Glass composition
By rationally designing the components of the glass composition, the problems of poor transmittance and high wear in optical fiber transmission are solved, high light transmittance and excellent wear, meeting environmental protection and health requirements, and reducing the problem of existing glasses. cost and environmental impact.
Patent Information
- Application Number
- CN202411314577.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-26
AI Technical Summary
Existing glasses have poor transmittance and high wear and are difficult to meet the requirements of environmental protection policies and health awareness, especially when they do not contain lead and arsenic compounds, it is difficult to achieve high refractive index and excellent light transmission. Overrate.
By rationally designing the components of the glass composition, it contains components such as SiO2, B2O3, BaO, SrO and La2O3, and controls its proportions to achieve high light transmittance and excellent wear. The specific components range is SiO2 17-32%, B2O3 18 -32%, La2O3/SiO2 0.3-1.2, B2O3/SiO2 0.7-1.7, La2O3/SiO2 0.3-1.2, La2O3+SrO/BaO 0.5-2.5, etc., combined with other ingredients such as Al2O3, ZrO2, Nb2O5, WO3, etc., optimize glass optical and mechanical properties.
It achieves high light transmittance and excellent wear, meets environmental protection and health requirements, while reducing the cost and environmental impact of glass.
Smart Images

Figure BDA0005051776720000131 
Figure BDA0005051776720000141 
Figure BDA0005051776720000171
Abstract
Description
Technical Field
[0001] The present invention relates to a glass composition, and in particular to a glass composition with high light transmittance and excellent abrasiveness. Background Art
[0002] In recent years, glass has been used in various devices, especially as a multi-component optical fiber core used in light guides, image conductors, and endoscopes. Glass used in the above fields is required to have a higher refractive index to increase the amount of light transmitted. In most cases, the transmission path using optical fiber is longer, and the transmission loss becomes larger when the transmittance of the glass is poor, so the glass is required to have excellent light transmittance. In the prior art, the above performance is mainly achieved by adding a high content of PbO to the glass, but with the requirements of environmental protection policies and the improvement of health awareness, lead-containing glass cannot meet the requirements of environmental protection. CN103466936A discloses a glass core material for optical fiber with a refractive index of more than 1.50. Although its components do not contain lead compounds and arsenic compounds, it contains a high content of GeO2, and the cost of glass raw materials is relatively high.
[0003] Generally, glass preforms can be made by mechanical processing such as grinding or polishing of glass, or by making a preform for molding from glass, hot pressing the preform and then grinding the preform to make a glass preform, or by precision stamping the preform made by grinding to make a glass preform, which requires the glass to have good processing performance. CN115385575A discloses a glass with a refractive index of 1.55 to 1.62 and an Abbe number of 55 to 62.97. The glass has a high abrasiveness, which increases the difficulty of precision machining of the glass. Therefore, it is expected that the glass composition has excellent abrasiveness. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a glass composition with high light transmittance and excellent abrasiveness.
[0005] The technical solution adopted by the present invention to solve the technical problem is:
[0006] (1) A glass composition, wherein the components are expressed in weight percentage and contain: SiO2: 17-32%; B2O3: 18-32%; BaO: 12-27.5%; SrO: 2-15%; Ln2O3: 7.5-28%, wherein La2O3 / SiO2 is 0.3-1.2, and Ln2O3 is the total content of La2O3, Gd2O3, Y2O3, and Yb2O3.
[0007] (2) The glass composition according to (1), wherein the components, expressed in weight percentage, further contain: Al2O3: 0-10%; and / or ZrO2: 0-10%; and / or Nb2O5: 0-5%; and / or WO3: 0-5%; and / or ZnO: 0-4.5%; and / or Rn2O: 0-6.5%; and / or MgO: 0-5%; and / or CaO: 0-4%; and / or TiO2: 0-5%; and / or Ta2O5: 0-5%; and / or P2O5: 0-4%; and / or F: 0-5%; and / or a clarifier: 0-1%, wherein the Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO2, SnO, and CeO2.
[0008] (3) A glass composition comprising SiO2, B2O3, BaO, SrO and La2O3, wherein the composition is expressed in weight percentage, wherein La2O3 / SiO2 is 0.3 to 1.2, and the abrasiveness F of the glass composition is A Below 200.
