the short silicon carbide fiber length is 8μm, the diameter is 1μm, the mass ratio of short silicon carbide fiber to HfC ultra-high temperature ceramic powder is 1:4, and the median particle size (D50) of the powder is 25μm.

[0127] ③Preparation of bottom coating by low-pressure plasma spraying: The pretreated ceramic matrix composite substrate obtained in step ① is fixed on the rotating table of the vacuum chamber of the low-pressure plasma spraying equipment; before spraying, the vacuum chamber is evacuated to 5Pa, and then filled with argon gas to an absolute pressure of 8×10 2Pa. The surface of the ceramic matrix composite material substrate pretreated by plasma jet heating was heated to 800°C. Argon and helium were used as plasma gases (argon flow rate 30L / min, helium flow rate 20L / min), the spraying distance was 600mm, the rotating table speed was 10r / min, the arc voltage was 30V, the arc current was 1000A, and after the plasma beam was stable, the powder feeder containing the short-cut carbon fiber reinforced HfC ultra-high temperature ceramic powder in step ② was turned on, and the powder feeding rate was 12g / min, and a short-cut carbon fiber reinforced HfC ultra-high temperature ceramic bottom coating with a thickness of 200μm was prepared.

[0128] ④ Preparation of the surface coating by low-pressure plasma spraying: keeping the absolute pressure in the vacuum chamber unchanged, the surface coating was prepared with the same plasma gas ratio, spraying distance and turntable speed as in step ③, arc voltage of 30V, arc current of 1100A, and after the plasma beam was stable, the powder feeder containing the chopped silicon carbide fiber reinforced HfC ultra-high temperature ceramic powder in step ③ was turned on at a powder feeding rate of 15g / min. On the basis of the chopped carbon fiber reinforced HfC ultra-high temperature ceramic base coating, a chopped silicon carbide fiber reinforced HfC ultra-high temperature ceramic surface coating with a thickness of 150μm was prepared, thereby obtaining an antioxidant ablation composite coating on the surface of the C / SiC ceramic-based composite material.

[0129] ⑤ Cooling and taking out: After the vacuum chamber is cooled to room temperature, the atmospheric pressure is restored and the C / SiC ceramic-based composite material with the anti-oxidation and ablation composite coating is taken out.

[0130] The bonding strength, porosity and anti-ablation performance of the anti-oxidation ablation composite coating prepared in this comparative example were tested using the same testing method as in Example 1. The performance test results are shown in Table 1.

[0131] Comparative Example 7

[0132] ① Pretreated ceramic matrix composite material: the size is 30mm (diameter) × 5mm (thickness), and the density is 1.88g / cm 3 A carbon fiber reinforced silicon carbide ceramic matrix composite material (C / SiC) was used as a matrix, and the surface of the matrix was polished with 400#, 800#, and 1000# sandpapers in sequence, then ultrasonically cleaned in acetone for 10 minutes, and finally dried in an oven at 120°C to obtain a pretreated ceramic matrix composite material.

[0133] ②Prepare the spraying material: Use the CVD method to prepare a PyC layer shell with a thickness of 300nm on the surface of the carbon fiber to obtain a PyC layer shell coated carbon fiber; then use a mechanical cutting device to cut the PyC layer shell coated carbon fiber to obtain a PyC layer shell coated short carbon fiber with a length of 5μm and a diameter of 0.8μm. The spray granulation method is used to obtain the PyC layer shell coated short carbon fiber reinforced hafnium carbide (HfC) ultra-high temperature ceramic powder, wherein the mass ratio of the PyC layer shell coated short carbon fiber to the HfC ultra-high temperature ceramic powder is 1:3, and the median particle size (D50) of the powder is 20μm. The spray granulation method is used to obtain the HfC ultra-high temperature ceramic powder reinforced with short-cut silicon carbide fibers, wherein the short-cut silicon carbide fibers are 8μm in length and 1μm in diameter, and the mass ratio of the short-cut silicon carbide fibers to the HfC ultra-high temperature ceramic powder is 1:4, and the median particle size (D50) of the powder is 25μm.

