Method for stabilizing alkali metal oxysalt nanocluster by using confinement effect of molecular sieve as well as product and application thereof

By modifying the acid-base environment of alkali metal oxoate precursor and SiO2, combined with ionic liquid template agent and evaporation crystallization technology, the alkali metal oxoate dispersion under high load on the SiO2 carrier is successfully achieved, improving the performance of the catalyst and stability solve the problems of poor dispersion and insufficient stability of the catalyst in the prior art.

CN119018909AInactive Publication Date: 2024-11-26ZHEJIANG UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411514736.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-29
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art is difficult to realize high load and high dispersion alkali metal oxoate catalysts on SiO2 support, resulting in poor catalytic performance and poor stability. In traditional synthesis methods, alkali metal oxoate is prone to agglomeration and sintering, making it difficult to maintain. Dispersed state.

Method used

By modifying the acid-base environment of the alkali metal oxoate precursor and the amorphous SiO2 precursor of molecular sieve, the amount and order of acid-base addition are controlled, and the stable interaction between alkali metal oxoate and SiO2 is achieved. The ionic liquid template agent is used. 蒸发结晶条件下合成氧酸盐@ZSM-22分子筛原粉,并在高温下焙烧得到高浓度分散的催化剂。

Benefits of technology

The high dispersion of alkali metal oxidate under high load was achieved, which improved the product yield and stability of the catalyst. The catalyst showed a 54.5% vinyl chloride yield and 50 hours in the vinyl chloride preparation reaction of chloromethane oxidation coupling. The above stability solves the problems of expensive raw materials and high pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018909A_ABST
    Figure CN119018909A_ABST
Patent Text Reader

Abstract

The invention discloses a method for stabilizing an alkali metal oxysalt nanocluster by using a molecular sieve confinement effect as well as a product and application thereof. According to the present invention, the means of acid treatment and alkali treatment are innovatively introduced under the in-situ condition, the stable confinement of the alkali metal oxysalt is achieved by using the skeleton of the ZSM-22 pure silicon molecular sieve, and the oxysalt is obtained after the high temperature roasting and is dispersed in the SiO2 carrier; the catalyst can still keep highly uniform dispersion of oxysalt nanoclusters under the condition that the oxysalt feeding amount reaches up to 25%, the average size of a single nanocluster is only about 1.7 nm, and the catalyst shows high yield and high stability in a catalytic reaction for preparing vinyl chloride through oxidative coupling of chloromethane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of molecular sieve confinement, and relates to a method for stabilizing alkali metal oxoate nanoclusters by utilizing the confinement effect of molecular sieves, and its products and applications. Specifically, it relates to a synthesis method for stably dispersing high-concentration alkali metal oxoate in a molecular sieve, and a catalyst in which the alkali metal oxoate is highly dispersed in a SiO2 carrier obtained by high-temperature calcination, and the application of such catalyst in the reaction of methyl chloride oxidation to prepare vinyl chloride. Background Art

[0002] Vinyl chloride (C2H3Cl) is the basic monomer of polyvinyl chloride, the world's third largest plastic. At present, the production process of vinyl chloride mainly uses C2 hydrocarbons derived from coal or petroleum as raw materials, and there are still problems such as expensive raw materials, high energy consumption, and high pollution. The development of a new vinyl chloride production process using low-cost renewable C1 platform molecules as raw materials is of great significance for the production process of vinyl chloride. In previous studies, we reported a new route for preparing vinyl chloride (MCTV) by highly selective methyl chloride coupling (Chinese patent CN 118084610 A). The catalyst used is a surface-supported alkali metal oxoate prepared by coprecipitation. The strong interaction of the carrier containing zirconium, aluminum and other elements with the alkali metal oxoate is used to anchor and disperse these active centers. High-concentration and highly dispersed clusters are the key to improving catalytic performance. However, there are the following problems in this work: the metal precursors required for the synthesis of carriers such as zirconium silicate, aluminum silicate, and zirconium cerate are relatively expensive, and the activity of the metal in the carrier also affects the active center.

[0003] As an inert carrier, SiO2 is widely available, low-cost, has no redox ability and the ability to adsorb and activate oxygen, and does not affect the performance of the active center. It performs well in many aspects such as molding and processing. People have been exploring this material. However, in the past, people found in the research process that it was very difficult to obtain high-loaded and highly dispersed oxoacid salts on SiO2 carriers. The reason is that the inherent properties of SiO2 make it impossible for it to form a strong interaction with oxoacid salts. SiO2 doped with alkali metal oxoacid salts is synthesized using traditional synthesis methods. During the calcination process, the oxoacid salts are very easy to agglomerate and sinter. As shown by the above work data of this team, the catalytic performance of alkali metal oxoacid salts loaded on SiO2 carriers is significantly worse than that on carriers containing zirconium, aluminum and other metals such as zirconium silicate and aluminum silicate, and serious agglomeration occurs at 35% oxoacid salt loading, resulting in poor catalytic stability.

[0004] It is a common work to use the in-situ confinement of the pores of pure silicon molecular sieves to achieve high dispersion of nanoclusters, which is mainly reflected in the confinement of some metal or metal oxide clusters. The reason why this method can achieve dispersion is that, first, the ligand stabilization strategy is used to enable the metal or metal oxide clusters to form a good coordination effect with the molecular sieve precursor, thereby achieving high dispersion, and second, the calcination temperature is low (generally at 550 ℃-600 ℃, which can maintain the molecular sieve structure), so as not to cause the metal or metal oxide to sinter. However, this strategy is also limited to a low loading of about 5% to ensure the dispersion effect. When the concentration is increased to more than 20%, large-scale agglomeration will also occur due to the high surface energy of the metal clusters. That is, to obtain metal or metal oxide nanoclusters with high dispersion at high loading in molecular sieves is itself a considerable challenge, and the work of confining alkali metal oxoacids in molecular sieves is rarely studied but is crucial.

[0005] The research team of the present invention has found through in-depth analysis of the acid-base properties of alkali metal oxo salts that alkali metal oxo salts are stable in alkaline environments, and will become corresponding acids in acidic environments, and then become metal oxides with poor catalytic performance after roasting. However, the oxo salt precursor solution in the molecular sieve precursor is easy to form block precipitation and then separate from the molecular sieve carrier later. Only when it exists in the form of acid can it be stably cross-linked with the amorphous SiO2 precursor of the molecular sieve and dispersed.