[0009] (4) The glass composition according to (3), wherein the components, expressed in weight percentage, include: SiO2: 17-32%; and / or B2O3: 18-32%; and / or BaO: 12-27.5%; and / or SrO: 2-15%; and / or Ln2O3: 7.5-28%; and / or Al2O3: 0-10%; and / or ZrO2: 0-10%; and / or Nb2O5: 0-5%; and / or WO3: 0-5%; and / or ZnO: 0-4.5%; and / or Rn2O ...10%; and / or ZnO: 0-4.5%; and / or Rn2O: 0-10%; and / or ZrO2: 0-10%; and / or ZrO2: 0-10%; and / or Nb2O5: 0-5%; and / or WO3: 0-10%; and / or ZnO: 0-10%; and / or ZrO: 0-10%; and / or ZrO: 0-10%; and / or ZrO: 0-10%; and / or ZrO: 0-10%; and / or ZrO: 0-10%; and / or ZrO: 0-10%; and / or ZrO: 0-10%; and / or ZrO: 6.5%; and / or MgO: 0-5%; and / or CaO: 0-4%; and / or TiO2: 0-5%; and / or Ta2O5: 0-5%; and / or P2O5: 0-4%; and / or F: 0-5%; and / or clarifier: 0-1%, wherein Ln2O3 is the total content of La2O3, Gd2O3, Y2O3, and Yb2O3, Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO2, SnO, and CeO2.
[0010] (5) The glass composition according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: B2O3 / SiO2 is 0.7 to 1.7, preferably B2O3 / SiO2 is 0.75 to 1.5, more preferably B2O3 / SiO2 is 0.8 to 1.3, and further preferably B2O3 / SiO2 is 0.85 to 1.1; and / or (La2O3+SrO) / BaO is 0.5 to 2.5, preferably (La2O3+SrO) / BaO is 0.7 to 2.0, more preferably (La2O3+SrO) / BaO is 0.8 to 1.8, and further preferably (La2O3+SrO) / BaO is 0.9 to 1.5; and / or SrO / La2O3 is 0.1 to 1.5, preferably SrO / La2 O3 is 0.2~1.2, more preferably SrO / La2O3 is 0.3~1.0, and further preferably SrO / La2O3 is 0.35~0.8; and / or La2O3 / SiO2 is 0.35~1.0, preferably La2O3 / SiO2 is 0.4~0.9, and more preferably La2O3 / SiO2 is 0.45~0.8; and / or (BaO+SrO) / (ZrO2+Al2O3) is 1.0~15.0, preferably (BaO+SrO) / (ZrO2+Al2O3) is 1.5~10.0, more preferably (BaO+SrO) / (ZrO2+Al2O3) is 2.0~8.0, and further preferably (BaO+SrO) / (ZrO2+Al2O3) is 2.5~5.0.
[0011] (6) A glass composition according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: Al2O3 / B2O3 is 0.01 to 0.45, preferably Al2O3 / B2O3 is 0.05 to 0.4, and more preferably Al2O3 / B2O3 is 0.1 to 0.3; and / or ZrO2 / SiO2 is 0.01 to 0.4, preferably ZrO2 / SiO2 is 0.05 to 0.35, and more preferably ZrO2 / SiO2 is 0.1 to 0.3; and / or Al2O3 / ZrO2 is 0.2 to 8.0, preferably Al2O3 / ZrO2 is 0.5 to 6.0, more preferably Al2O3 / ZrO2 is 0.8 to 4.0, and further preferably Al2O3 / ZrO2 is 1.0 to 2.0; and / or (Y2O3+Gd2O3+ZnO+CaO+R Preferably, (Y2O3+Gd2O3+ZnO+CaO+Rn2O) / SrO is less than 1.0, preferably (Y2O3+Gd2O3+ZnO+CaO+Rn2O) / SrO is less than 0.8, more preferably (Y2O3+Gd2O3+ZnO+CaO+Rn2O) / SrO is less than 0.5, and further preferably (Y2O3+Gd2O3+ZnO+CaO+Rn2O) / SrO is less than 0.3; and / or (ZnO+CaO+Rn2O) / La2O3 is less than 1.0, preferably (ZnO+CaO+Rn2O) / La2O3 is less than 0.8, more preferably (ZnO+CaO+Rn2O) / La2O3 is less than 0.5, and further preferably (ZnO+CaO+Rn2O) / La2O3 is less than 0.3, and the Rn2O is one or more of Li2O, Na2O, and K2O.