[0134] ③Preparation of bottom coating by low-pressure plasma spraying: The pretreated ceramic matrix composite substrate obtained in step ① is fixed on the rotating table of the vacuum chamber of the low-pressure plasma spraying equipment; before spraying, the vacuum chamber is evacuated to 5Pa, and then filled with argon gas to an absolute pressure of 8×10 2 Pa. The surface of the ceramic matrix composite material substrate pretreated by plasma jet heating was heated to 800°C. Argon and helium were used as plasma gases (argon flow rate 30L / min, helium flow rate 20L / min), the spraying distance was 600mm, the rotating table speed was 10r / min, the arc voltage was 30V, the arc current was 1000A, and after the plasma beam was stable, the powder feeder containing the PyC layer shell coated short carbon fiber reinforced HfC ultra-high temperature ceramic powder obtained in step ② was turned on, and the powder feeding rate was 12g / min, and a PyC layer shell coated short carbon fiber reinforced HfC ultra-high temperature ceramic bottom coating with a thickness of 200μm was prepared.

[0135] ④ Preparation of the surface coating by low-pressure plasma spraying: keeping the absolute pressure in the vacuum chamber unchanged, the surface coating was prepared with the same plasma gas ratio, spraying distance and turntable speed as in step ③, arc voltage of 30V, arc current of 1100A, and after the plasma beam was stable, the powder feeder containing the chopped silicon carbide fiber reinforced HfC ultra-high temperature ceramic powder in step ③ was turned on at a powder feeding rate of 15g / min. On the basis of the PyC layer shell-coated chopped carbon fiber reinforced HfC ultra-high temperature ceramic bottom coating, a 150μm thick chopped silicon carbide fiber reinforced HfC ultra-high temperature ceramic surface coating was prepared, thereby obtaining an antioxidant ablation composite coating on the surface of the C / SiC ceramic-based composite material.

[0136] ⑤ Cooling and taking out: After the vacuum chamber is cooled to room temperature, the atmospheric pressure is restored and the C / SiC ceramic-based composite material with the anti-oxidation and ablation composite coating is taken out.

[0137] The bonding strength, porosity and anti-ablation performance of the anti-oxidation ablation composite coating prepared in this comparative example were tested using the same testing method as in Example 1. The performance test results are shown in Table 1.

[0138] Comparative Example 8

[0139] ① Pretreated ceramic matrix composite material: the size is 30mm (diameter) × 5mm (thickness), and the density is 1.88g / cm 3 A carbon fiber reinforced silicon carbide ceramic matrix composite material (C / SiC) was used as a matrix, and the surface of the matrix was polished with 400#, 800#, and 1000# sandpapers in sequence, then ultrasonically cleaned in acetone for 10 minutes, and finally dried in an oven at 120°C to obtain a pretreated ceramic matrix composite material.

[0140] ②Prepare spraying materials: Use a spray granulation method to obtain short carbon fiber reinforced hafnium carbide (HfC) ultra-high temperature ceramic powder, the short carbon fiber length is 5μm, the diameter is 0.8μm, wherein the mass ratio of short carbon fiber to HfC ultra-high temperature ceramic powder is 1:3, and the median particle size (D50) of the powder is 20μm. Use the CVD method to prepare a SiC layer shell with a thickness of 300nm on the surface of the silicon carbide fiber to obtain SiC layer shell coated silicon carbide fiber; then use a mechanical cutting device to cut the SiC layer shell coated silicon carbide fiber to obtain a SiC layer shell coated short chopped silicon carbide fiber with a length of 8μm and a diameter of 1μm. Use a spray granulation method to obtain SiC layer shell coated short chopped silicon carbide fiber reinforced HfC ultra-high temperature ceramic powder, wherein the mass ratio of SiC layer shell coated short chopped silicon carbide fiber to HfC ultra-high temperature ceramic powder is 1:4, and the median particle size (D50) of the powder is 25μm.

[0141] ③Preparation of bottom coating by low-pressure plasma spraying: The pretreated ceramic matrix composite substrate obtained in step ① is fixed on the rotating table of the vacuum chamber of the low-pressure plasma spraying equipment; before spraying, the vacuum chamber is evacuated to 5Pa, and then filled with argon gas to an absolute pressure of 8×10 2 Pa. The surface of the ceramic matrix composite material substrate pretreated by plasma jet heating was heated to 800°C. Argon and helium were used as plasma gases (argon flow rate 30L / min, helium flow rate 20L / min), the spraying distance was 600mm, the rotating table speed was 10r / min, the arc voltage was 30V, the arc current was 1000A, and after the plasma beam was stabilized, the powder feeder containing the chopped carbon fiber reinforced HfC ultra-high temperature ceramic powder in step ② was turned on, and the powder feeding rate was 12g / min, and a chopped carbon fiber reinforced HfC ultra-high temperature ceramic bottom coating with a thickness of 200μm was prepared.