[0006] Based on the above background, the present invention innovatively proposes a technical means to adjust the acid-base environment of the alkali metal oxoate precursor and the amorphous SiO2 precursor of the molecular sieve, that is, to control the amount and order of addition of acid and alkali to regulate the interaction between the alkali metal oxoate precursor and the molecular sieve precursor, so as to achieve a highly dispersed state of oxoate clusters under high loading, and at the same time, this technical means does not affect the skeleton formation of the molecular sieve. It is worth noting that under the same conditions, the samples obtained by the conventional impregnation method show obvious sodium tungstate agglomeration phenomenon. The in-situ obtained sample is calcined at high temperature to finally obtain a catalyst in which the oxoate active sites are highly dispersed on the SiO2 carrier - alkali metal oxoate @Z-SiO2. This catalyst helps to greatly improve the product yield and stability of the catalyst with SiO2 as the carrier in the MCTV reaction, and also helps to solve the problems of expensive raw materials and high pollution of catalyst synthesis in this field. Summary of the invention

[0007] The purpose of the present invention is to address the deficiencies in the prior art and provide a method for stabilizing alkali metal oxoate nanoclusters by utilizing the confinement effect of molecular sieves, as well as its products and applications. The method utilizes the interaction between an alkali metal oxoate precursor and a molecular sieve amorphous SiO2 precursor during the acid-base modulation process, and prepares an oxoate@ZSM-22 molecular sieve raw powder of stable confined high-concentration alkali metal oxoate nanoclusters by evaporation and crystallization. The oxoate@ZSM-22 molecular sieve raw powder is then calcined at high temperature to obtain a catalyst for the catalytic reaction of preparing vinyl chloride by oxidative coupling of methyl chloride.

[0008] In the first aspect, the present invention provides a method for synthesizing a molecular sieve of stable confined alkali metal oxoate nanoclusters, namely, an alkali metal oxoate@ZSM-22 molecular sieve raw powder, which uses an ionic liquid as a template, first adds an inorganic acid and an alkali metal oxoate precursor to a silicon source, then adds an inorganic base and a template, and synthesizes the alkali metal oxoate@ZSM-22 molecular sieve raw powder under the condition of evaporation-assisted crystallization; the specific preparation steps are as follows: Step S1, stirring the inorganic acid and the silicon source at room temperature for 5-12 hours, then adding the alkali metal oxoate precursor, and ensuring that the pH value of the solution reaches 3-6, and then continuing to stir for a second time for 6-24 hours to obtain a mixed solution; Preferably, the inorganic acid source is selected from at least one of sulfuric acid, nitric acid, hydrochloric acid and phosphoric acid; Preferably, the silicon source is selected from at least one of tetraethyl orthosilicate and silica gel, more preferably tetraethyl orthosilicate; Preferably, the oxoacid salt precursor is selected from at least one of tungstate, metavanadate, molybdate, sulfate, phosphate and carbonate; Preferably, the alkali metal is selected from at least one of sodium and potassium; Preferably, the molar ratio of the effective component SiO2 in the silicon source to the solvent in the mixed solution is 1:20-50; wherein the solvent in the mixed solution is H2O; Preferably, the mass fraction of the alkali metal oxosalt precursor is 5 wt%-55 wt%.

[0009] Step S2, adding an inorganic base to the mixed solution of step S1 until the pH value reaches 8-12, stirring for 0.5-3 hours, then adding an ionic liquid as a template, and then stirring for a second time for 6-24 hours to form a gel system; Preferably, the ionic liquid is 1-butyl-3-methylimidazolium hydrobromide ([BMIm]Br); Preferably, the inorganic base source is at least one of sodium hydroxide and potassium hydroxide; Preferably, the molar ratio of the effective ingredient SiO2 in the silicon source, the template, and the solvent in the gel system is 1:0.2-0.4:30-60, wherein the solvent in the gel system is H2O.

[0010] Step S3, directly drying the gel system of step S2 to obtain a solid xerosol; Preferably, the drying temperature is 50-80° C. and the drying time is more than 6 hours.

[0011] Step S4, taking the solid dry sol and water and placing them on the upper and lower layers of the lining in the reaction kettle respectively, and performing high-temperature evaporation and crystallization; Preferably, the evaporation crystallization temperature is 160-180°C; the evaporation crystallization time is 48-100 hours; Step S5, drying the solid product obtained by cooling after the crystallization in step S4 to obtain the original powder of oxygen acid salt @ ZSM-22.

[0012] In a second aspect, the present invention provides a molecular sieve of stable confined alkali metal oxoate nanoclusters, which is prepared by the above synthesis method.

[0013] In a third aspect, the present invention provides a silicon-based composite material of confined alkali metal oxoate nanoclusters, which is obtained by high-temperature calcination of the above-mentioned molecular sieve (oxoate@ZSM-22 raw powder).

[0014] Preferably, the calcination temperature is 700-800° C., the calcination time is 1 hour, and the calcination atmosphere is air.

[0015] The silicon-based composite material of SiO2 (α-cristobalite) confined alkali metal oxoate nanoclusters prepared by the present invention has excellent thermal stability in an air atmosphere, can withstand a high temperature of 700-800° C., and will not be damaged or decomposed.

[0016] In a fourth aspect, the present invention provides the use of the above-mentioned SiO2 confined alkali metal oxoate nanoclusters as a catalyst in the oxidative coupling reaction of methyl chloride to produce vinyl chloride; Preferably, the chloromethane oxidative coupling catalytic reaction uses chloromethane and oxygen as raw materials and is carried out in a fixed bed reactor, and its products include vinyl chloride, C2 hydrocarbons, carbon oxides and C3 hydrocarbons; Preferably, the raw material gas further comprises an inert gas; the inert gas is more preferably any one or more of nitrogen, helium and argon; Preferably, the flow rate of the feed gas is 0-100 mL / min, but excluding 0, more preferably 20-80 mL / min, and most preferably 30-60 mL / min; Preferably, the molar ratio of methyl chloride to oxygen is (0.5-5):1, more preferably 0.5-1:1; Preferably, the reaction temperature is 600-900°C, preferably 675-750°C, more preferably 700-725°C; Preferably, the reaction space velocity is 12000-48000 , more preferably 24000 -36000 .

[0017] Compared with the prior art, the beneficial effects of the present invention are at least: (1) The present invention provides a synthesis method for stably dispersing high-concentration alkali metal oxoate in a molecular sieve, and a catalyst in which a high concentration (up to 25 wt% or more) of alkali metal oxoate is dispersed in a SiO2 carrier by high-temperature calcination. A large number of alkali metal oxoate nanoclusters are evenly distributed on this type of catalyst. After particle size statistics, the average size is calculated to be about 1.7 nm. The dispersion effect is obvious because the oxoate particle size obtained by the impregnation method under the same conditions is irregularly aggregated (about 50 nm). The present invention is significantly different from the existing synthesis route of carrier-supported alkali metal oxoate catalysts and meets the concepts of high efficiency, stability, greenness and low cost.

[0018] (2) The present invention provides a high-yield and high-stability catalyst for the oxidative coupling of methyl chloride to vinyl chloride, alkali metal oxoate @ Z-SiO2, where Z represents a molecular sieve. Methyl chloride is used as a raw material and introduced into a fixed-bed catalytic reactor under aerobic conditions. At a certain temperature, the yield of vinyl chloride in the reaction product can reach 54.5%, the reaction stability is good, and the service life of the catalyst is greater than 50 hours, which are at least about 1.4 times and 10 times the best performance of SiO2-based carrier catalysts in the MCTV catalysis field. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 Figure (a) shows the XRD patterns of NaW@ZSM-22-n% catalysts with different sodium tungstate feed amounts.

[0020] Figure 1 Figure (b) shows the XRD patterns of NaW@Z-SiO2-n% catalysts with different sodium tungstate dosages after calcination.

[0021] Figure 1 Figure (c) shows the I calculated for each catalyst based on the two XRD characteristic peaks of sodium tungstate and α-cristobalite. 27.8° / I 22.2° .

[0022] Figure 2Figure (a) shows the W / Si ratio of NaW@Z-SiO2-25% and NaW / Z-SiO2-25%-imp catalysts measured by ICP-MS and XPS.

[0023] Figure 2 Figure (b) shows the W 4f XPS spectra of NaW@Z-SiO2-25% and NaW / Z-SiO2-25%-imp.

[0024] Figure 3 HRTEM image of NaW@Z-SiO2-25% catalyst.

[0025] Figure 4 Figure (a) in the middle is the HRTEM image of NaW / Z-SiO2-25%-imp.

[0026] Figure 4 Figure (b) is the Haadf image of NaW@Z-SiO2-25% catalyst.

[0027] Figure 4 Figure (c) in the middle is the EDS distribution diagram of the Na element in the c region of the NaW@Z-SiO2-25% catalyst.

[0028] Figure 4 Figure (d) is the EDS distribution diagram of Si element in the c region of NaW@Z-SiO2-25% catalyst.

[0029] Figure 4 Figure (e) is the EDS distribution of W element in region c of NaW@Z-SiO2-25% catalyst.

[0030] Figure 4 The middle (f) figure is the Haadf image of NaW / Z-SiO2-25%-imp.

[0031] Figure 4 Figure (g) in the middle is the EDS distribution diagram of Na element in the c region of NaW / Z-SiO2-25%-imp.

[0032] Figure 4 The middle figure (h) is the EDS distribution diagram of Si element in the c region of NaW / Z-SiO2-25%-imp.

[0033] Figure 4 Figure (i) in the middle is the EDS distribution diagram of W element in the c region of NaW / Z-SiO2-25%-imp.

[0034] Figure 5 Figure (a) shows the XRD patterns of NaVO3 as an alkali metal oxoate before and after in-situ calcination in ZSM-22 and the XRD pattern of the impregnated sample after calcination.

[0035] Figure 5 Figure (b) shows the XRD patterns of Na3PO4 as an alkali metal oxoate before and after in-situ calcination in ZSM-22 and the XRD pattern of the impregnated sample after calcination.

[0036] Figure 5 Figure (c) shows the XRD patterns of Na2SO4 as an alkali metal oxoate before and after in-situ calcination in ZSM-22 and the XRD pattern of the impregnated sample after calcination.

[0037] Figure 5 Figure (d) shows the XRD patterns of NaNbO3 as alkali metal oxoate before and after in-situ calcination in ZSM-22 and the XRD patterns of the impregnated sample after calcination.

[0038] Figure 5 Figure (e) shows the XRD patterns of Na2CO3 as alkali metal oxoacid in situ before and after calcination in ZSM-22 and the XRD patterns of the impregnated sample after calcination.

[0039] Figure 6 Figure (a) shows the XRD patterns of NaW@ZSM-22-25% and NaW@ZSM-22-25%-imp catalysts.

[0040] Figure 6 Figure (b) shows the XRD patterns of NaW@Z-SiO2-25% and NaW@Z-SiO2-25%-imp catalysts after calcination.

[0041] Figure 6 Figure (c) shows the I calculated for each catalyst based on the two XRD characteristic peaks of sodium tungstate and α-cristobalite. 27.8° / I 22.2° .

[0042] Figure 7 Figure (a) shows the XRD patterns of NaW@ZSM-22-25%, NaW@ZSM-22-25%-UH and NaW@ZSM-22-25%-NT catalysts.

[0043] Figure 7 Figure (b) shows the XRD patterns of NaW@Z-SiO2-25%, NaW@SiO2-25%-UH and NaW@SiO2-25%-NT catalysts after calcination.

[0044] Figure 7 Figure (c) shows the I calculated for each catalyst based on the two XRD characteristic peaks of sodium tungstate and α-cristobalite. 27.8° / I 22.2° .

[0045] Figure 8XRD patterns of three catalysts for adjusting acidity and base.

[0046] Fig. 9 Figure (a) shows the methyl chloride conversion rate of NaW@Z-SiO2-25% and NaW / Z-SiO2-25%-imp for the oxidative coupling of methyl chloride to prepare vinyl chloride.

[0047] Fig. 9 Figure (b) shows the vinyl chloride selectivity of NaW@Z-SiO2-25% and NaW / Z-SiO2-25%-imp for the oxidative coupling of methyl chloride to prepare vinyl chloride.

[0048] Fig. 9 Figure (c) shows the yield of vinyl chloride in the oxidative coupling reaction of methyl chloride to prepare vinyl chloride by NaW@Z-SiO2-25% and NaW / Z-SiO2-25%-imp.

[0049] Fig. 9 Figure (d) shows the catalytic stability test of NaW@Z-SiO2-25% and NaW / Z-SiO2-25%-imp for the oxidative coupling of methyl chloride to prepare vinyl chloride. DETAILED DESCRIPTION

[0050] As mentioned above, in view of the shortcomings of the prior art, the inventors of this case have proposed the technical solution of the present invention after long-term research and extensive practice, which is mainly based on at least: by adjusting the acid-base environment of the alkali metal oxoate precursor and the amorphous SiO2 precursor of the molecular sieve, that is, by controlling the amount and order of addition of acid and alkali to regulate the interaction between the alkali metal oxoate precursor and the molecular sieve precursor, the high dispersion state of the oxoate clusters under high loading is achieved, and the skeleton formation of the molecular sieve is not affected. That is, the present invention innovatively introduces acid treatment and alkali treatment under in-situ conditions, and uses the skeleton of pure silicon molecular sieve (such as ZSM-22) to achieve stable confinement of alkali metal oxoate, and the oxoate is dispersed in the SiO2 carrier after high-temperature calcination. This type of catalyst can still maintain a highly uniform dispersion of oxoate nanoclusters when the oxoate feed amount is as high as 25%, and the average size of a single nanocluster is only about 1.7 nm, and it shows high yield and high stability in the catalytic reaction of chloromethane oxidative coupling to prepare vinyl chloride.

[0051] SiO2 refers to α-cristobalite. Except for the silicon source and amorphous SiO2 specifically mentioned, all types of SiO2 mentioned in the present invention refer to quartz obtained by high-temperature calcination of molecular sieves, which will not be repeated here.