[0142] ④ Preparation of the surface coating by low-pressure plasma spraying: keeping the absolute pressure in the vacuum chamber unchanged, the surface coating was prepared with the same plasma gas ratio, spraying distance and turntable speed as in step ③, arc voltage of 30V, arc current of 1100A, and after the plasma beam was stable, the powder feeder containing the SiC layer shell coated short-cut silicon carbide fiber reinforced HfC ultra-high temperature ceramic powder obtained in step ③ was turned on, and the powder feeding rate was 15g / min. On the basis of the short-cut carbon fiber reinforced HfC ultra-high temperature ceramic bottom coating, a SiC layer shell coated short-cut silicon carbide fiber reinforced HfC ultra-high temperature ceramic surface coating with a thickness of 150μm was prepared, thereby obtaining an antioxidant ablation composite coating on the surface of the C / SiC ceramic-based composite material.

[0143] ⑤ Cooling and taking out: After the vacuum chamber is cooled to room temperature, the atmospheric pressure is restored and the C / SiC ceramic-based composite material with the anti-oxidation and ablation composite coating is taken out.

[0144] The bonding strength, porosity and anti-ablation performance of the anti-oxidation ablation composite coating prepared in this comparative example were tested using the same testing method as in Example 1. The performance test results are shown in Table 1.

[0145] Comparative Example 9

[0146] Comparative Example 9 is substantially the same as Example 7, except that:

[0147] ② Prepare the spraying material: Use the CVD method to prepare a PyC shell with a thickness of 300 nm on the surface of the carbon fiber to obtain PyC shell-coated carbon fiber, and prepare a SiC shell with a thickness of 300 nm on the surface of the silicon carbide fiber to obtain SiC shell-coated silicon carbide fiber; then use mechanical cutting equipment to cut the PyC shell-coated carbon fiber and the SiC shell-coated silicon carbide fiber to obtain PyC shell-coated chopped carbon fiber with a length of 5 μm and a diameter of 0.8 μm, and obtain SiC shell-coated chopped silicon carbide fiber with a length of 8 μm and a diameter of 1 μm. A spray granulation method is used to compound PyC layer shell coated chopped carbon fibers, hafnium carbide (HfC) ultra-high temperature ceramic powder and yttrium aluminum garnet powder to obtain PyC layer shell coated chopped carbon fibers reinforced with hafnium carbide (HfC) ultra-high temperature ceramic powder, wherein the mass ratio of the PyC layer shell coated chopped carbon fibers to the HfC ultra-high temperature ceramic powder is 1:3, the volume fraction of yttrium aluminum garnet powder in the PyC layer shell coated chopped carbon fibers reinforced with hafnium carbide (HfC) ultra-high temperature ceramic powder is 27%, and the median particle size (D50) of the powder is 10 μm. A spray granulation method is used to composite SiC layer shell coated chopped silicon carbide fibers, hafnium carbide (HfC) ultra-high temperature ceramic powder and yttrium aluminum garnet powder to obtain SiC layer shell coated chopped silicon carbide fiber reinforced HfC ultra-high temperature ceramic powder, wherein the mass ratio of SiC layer shell coated chopped silicon carbide fibers to HfC ultra-high temperature ceramic powder is 1:4, the volume fraction of yttrium aluminum garnet powder in the SiC layer shell coated chopped silicon carbide fiber reinforced HfC ultra-high temperature ceramic powder is 18%, and the median particle size (D50) of the powder is 13μm.

[0148] The bonding strength, porosity and anti-ablation performance of the anti-oxidation ablation composite coating prepared in this comparative example were tested using the same testing method as in Example 1. The performance test results are shown in Table 1.