[0052] Therefore, the embodiment of the present invention provides a molecular sieve of stable confined high-concentration alkali metal oxoate nanoclusters, namely, alkali metal oxoate@ZSM-22 molecular sieve and a synthesis method thereof, wherein an ionic liquid is used as a template, an inorganic acid and an alkali metal oxoate precursor are first added to a silicon source, and then an inorganic base and a template are added, and an alkali metal oxoate@ZSM-22 molecular sieve raw powder is synthesized under the condition of evaporation-assisted crystallization, and the specific preparation steps are as follows: Step S1, stirring the inorganic acid and the silicon source at room temperature for 5-12 hours, then adding the alkali metal oxoate precursor, and ensuring that the pH value of the solution reaches 3-6, and then continuing to stir for a second time for 6-24 hours to obtain a mixed solution; In the embodiment, the secondary stirring time is preferably 10-15 hours; In the embodiment, the inorganic acid source is selected from at least one of sulfuric acid, nitric acid, hydrochloric acid, and phosphoric acid, more preferably sulfuric acid; In the embodiment, after adding the alkali metal oxo salt precursor, the solution preferably has a pH of 4-5; In the embodiment, the silicon source is selected from at least one of tetraethyl orthosilicate and silica gel, and more preferably tetraethyl orthosilicate; In the embodiment, the oxoacid salt precursor is selected from at least one of tungstate, metavanadate, molybdate, sulfate, phosphate and carbonate; In the embodiment, the alkali metal is selected from at least one of sodium and potassium; In the embodiment, the molar ratio of the effective component SiO2 in the silicon source to the solvent of the mixed solution is preferably 1:20-50; wherein the solvent of the mixed solution is H2O; In the embodiment, the mass fraction of the alkali metal oxo salt precursor is n%, wherein n = 100 × [ ], n = 5, 15, 25, 35, 45 and 55. That is, n% is preferably 5 wt%-55 wt%, more preferably 15 wt%-45 wt%, more preferably 25 wt%-35 wt%.

[0053] Step S2, adding an inorganic base to the mixed solution of step S1 until the pH value reaches 8-12, stirring for 0.5-3 hours, then adding an ionic liquid as a template, and then stirring for a second time for 6-24 hours to form a gel system; In the embodiment, the secondary stirring time is preferably 12-18 hours; In the embodiment, the template agent is preferably 1-butyl-3-methylimidazolium hydrobromide ([BMIm]Br); In an embodiment, the inorganic base source is selected from at least one of sodium hydroxide and potassium hydroxide; In the embodiment, the pH value of the solution after the addition of the inorganic base preferably reaches 10-12; In the embodiment, the molar ratio of the effective ingredient SiO2 in the silicon source, the template, and the solvent in the gel system is preferably 1:0.2-0.4:30-60, wherein the solvent in the gel system is H2O.

[0054] Step S3, directly drying the gel system of step S2 to obtain a solid xerosol; In the embodiment, the drying temperature is preferably 50-80°C; In the embodiment, the drying time is preferably 6 hours or longer, more preferably 12 hours or longer.

[0055] Step S4, taking the solid dry sol and water and placing them on the upper and lower layers of the lining in the reaction kettle respectively, and performing high-temperature evaporation and crystallization; In the embodiment, the evaporation crystallization temperature is preferably 160-180°C; In the embodiment, the evaporation crystallization time is preferably 48-100 hours, more preferably 48-60 hours; In the embodiment, the mass ratio of water to dry sol in the reaction kettle is 0.5-1:1.

[0056] Step S5, drying the solid product obtained by cooling after the crystallization in step S4 to obtain the original powder of oxoacid salt @ ZSM-22; In the embodiment, the drying temperature is preferably 50-100°C; In the embodiment, the drying time is preferably 6 hours or longer, more preferably 12 hours or longer.

[0057] The embodiment of the present invention also provides a silicon-based composite material of SiO2-confined alkali metal oxoate nanoclusters, which is obtained by high-temperature calcination of the above molecular sieve (oxoate@ZSM-22 raw powder). And the use of the above silicon-based composite material of SiO2-confined alkali metal oxoate nanoclusters as a catalyst in the reaction of chloromethane oxidative coupling to produce vinyl chloride.

[0058] In the embodiment, the calcination temperature is preferably 700-800° C., the calcination time is preferably 1 hour, and the calcination atmosphere is preferably air.

[0059] The SiO2 confined alkali metal oxoate nanocluster compound prepared by the present invention has excellent thermal stability in an air atmosphere, can withstand a high temperature of 700-800°C, and will not be damaged or decomposed.

[0060] The chloromethane oxidative coupling catalytic reaction uses chloromethane and oxygen as raw materials and is carried out in a fixed bed reactor, and its products include vinyl chloride, C2 hydrocarbons, carbon oxides and C3 hydrocarbons; In an embodiment, the raw material gas further comprises an inert gas; the inert gas is more preferably any one or more of nitrogen, helium, and argon; In an embodiment, the flow rate of the feed gas is preferably 0-100 mL / min, but excluding 0, more preferably 20-80 mL / min, and most preferably 30-60 mL / min; In an embodiment, the molar ratio of methyl chloride to oxygen is preferably (0.5-5):1, more preferably 0.5-1:1; In an embodiment, the reaction temperature is preferably 600-900°C, more preferably 675-750°C, and most preferably 700-725°C; In an embodiment, the space velocity of the reaction is preferably 12000-48000 , more preferably 24000 -36000 .

[0061] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0062] In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0063] Unless otherwise specified, all reagents used in the examples were analytically pure. The following methods are described as follows:

[0064] 1. In the following examples, the composition of the samples was measured using a Rigaku Ultima IV X-ray fluorescence spectrometer; scanning electron microscope (SEM) images and element energy distribution surface scanning analysis maps (EDS Mapping) were obtained on a Hitachi S-4800 microscope; the relative contents of W and Si in the bulk and surface of the samples were obtained on a PerkinElmer nexion 300x ICP-MS and a PHI1600 XPS, respectively; the UV-visible diffuse reflectance spectrum of the catalyst was measured on a Shimadzu UV-2700 spectrometer; and the Raman spectrum of the catalyst was measured on a Nicolet Nexus 470 FTIR.

[0065] 2. The catalytic test of chloromethane oxidative coupling to vinyl chloride was carried out on a fixed bed reactor with normal pressure, controllable temperature and continuous flow. The tail gas after the reaction was directly introduced into a gas chromatograph with dual detectors including a thermal conductivity detector (TCD) and a hydrogen flame ionization detector (FID) for analysis. The reaction tube was 300 mm long and 9 mm in inner diameter. The reaction was carried out under normal pressure. A small piece of quartz wool was placed in the middle of the reaction tube to support the catalyst powder. The reaction tube was placed vertically in a heating furnace. A thermocouple was installed in the tube to monitor the temperature of the reaction bed. During the test, a certain mass of catalyst was loaded in the reactor. CH3Cl, O2 and N2 were injected into the reactor in a certain proportion. After the reaction temperature reached a stable state for half an hour, the sample was injected and the product was detected online. The product was analyzed by online gas chromatography equipped with a flame ionization detector (FID) and a thermal conductivity detector (TCD). CH3Cl, CH4, C2H4, C2H2 and C2H3Cl were determined by FID, and CO and CO2 were determined by TCD.

[0066] Product detection and analysis methods: All carbon products in the oxidative coupling of methyl chloride to prepare vinyl chloride were detected using the standard curve method.

[0067] The CH3Cl conversion was calculated according to the following equation: in Indicates the inlet of the reaction system The amount of substance, Represents the outlet of the reaction system the amount of a substance; The C2H3Cl product selectivity was calculated according to the following equation: in Indicates the amount of substance of the C2H3Cl product; The C2H3Cl product yield was calculated according to the following equation: Embodiment 1: First, add 25.26 g of sulfuric acid aqueous solution (pH=1.0) and 7.4 g of tetraethyl orthosilicate (TEOS) into a beaker, stir at room temperature for 6 hours, then add 0.066 g of sodium tungstate dihydrate, at which time the pH value of the solution reaches 4-6, stir at room temperature for 24 hours to obtain a mixed solution. The molar ratio of the active ingredient SiO2 in tetraethyl orthosilicate to the solvent water in the mixed solution is 1:40.

[0068] Then, 1.70 g of sodium hydroxide aqueous solution (concentration of 12.5 mol / L) was added to the mixed solution, and the pH value of the solution reached 10-12. After stirring for 1 hour, 2.72 g of ionic liquid 1-butyl-3-methylimidazolium hydrobromide ([BMIm]Br) was added as an organic template and stirred for 24 hours to obtain a gel. The molar ratio of the active ingredient SiO2 in tetraethyl orthosilicate, 1-butyl-3-methylimidazolium hydrobromide, and the solvent water in the gel system was 1:0.3:60.

[0069] The obtained gel was dried at 80 °C for 4 hours, and then 1.0 g of the dry sol was taken in a 100 mL polytetrafluoroethylene reactor and crystallized at 170 °C for 48 hours. There is a concave polytetrafluoroethylene support in the hydrothermal reactor, and the gel (1.0 g) and water (1.0 g) are placed on the top and bottom respectively. After crystallization, the solid was collected and dried at 100 °C for 12 h to obtain the ZSM-22 molecular sieve raw powder with a confined mass fraction of 5% sodium tungstate, named NaW @ZSM-22-5%.

[0070] The calcined product was obtained at 750 °C in air for 1 h and named as NaW@Z-SiO2-5%.

[0071] In the absence of sodium tungstate, the W-free ZSM-22 was synthesized by the same method and named NaW@ZSM-22-0%.

[0072] The XRD characterization results are shown in Figure 1 As shown in Figure (a), it can be observed that compared with NaW@ZSM-22-0%, NaW@ZSM-22-5% exhibits a typical ZSM-22 molecular sieve structure, and no obvious diffraction peak of Na2WO4 is observed, proving that sodium tungstate is highly dispersed in the ZSM-22 molecular sieve when the sodium tungstate feed amount is 5 wt%.

[0073] After calcination at 750 °C for 1 h, the NaW@Z-SiO2-5% catalyst lost the structure of the ZSM-22 molecular sieve and transformed into a main component of α-cristobalite ( Figure 1 (b)). Similar to before calcination, the diffraction peak of Na2WO4 of NaW@Z-SiO2-5% is also weak. The two strongest diffraction peaks of Na2WO4 and α-cristobalite are selected respectively: 27.8° and 22.2°. According to the ratio of their integrated areas, I 27.8° / I 22.2° , the relative dispersion of sodium tungstate in NaW@Z-SiO2-5% catalyst can be semi-quantitatively calculated, and this method is widely used in the semi-quantitative analysis of metal species in M@Zeo catalyst. Figure 1As shown in Figure (c), NaW@Z-SiO2-5% I 27.8° / I 22.2° Only 0.9%. This proves that after high-temperature calcination, the molecular sieve confined sodium tungstate is still well dispersed in quartz.

[0074] Embodiment 2-5: Referring to the synthesis method described in Example 1, only the amount of sodium tungstate dihydrate added was changed to obtain NaW@ZSM-22-n% and NaW@Z-SiO2-n% catalysts for XRD characterization. Figure 1 As shown, n=15, 25, 35, 45.

[0075] from Figure 1 It can be observed in Figure (a) that NaW@ZSM-22-n% with different sodium tungstate loadings all exhibit a typical ZSM-22 molecular sieve structure, and no obvious Na2WO4 diffraction peaks are observed for NaW@ZSM-22-15%, NaW@ZSM-22-25%, and NaW@ZSM-22-35%, proving that sodium tungstate is highly dispersed in the ZSM-22 molecular sieve when the sodium tungstate feed amount does not exceed 35 wt%. Only when the sodium tungstate feed amount reaches 45 wt%, can an obvious Na2WO4 diffraction peak be observed, which indicates that when the amount of sodium tungstate in the catalyst is too high, the excess sodium tungstate will agglomerate in the molecular sieve structure.

[0076] After calcination at 750 °C for 1 h, the NaW@Z-SiO2-n% catalyst lost the structure of ZSM-22 molecular sieve and transformed into α-cristobalite ( Figure 1 (b)). Similar to before calcination, the diffraction peaks of Na2WO4 observed in NaW@Z-SiO2-15%, NaW@Z-SiO2-25%, and NaW@Z-SiO2-35% are very weak. Only when the sodium tungstate feed amount reaches 45 wt%, can a very obvious peak of Na2WO4 be observed. Figure 1 As shown in Figure (c), the I 27.8° / I 22.2° All of them are below 5%, while NaW@Z-SiO2-45% I 27.8° / I 22.2° It reached 52.4%. This proves that when the sodium tungstate feed reached 45%, obvious agglomeration occurred and its relative dispersion decreased sharply.

[0077] The NaW@ Z-SiO2-25% catalyst corresponding to Example 3 was selected, and the two quantitative analysis methods, ICP-MS and XPS, were further used to detect the molar ratio of W element to Si element (W / Si ratio). Based on the principles of the two characterization methods, we used XPS technology to detect the W / Si ratio of the sample surface (capable of detecting information of 0.5-4 nm on the surface), and used ICP-MS to detect the overall W / Si ratio. Figure 2 In Figure (a), the bulk W / Si ratio of the catalyst is close to the feed ratio, indicating that the dry sol conversion method has well retained the sodium tungstate put into the reaction system and avoided its loss. XPS quantitative results show that the surface W / Si of NaW@Z-SiO2-25% is close to the feed ratio. Combining the information given by the ICM-MS and XPS methods, it can be known that the bulk W element contained in the catalyst synthesized by the in-situ method has not been lost, which is consistent with the expected W / Si ratio. And due to the pore confinement effect of the ZSM-22 molecular sieve, the distribution of sodium tungstate in the entire NaW@Z-SiO2-n% catalyst is very uniform. Whether it is on the surface or in the bulk, the detected W / Si is close to the feed ratio. This is also consistent with Figure 1 The XRD results shown in Figure (a) are consistent, that is, the diffraction peak of sodium tungstate in the XRD spectrum of the NaW@Z-SiO2-25% catalyst is very weak, and its characteristic peak intensity ratio is 4.2%.