[0149]

[0150]

[0151]

[0152] It can be seen from the data in Table 1 that the high bonding strength anti-oxidation ablation composite coating designed and prepared by the present invention has excellent bonding strength and high temperature oxidation ablation resistance. The bonding strength of the layer shell coated short carbon fiber reinforced HfC / layer shell coated short silicon carbide fiber reinforced HfC composite coating prepared by the present invention is not less than 58MPa, the porosity is less than 10%, and the oxyacetylene ablation rate at 2000℃ is less than 1×10 -3mm / s. In Example 2, compared with Example 1, by increasing the current and voltage during spraying, that is, increasing the power of the plasma beam, the sprayed powder has a better melting effect in the beam, spreads more fully on the substrate, has a lower coating porosity, a higher coating bonding strength, and better anti-ablation performance. In Example 3, compared with Example 1, by extending the spraying time, the thickness of the composite coating is improved, and the bonding strength and anti-ablation performance of the composite coating are not affected. In Example 4, compared with Example 1, the bottom layer is a PyC layer shell coated with chopped fiber reinforced ZrB2, and the surface layer is a SiC layer shell coated with chopped silicon carbide fiber reinforced ZrC coating, and other spraying parameters remain unchanged. Since the melting point of ZrB2 is lower than that of HfC, the powder is easier to melt in the beam, so the prepared coating has a lower porosity. Although the ablation resistance of ZrC is inferior to that of HfC, the presence of SiC shell coated short-cut silicon carbide fibers improves the oxidation resistance of ZrC. The ablation rate of the ZrC coating reinforced by the surface SiC shell coated short-cut silicon carbide fibers is still less than 1×10 - 3 mm / s. In Example 5, a relatively high-density carbon fiber reinforced ultra-high temperature ceramic-based composite material is used as the matrix, the bottom layer is a PyC layer shell-coated short carbon fiber reinforced TaN material, and the surface layer is a SiC layer shell-coated short silicon carbide fiber reinforced HfB2. The performance results show that the composite coating proposed by the present invention and its preparation method are also applicable to boride and nitride ultra-high temperature ceramic materials. In Example 6, compared with Example 1, the bottom layer is a BN layer shell-coated short carbon fiber reinforced HfC, and the surface layer is a SiC layer shell-coated short silicon carbide fiber reinforced HfC. The bonding strength of the composite coating is still not less than 60MPa, the porosity is still less than 10%, and the oxyacetylene ablation rate at 2000°C is still less than 1×10 -3 mm / s; In Example 7, a suitable amount of yttrium aluminum garnet powder is added to the base layer and the surface layer coating, which can further improve the bonding strength and anti-oxidation and ablation performance of the composite coating and reduce the porosity compared with Example 1.

[0153] Corresponding to the embodiment, in Comparative Example 1, a chopped carbon fiber reinforced HfC / chopped silicon carbide fiber reinforced HfC composite coating with the same thickness as in Example 1 was prepared by atmospheric plasma spraying. Due to the limitation of the atmospheric plasma spraying process itself, the beam has poor heating ability for the powder and poor powder spreading ability, resulting in a relatively large porosity of the prepared composite coating, and relatively poor coating bonding strength and ablation resistance. In Comparative Example 2, a pure HfC coating was prepared by low-pressure plasma spraying technology using HfC spraying powder without chopped fiber reinforcement. After the coating was free of chopped fibers, the bonding strength and ablation resistance of the coating were reduced. In Comparative Example 3, a chopped carbon fiber reinforced HfC powder without shell coating was used to prepare a chopped carbon fiber reinforced HfC single-layer coating by low-pressure plasma spraying technology. Compared with Comparative Example 2, the bonding strength between the coating and the substrate was improved, but the ablation resistance was still relatively poor. In Comparative Example 4, short-cut silicon carbide fiber reinforced HfC powder without shell coating was used to prepare short-cut silicon carbide fiber reinforced HfC single-layer coating by low-pressure plasma spraying technology. The coating has good anti-ablation performance, but low bonding strength. In Comparative Example 5, short-cut carbon fiber reinforced HfB2 powder was used to prepare a single-layer coating. Compared with Comparative Example 2, the bonding strength between the coating and the substrate was improved, and the anti-ablation performance was poor. This shows that the single-layer coating can only optimize one of the bonding strength or anti-oxidation ablation performance of ultra-high temperature ceramic materials, and the comprehensive improvement effect is significantly lower than that of the composite coating. In Comparative Examples 6 to 8, although a low-pressure plasma spraying process was used, the composite coatings were respectively composed of chopped carbon fiber reinforced HfC / chopped silicon carbide fiber reinforced HfC, PyC layer shell coated chopped carbon fiber reinforced HfC / chopped silicon carbide fiber reinforced HfC, and chopped carbon fiber reinforced HfC / SiC layer shell coated chopped silicon carbide fiber reinforced HfC. Such coating compositions result in lower bonding strength and / or antioxidant and ablation resistance of the composite coatings. In Comparative Example 9, an excessive amount of small-particle yttrium aluminum garnet powder was added to the base and surface coatings. Compared with Example 7, although the overall porosity of the composite coating was reduced, the bonding strength and antioxidant and ablation resistance of the coating were reduced, and the overall performance of the composite coating was reduced.