[0078] The W4f XPS spectrum of NaW@Z-SiO2-25% catalyst is shown in Figure 2 As shown in Figure (b), two characteristic peaks can be observed, located at 37.3 eV and 35.2 eV, which are completely consistent with the W4f peak position of sodium tungstate, corresponding to the photoelectrons at W4f 7 / 2 and W4f 5 / 2, respectively, while the W4f signal peak of tungsten oxide is located at 37.6 and 35.5 eV. This result proves that the state of W contained in the catalyst is sodium tungstate rather than tungsten oxide, which is consistent with the XRD results. The above results prove that the in-situ synthesis method can effectively confine the sodium tungstate species to make it evenly distributed on the catalyst surface and bulk.

[0079] In order to further study the distribution of sodium tungstate in the catalyst, the NaW@Z-SiO2-25% catalyst was characterized by high-resolution electron microscopy. Figure 3 As shown in Figure 2, a large number of clusters are evenly distributed on the surface of NaW@Z-SiO2-25%, and the average size is calculated to be 1.7 nm after particle size statistics. Figure 4 Figure (b) - Figure 4Figure (e) also proves the uniform dispersion of W and Na on the SiO2 surface. The results of electron microscopy characterization are consistent with the results of XRD, ICP and XPS, proving that the NaW@Z-SiO2-25% catalyst synthesized by the in-situ method can obtain a large number of sodium tungstate nanoclusters, and these clusters are highly dispersed in the bulk phase of the catalyst.

[0080] Embodiment 6-10 Referring to the synthesis method described in Example 1, the catalyst obtained was characterized by XRD at a loading amount of 25 wt % of the alkali metal oxoate and only the type of the alkali metal oxoate was changed. Figure 5 Figure (a) - Figure 5 As shown in Figure (e), the conclusions are shown in Table 1.

[0081] Table 1

[0082] Note: Na2CO3 is calcined at high temperature to form CO3 2- CO x The form of volatile, that is, after calcination, there is no Na2CO3 in the catalyst, so Figure 5 In the figure (e), there is no PDF card containing pure Na2CO3.

[0083] from Figure 5 Figure (a) - Figure 5 It can be observed in Figure (e) that the alkali metal oxoate@molecular sieve raw powders in Examples 6-10 all exhibit a typical ZSM-22 molecular sieve structure, and no obvious Na2WO4 diffraction peak is observed in the calcined alkali metal oxoate@Z-SiO2 catalyst, or the peak is extremely weak, proving that at a high loading of 25 wt% of oxoate feed, sodium tungstate is highly dispersed in the ZSM-22 molecular sieve and the quartz formed by calcination.

[0084] Comprehensive analysis of Examples 1-10 shows that the synthesis strategy of regulating the interaction between the alkali metal oxoate precursor and the molecular sieve precursor by controlling the amount and order of addition of acid and alkali is successful. In this synthesis strategy, the alkali metal oxoate is embedded in the amorphous SiO2 matrix in the form of acid under an acidic environment, and then the matrix environment is adjusted to alkaline so that the dispersed oxoacid is converted back into oxoacid for the crystallization of the molecular sieve. As SiO2 is consumed and crystallized into the molecular sieve, the high concentration of oxoacid inside is simultaneously encapsulated and stabilized in the molecular sieve, and can still maintain a stable and highly dispersed state after high-temperature calcination.

[0085] Comparative Example 1 After obtaining the NaW@ZSM-22-0% raw powder according to the synthesis method described in Example 1, it was calcined in air at 550 °C for 5 hours, and the template was removed to obtain a calcined product. Take 0.75 g of the calcined product and mix it with 0.28 g Na2WO4·2H2O and add it to the culture bottle, add 20 g deionized water, and stir at 65 °C until the water is completely evaporated. The obtained product was calcined in air at 750 °C for 1 hour to obtain a calcined product, named NaW / Z-SiO2-25%-imp (imp stands for impregnation). Its XRD characterization results ( Figure 6 Figure (a) - Figure 6 Figure (c) shows that the I 27.8° / I 22.2° The value is 62.3%. The quantitative results of ICP-MS and XPS are as follows Figure 2 Figure (a) - Figure 2 As shown in Figure (b), the bulk W element contained in the catalyst also did not lose, which was consistent with the expected W / Si ratio. However, the sodium tungstate contained in it was more located on the surface, resulting in more sodium tungstate agglomeration, thus showing obvious diffraction peaks on XRD, and the XPS test results also proved that the W / Si ratio on its surface was much larger than the feed ratio. At the same time, the high-resolution electron microscopy characterization results are shown in Figure 4 As shown in Figure (a).

[0086] For NaW / Z-SiO2-25%-imp, the HRTEM images show no clusters, but rather large aggregates of particles with a size of about 50 nm ( Figure 4 Middle (f) Figure - Figure 4 (i) in the middle. The EDS image shows the agglomeration of W and Na elements, and the location of the agglomeration is the same as the location of the large particles in the HAADF image, which also proves that the agglomerated particles are sodium tungstate. Both prove that the conventional synthesis method of impregnation will cause obvious agglomeration of sodium tungstate species, making NaW / Z-SiO2-25%-imp show more sodium tungstate nanoparticles.

[0087] Comparative Example 2 Referring to the synthesis method of Example 1, NaW@ZSM-22-25%-NT (NT stands for no template) was synthesized by the same method without adding [BMIm]Br, and calcined at 750 °C in an air atmosphere for 1 hour to obtain a calcined product, named NaW@SiO2-25%-NT.

[0088] Comparative Example 3 Referring to the synthesis method of Example 1, NaW@ZSM-22-25%-UH (UH represents no high temperature evaporation crystallization) was synthesized by the same method without high temperature evaporation crystallization, and NaW@SiO2-25%-UH was obtained by direct calcination.

[0089] From the XRD characterization results of Comparative Examples 2-3 ( Figure 7 Figure (a) - Figure 7 It can be observed in Figure (c) that before calcination, only NaW@ZSM-22-25% showed the typical ZSM-22 molecular sieve structure, while NaW@ZSM-22-25%-UH and NaW@ZSM-22-25%-NT only showed the diffraction peak of sodium tungstate, indicating that the SiO2 of the two was still in an amorphous state and no molecular sieve structure was formed in situ. After calcination at 750 °C for 1 hour, all three were transformed into α-cristobalite as the main body. The sodium tungstate diffraction peak of NaW@Z-SiO2-25% was the weakest, while the sodium tungstate diffraction peaks of NaW@SiO2-25%-UH and NaW@SiO2-25%-NT were relatively obvious. From I 27.8° / I 22.2° The value of I 27.8° / I 22.2° The value is only 4.4%, while the I 27.8° / I 22.2° The values ​​are 70.3% and 68.4% respectively. This result shows that in the in-situ synthesis method, only when the two conditions of template addition and hydrothermal treatment are met at the same time, can the molecular sieve structure of ZSM-22 be formed in situ and the pore confinement of sodium tungstate be achieved, so that sodium tungstate can be evenly dispersed in the catalyst. If any one of the conditions is not met, the molecular sieve structure cannot be formed, and the final catalyst will also show agglomeration of sodium tungstate. This result proves that the in-situ formed ZSM-22 molecular sieve structure has an important influence on the dispersion of sodium tungstate, and this influence is achieved through the pore confinement of the molecular sieve.

[0090] Comparative Example 4 Referring to the synthesis method of Example 1, NaW@ZSM-22-25%-NOH (NOH stands for no alkali added) was synthesized by the same method without adding sodium hydroxide aqueous solution, and calcined at 750 °C in an air atmosphere for 1 hour to obtain a calcined product, named NaW@SiO2-25%-NOH.

[0091] Comparative Example 5 Referring to the synthesis method of Example 1, NaW@ZSM-22-25%-NH (NH represents no acid addition) was synthesized by the same method without adding sulfuric acid aqueous solution. However, after adding alkaline solution to the precursor, a large amount of sticky precipitate was formed and a gel could not be formed, that is, the subsequent synthesis steps could not be carried out.

[0092] Comparative Example 6 Referring to the synthesis method of Example 1, NaW@ZSM-22-25%-OHH (OHH represents the addition of alkali before acid) was synthesized by the same method except that the order of adding the aqueous sulfuric acid solution and the aqueous sodium hydroxide solution was reversed. The product was calcined at 750 °C in an air atmosphere for 1 hour to obtain a calcined product, named NaW@SiO2-25%-OHH.

[0093] Comparative Example 7 Referring to the synthesis method of Example 1, except that the sulfuric acid aqueous solution and the sodium hydroxide aqueous solution were not added, NaW@ZSM-22-25%-NHOH (NHOH represents no acid and alkali solution was added) was synthesized by the same method, and calcined at 750 °C in an air atmosphere for 1 hour to obtain a calcined product, named NaW@SiO2-25%-NHOH.

[0094] The XRD results of Comparative Examples 4, 6, and 7 are as follows: Figure 8 As shown, it can be seen that although the sodium tungstate diffraction peak of the corresponding catalyst of Comparative Example 4 is not strong, the tungsten oxide peak is obvious. From the perspective of the synthesis effect, it is confirmed that the presence of acid and base and the order of their addition play a crucial role in the high concentration and high dispersion of alkali metal oxoacids. Alkali metal oxoacids are stably present in an alkaline environment, and will become the corresponding acid in an acidic environment, and then become metal oxides after calcination. However, the solution of the oxoacid precursor in the molecular sieve precursor is easy to form a block precipitate and then separate from the molecular sieve carrier later. Only in the form of acid in an acidic environment can it be stably cross-linked with the amorphous SiO2 precursor of the molecular sieve to disperse, and then converted into oxoacids in an alkaline environment for evaporation and crystallization, and finally the oxoacid clusters can be highly dispersed under high loading.

[0095] Comparative Example 8 Referring to the synthesis method of Comparative Example 1, 0.28 g Na2WO4·2H2O was replaced with 0.25 g NaVO3, and NaV / ZSM-22-25%-imp was synthesized by the same method. The product was calcined at 750 °C in air atmosphere for 1 hour to obtain a calcined product named NaV / SiO2-25%-imp. XRD characterization is shown in Figure 5 As shown in Figure (a).

[0096] Comparative Example 9 Referring to the synthesis method of Example 6, NaV@ZSM-22-25%-NOH (NOH stands for no alkali added) was synthesized by the same method without adding sodium hydroxide aqueous solution, and calcined at 750 °C in an air atmosphere for 1 hour to obtain a calcined product, named NaV@SiO2-25%-NOH.

[0097] Comparative Example 10 Referring to the synthesis method of Example 6, NaV@ZSM-22-25%-NH (NH represents no acid addition) was synthesized by the same method without adding sulfuric acid aqueous solution. However, after adding alkaline solution to the precursor, a large amount of sticky precipitate was also formed, and a gel could not be formed, that is, the subsequent synthesis steps could not be carried out.

[0098] Comparative Example 11 Referring to the synthesis method of Example 6, NaV@ZSM-22-25%-OHH (OHH represents the addition of alkali before acid) was synthesized by the same method except that the order of adding the aqueous sulfuric acid solution and the aqueous sodium hydroxide solution was reversed. The product was calcined at 750 °C in an air atmosphere for 1 hour to obtain a calcined product, named NaV@SiO2-25%-OHH.

[0099] Comparative Example 12 Referring to the synthesis method of Example 6, NaV@ZSM-22-25%-NHOH (NHOH represents no acid and alkali solution) was synthesized by the same method without adding acid or alkali solution, and calcined at 750 °C in air atmosphere for 1 hour to obtain a calcined product, named NaV@Z-SiO2-25%-NHOH.

[0100] Embodiment 11 We selected the catalysts obtained from some embodiments and comparative examples as typical representatives and conducted catalytic performance tests on the oxidative coupling of methyl chloride to vinyl chloride. The catalytic performance at 725 °C is shown in Table 2.

[0101] Table 2

[0102]

[0103] Reaction conditions: catalyst 150 mg, gas flow rate (mL / min) CH3Cl:O2:N2=1:2:57, total gas flow rate 60 mL min −1 The catalytic data are selected at the temperature corresponding to the highest conversion rate / selectivity / yield.

[0104] Taking Example 12 as an example, the trend of the reaction catalytic performance changing with temperature is as follows Fig. 9 Figure (a) - Fig. 9As shown in Figure (c), during the entire test process, the selectivity of vinyl chloride was greater than 55%, while the conversion rate of methyl chloride and the yield of vinyl chloride increased with the increase of reaction temperature. When the reaction temperature was 725 °C, the highest value was reached, and the yield of vinyl chloride could reach 54.5%. The stability of the catalyst is an important indicator for evaluating the catalytic performance. Fig. 9 As shown in Figure (d), in the 50-hour stability test at 725 °C, the reaction performance did not decrease significantly, proving the catalytic stability of the reaction of the present invention. In summary, the excellent catalytic performance of this route has potential industrial value.

[0105] From the data of Examples 11-13, 23, and 24, it can be seen that with the increase of sodium tungstate loading, the methyl chloride conversion rate of the NaW@Z-SiO2-n% catalyst gradually increases, and the conversion rate of NaW@Z-SiO2-25% is the highest, reaching nearly 80% at 725 °C. NaW@Z-SiO2-0% and pure sodium tungstate show extremely low vinyl chloride selectivity, while the vinyl chloride selectivity of NaW@Z-SiO2-5% and NaW@Z-SiO2-25% is higher than 65%. When the loading is further increased, the vinyl chloride selectivity of NaW@Z-SiO2-45% suddenly decreases significantly, only 43%. From the yield of vinyl chloride, NaW@Z-SiO2-0% and pure sodium tungstate have the lowest yield, and NaW@Z-SiO2-25% has the highest yield, which can reach 54.5% at 725 °C.

[0106] Combination Figure 1 Figure (a) - Figure 1 From the XRD results in Figure (c) and the calculation of the relative dispersion of sodium tungstate, we can infer that: (1) Pure sodium tungstate has basically no MCTV activity without loading and dispersion, and the catalyst has basically no MCTV catalytic activity when sodium tungstate is not loaded. The corresponding MCTV catalytic activity is also poor when sodium tungstate is loaded in the ZSM-22 molecular sieve structure but clustered. (2) Sodium tungstate is the active center of the NaW@Z-SiO2-n% catalyst, and its relative dispersion has an important influence on the catalyst activity, especially for the conversion rate of methyl chloride. Within a certain feed range (5 wt%-35 wt%), the larger the feed amount of sodium tungstate, the higher the concentration of highly dispersed sodium tungstate species on the catalyst, and the higher the conversion rate. However, the selectivity of vinyl chloride is not sensitive to this. Only a small amount of dispersed sodium tungstate species is needed to show a high selectivity of vinyl chloride.