[0154] By comparing the data of the embodiments and the comparative examples, it can be clearly seen that the composite coating of ultra-high temperature ceramic bottom layer reinforced by chopped carbon fiber coated with a shell / ultra-high temperature ceramic surface layer reinforced by chopped silicon carbide fiber coated with a shell prepared by the present invention is significantly superior to traditional coatings in terms of bonding strength, porosity and ablation resistance. This composite coating not only improves the bonding strength with the ceramic-based composite material, but also improves the high-temperature oxidation and ablation resistance of the ceramic-based composite material.

[0155] Parts of the present invention that are not described in detail are well known to those skilled in the art.

[0156] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A high bonding strength, anti-oxidation and ablation composite coating for ceramic matrix composite materials, characterized by: The high bonding strength anti-oxidation and ablation composite coating comprises, from the ceramic-based composite material outward, a layer shell-coated short carbon fiber reinforced ultra-high temperature ceramic bottom layer coating and a layer shell-coated short silicon carbide fiber reinforced ultra-high temperature ceramic surface layer coating.

2. The high bonding strength anti-oxidation ablation composite coating according to claim 1, characterized in that: The shell material in the shell-coated chopped carbon fibers and / or the shell-coated chopped silicon carbide fibers is one or more of pyrolytic carbon, silicon carbide and boron nitride; The preparation of the shell-coated chopped carbon fiber is as follows: a shell with a thickness of 100 to 500 nm is deposited on the surface of the carbon fiber by chemical vapor deposition to obtain the shell-coated carbon fiber, and then the shell-coated carbon fiber is cut to obtain the shell-coated carbon fiber; The preparation of the layer shell coated short-cut silicon carbide fiber is as follows: a layer shell with a thickness of 100 to 500 nm is deposited on the surface of the silicon carbide fiber by chemical vapor deposition to obtain the layer shell coated silicon carbide fiber, and then the layer shell coated silicon carbide fiber is cut to obtain; Preferably, the length of the layer shell coated chopped carbon fiber and / or the layer shell coated chopped silicon carbide fiber is 1 μm to 10 μm, and the diameter is 0.2 μm to 2 μm.

3. The high bonding strength anti-oxidation ablation composite coating according to claim 1, characterized in that: The ultra-high temperature ceramic in the ultra-high temperature ceramic bottom coating and / or the ultra-high temperature ceramic surface coating is one or more of carbides, borides and nitrides with high melting points; Preferably, the carbide is one or more of silicon carbide, zirconium carbide, hafnium carbide, tantalum carbide, titanium carbide and niobium carbide, the boride is one or more of zirconium boride, hafnium boride, tantalum boride, titanium boride and niobium boride, and the nitride is one or more of zirconium nitride, hafnium nitride, tantalum nitride, titanium nitride and niobium nitride.

4. The high bonding strength anti-oxidation ablation composite coating according to claim 1, characterized in that: The shell-coated short carbon fiber reinforced ultra-high temperature ceramic bottom layer coating and the shell-coated short silicon carbide fiber reinforced ultra-high temperature ceramic surface layer coating are respectively formed on the surface of the ceramic-based composite material by low-pressure plasma spraying using shell-coated short carbon fiber reinforced ultra-high temperature ceramic powder and shell-coated short silicon carbide fiber reinforced ultra-high temperature ceramic powder as spraying materials; The layer shell coated short carbon fiber reinforced ultra-high temperature ceramic powder is compounded by layer shell coated short carbon fiber and ultra-high temperature ceramic powder through spray granulation method; The layer shell coated short-cut silicon carbide fiber reinforced ultra-high temperature ceramic powder is compounded by layer shell coated short-cut silicon carbide fiber and ultra-high temperature ceramic powder through spray granulation method; Preferably, the median particle size D50 of the ultra-high temperature ceramic powder reinforced by chopped carbon fibers coated with the shell and / or the ultra-high temperature ceramic powder reinforced by chopped silicon carbide fibers coated with the shell is 5 to 50 μm.