[0107] From the data of Examples 12 and 14, it can be seen that the chloromethane conversion rates of NaW@Z-SiO2-25% and NaW / Z-SiO2-25%-imp are basically close, but the vinyl chloride selectivity of NaW@Z-SiO2-25% is much higher than that of W@Z-SiO2-25%-imp. The vinyl chloride yield results of the two catalysts also show that the vinyl chloride yield of NaW@Z-SiO2-25% is higher, reaching 54.5% at 725 °C, while the vinyl chloride yield of NaW@Z-SiO2-25%-imp is only 18.6% at the same temperature. The results of the catalytic experiment show that under the premise of the same sodium tungstate feed amount, the NaW@Z-SiO2-25% catalyst with highly dispersed sodium tungstate clusters has a better ability to oxidatively couple chloromethane to vinyl chloride. However, due to the agglomeration of sodium tungstate species, the catalytic performance of NaW@Z-SiO2-25%-imp catalyst is poor, which further proves that dispersed sodium tungstate clusters are the active centers of the oxidative coupling reaction of methyl chloride to produce vinyl chloride. Achieving high dispersion of sodium tungstate clusters is the key to obtaining better performance of the catalyst.

[0108] The data of Examples 12, 15-17 further confirm from the perspective of catalytic effect that the presence of acid and base and the order of their addition play a crucial role in the high concentration and high dispersion of alkali metal oxoacid salts. Whether the acid-base order is reversed, no base is added, or neither base nor acid is added, the selectivity of the corresponding catalyst is very poor, resulting in a very low yield.

[0109] The data of Examples 18-22 show a law that is basically consistent with that of Examples 12, 14-17 from the perspective of NaVO3. In addition, taking Example 18 as an example, a high temperature stability performance test was performed, and the stability performance was also excellent. This also further proves that it is completely feasible to expand the synthesis method explored by the invention from sodium tungstate, an alkali metal oxoacid salt, to sodium metavanadate and other alkali metal oxoacid salts. The corresponding catalytic properties of the remaining alkali metal oxoacid salts will not be repeated.

[0110] In summary, we have innovatively explored a technical means to adjust the acid-base environment of the alkali metal oxoate precursor and the amorphous SiO2 precursor of the molecular sieve, and achieved a highly dispersed state of the oxoate clusters at a high loading, and at the same time, this technical means did not affect the skeleton formation of the molecular sieve. The in-situ obtained sample was calcined at high temperature to finally obtain a catalyst in which the oxoate active sites were highly dispersed on the SiO2 carrier - alkali metal oxoate @SiO2. This catalyst helps to greatly improve the product yield and stability of chloromethane oxidative coupling to vinyl chloride, and also helps to solve the problems of expensive raw materials and high pollution in the synthesis of catalysts in this field. The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, several improvements and modifications can be made, and these improvements and modifications are also regarded as the scope of protection of the present invention.

Claims

1. A method for synthesizing a molecular sieve of stable confined alkali metal oxoate nanoclusters, characterized in that: Ionic liquid is used as a template, inorganic acid and alkali metal oxoate precursor are first added to a silicon source, and then an inorganic base and a template are added, and alkali metal oxoate@ZSM-22 molecular sieve raw powder is synthesized under the condition of evaporation-assisted crystallization.

2. The method according to claim 1, characterized in that: The specific steps include: Step S1, stirring the inorganic acid and the silicon source at room temperature for 5-12 hours, then adding the alkali metal oxoate precursor, and ensuring that the pH value of the solution reaches 3-6, and then continuing to stir for a second time for 6-24 hours to obtain a mixed solution; Step S2, adding an inorganic base to the mixed solution of step S1 until the pH value reaches 8-12, stirring for 0.5-3 hours, then adding an ionic liquid as a template, and then stirring for a second time for 6-24 hours to form a gel system; Step S3, directly drying the gel system of step S2 to obtain a solid xerosol; Step S4, taking the solid dry sol and water and placing them on the upper and lower layers of the lining in the reaction kettle respectively, and performing high-temperature evaporation and crystallization; Step S5, drying the solid product obtained by cooling after the crystallization in step S4 to obtain the original powder of oxygen acid salt @ ZSM-22.

3. The method according to claim 2, characterized in that: In step S1, the inorganic acid source is selected from at least one of sulfuric acid, nitric acid, hydrochloric acid, and phosphoric acid; the silicon source is selected from at least one of tetraethyl orthosilicate and silica gel; the oxoacid salt precursor is selected from at least one of tungstate, metavanadate, molybdate, sulfate, phosphate, and carbonate; the alkali metal is selected from at least one of sodium and potassium; In step S2, the template agent is 1-butyl-3-methylimidazole hydrobromide; and the inorganic base is selected from at least one of sodium hydroxide and potassium hydroxide.

4. The method according to claim 2, characterized in that: In step S1, the molar ratio of the effective component SiO2 in the silicon source to the solvent in the mixed solution is 1:20-50; wherein the solvent in the mixed solution is H2O; In step S2, the molar ratio of the effective ingredient SiO2 in the silicon source, the template, and the solvent in the gel system is 1:0.2-0.4:30-60, wherein the solvent in the gel system is H2O.

5. The method according to claim 2, characterized in that: In step S1, the mass fraction of the alkali metal oxosalt precursor is 5 wt%-55 wt%.

6. The method according to claim 2, characterized in that: In step S4, the evaporation crystallization temperature is 160-180° C.; and the evaporation crystallization time is 48-100 hours.

7. A molecular sieve of stable confined high-concentration alkali metal oxoate nanoclusters, prepared by the method according to any one of claims 1 to 6.

8. A silicon-based composite material of SiO2 confined alkali metal oxoate nanoclusters, characterized in that The molecular sieve according to claim 7 is obtained by high temperature calcination.

9. The silicon-based composite material according to claim 8, characterized in that: The calcination temperature is 700-800°C, the calcination time is 1 hour, and the calcination atmosphere is air.

10. Use of the catalyst in the oxidative coupling reaction of methyl chloride to prepare vinyl chloride, characterized in that: The catalyst adopts the silicon-based composite material according to any one of claims 8-9.

Citation Information

Patent Citations

  • Zeolite molecular sieve as well as preparation method and application thereof

    CN108706607A

  • Hydrodesulfurization catalyst as well as preparation method and application thereof

    CN114073980A

  • Composite oxide containing tungstate nanoclusters, and preparation method and application thereof

    CN114377671A

  • Method for preparing vinyl chloride through oxidative coupling of high-selectivity chloromethane

    CN118084610A

  • Oxidative coupling of methane catalyst and preparation method for same