5. The high bonding strength anti-oxidation ablation composite coating according to claim 1, characterized in that: In the layer shell coated short carbon fiber reinforced ultra-high temperature ceramic bottom coating, the mass ratio of the layer shell coated short carbon fiber to the ultra-high temperature ceramic is (0.2-9):1; In the layer shell coated short-cut silicon carbide fiber reinforced ultra-high temperature ceramic surface coating, the mass ratio of the layer shell coated short-cut silicon carbide fiber to the ultra-high temperature ceramic is (0.2-9):1; The thickness of the layer shell coated with the ultra-high temperature ceramic bottom layer coating reinforced by chopped carbon fiber and / or the layer shell coated with the ultra-high temperature ceramic top layer coating reinforced by chopped silicon carbide fiber is 50-500 μm.

6. The method for preparing a high bonding strength anti-oxidation and ablation composite coating for ceramic matrix composite materials according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: (1) grinding, cleaning and drying the ceramic-based composite material to obtain a pretreated ceramic-based composite material; (2) A shell-coated short carbon fiber reinforced ultra-high temperature ceramic base coating and a shell-coated short silicon carbide fiber reinforced ultra-high temperature ceramic surface coating are sequentially prepared on the surface of the pretreated ceramic-based composite material by a low-pressure plasma spraying method, thereby obtaining the high bonding strength and anti-oxidation and ablation composite coating on the surface of the ceramic-based composite material.

7. The preparation method according to claim 6, characterized in that: The density of the ceramic matrix composite material is 1.8 to 5.0 g / cm 3 ; The grinding is performed using sandpaper; The cleaning is ultrasonic cleaning in acetone and / or ethanol for 10 to 15 minutes; and / or The drying temperature is 100-150°C.

8. The preparation method according to claim 6, characterized in that: During the low-pressure plasma spraying process, the surface temperature of the pretreated ceramic-based composite material is 600-1000° C. by plasma jet heating; During the low-pressure plasma spraying process, the absolute pressure in the spraying chamber is 1×10 2 ~2×10 3 Pa; In the process of preparing the layer shell coated short carbon fiber reinforced ultra-high temperature ceramic bottom layer coating and / or the layer shell coated short silicon carbide fiber reinforced ultra-high temperature ceramic surface layer coating, argon and helium are used as plasma gases, the argon flow rate is 20-50L / min, the helium flow rate is 10-40L / min, the spraying distance is 400-1000mm, the rotation speed of the turntable is 0-20r / min, the arc voltage of the low-pressure plasma spraying equipment is 20-40V, the arc current is 800-1600A, and the powder feeding rate of the layer shell coated short carbon fiber reinforced ultra-high temperature ceramic powder and / or the layer shell coated short silicon carbide fiber reinforced ultra-high temperature ceramic powder is 10-20g / min.

9. A high bonding strength, anti-oxidation and ablation composite coating for ceramic matrix composite materials prepared by the preparation method according to any one of claims 6 to 8.

10. The high bonding strength anti-oxidation and ablation composite coating for ceramic matrix composite materials according to claim 9, characterized in that: The bonding strength of the high bonding strength anti-oxidation and ablation composite coating is not less than 50MPa; The porosity of the high bonding strength anti-oxidation and ablation composite coating is less than 10%; The linear ablation rate of the high bonding strength anti-oxidation ablation composite coating in an oxyacetylene ablation test at a coating surface temperature of 2000°C is less than 1×10 -3 mm / s.

Citation Information

Patent Citations

  • Coating inorganic fiber toughened MAX phase ceramic composite material, preparation method and uses thereof

    CN103910532A

  • Boron nitride / silicon carbide composite coating layer and preparation method thereof

    CN106431448A

  • Ablation-resistant fiber toughened Si-B-C-N-Zr ceramic matrix composite as well as preparation method and application thereof

    CN107827461A

  • High-temperature vacuum heat-insulation composite material having ceramic fiber shell

    CN108516858A

  • Fiber reinforced carbon-silicon carbide ceramic matrix composite material and preparation method thereof

    CN109293383A

Cited By

  • Ferromanganese erosion resistant refractory material and preparation method thereof

    CN120423863A

  • 3D printing rubber thermal insulation material and preparation method thereof

    CN121136455A

  • Ultrahigh-temperature-resistant and wear-resistant ceramic-based composite material and preparation method thereof

    CN121673073A

  • An ultra-high-temperature-resistant wear-resistant ceramic matrix composite material and a preparation method thereof