[0012] (7) The glass composition according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: SiO2: 21-30%, preferably SiO2: 22-28%; and / or B2O3: 21-30%, preferably B2O3: 22-29%; and / or Ln2O3: 10-25%, preferably Ln2O3: 11-20%; and / or BaO: 15-25%, preferably BaO: 16-23%; and / or SrO: 3-13%, preferably SrO: 5 .5~11%; and / or Al2O3: 1~8%, preferably Al2O3: 2~7%; and / or ZrO2: 0.5~8%, preferably ZrO2: 1~7%; and / or Nb2O5: 0~3%, preferably Nb2O5: 0~1%, more preferably no Nb2O5; and / or WO3: 0~3%, preferably WO3: 0~1%, more preferably no WO3; and / or ZnO: 0~3%, preferably ZnO: 0~2%, more preferably no ZnO; and / or Rn2 O: 0-5%, preferably Rn2O: 0-2%; and / or MgO: 0-3%, preferably MgO: 0-2%, more preferably no MgO; and / or CaO: 0-3%, preferably CaO: 0-2%, more preferably no CaO; and / or TiO2: 0-3%, preferably TiO2: 0-2%, more preferably no TiO2; and / or Ta2O5: 0-3%, preferably Ta2O5: 0-1%, more preferably no Ta2O5; and / or P2O5: 0-2 %, preferably P2O5: 0-1%, more preferably no P2O5; and / or F: 0-3%, preferably F: 0-2%, more preferably no F; and / or clarifier: 0-0.5%, preferably clarifier: 0-0.2%, the Ln2O3 is the total content of La2O3, Gd2O3, Y2O3, and Yb2O3, Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO2, SnO, and CeO2.
[0013] (8) The glass composition according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: La2O3: 7.5-23%, preferably La2O3: 11-20%, more preferably La2O3: 12-18%; and / or Gd2O3: 0-8%, preferably Gd2O3: 0-5%, more preferably Gd2O3: 0-1.5%, and more preferably no Gd2O3; and / or Y2O3: 0-8%, preferably Y2O3: 0-5%, more preferably Y2O3: 0-1.5%, and more preferably no Y2O3 ; and / or Yb2O3: 0-5%, preferably Yb2O3: 0-3%, more preferably Yb2O3: 0-2%, and further preferably, it does not contain Yb2O3; and / or Li2O: 0-5%, preferably Li2O: 0-3%, more preferably Li2O: 0-2%; and / or Na2O: 0-5%, preferably Na2O: 0-3%, more preferably Na2O: 0-2%, and further preferably, it does not contain Na2O; and / or K2O: 0-5%, preferably K2O: 0-3%, more preferably K2O: 0-2%, and further preferably, it does not contain K2O.
[0014] (9) The glass composition according to any one of (1) to (4), wherein the average light transmittance τ at 400 to 800 nm of the glass composition having a thickness of 12 mm or less 400~800nm 99.0% or more, preferably 99.5% or more, more preferably 99.7% or more; and / or the 400nm light transmittance τ of the glass composition with a thickness of 12 mm or less 400nm It is 99.0% or more, preferably 99.5% or more, and more preferably 99.7% or more.
[0015] (10) The glass composition according to (9), wherein the thickness of the glass composition is 1 to 12 mm, preferably 2 to 12 mm, more preferably 5 to 10 mm, and even more preferably 2 mm, 5 mm, 8 mm, or 10 mm.
[0016] (11) The glass composition according to any one of (1) to (4), wherein the refractive index n of the glass composition is d 1.59 to 1.66, preferably 1.60 to 1.65, more preferably 1.61 to 1.64; and / or Abbe number ν d 55 to 61, preferably 56 to 60, more preferably 57 to 59; and / or transition temperature T g 650°C or less, preferably 600-650°C, more preferably 605-645°C, and further preferably 610-640°C; and / or water resistance stability D W 3 or more, preferably 2 or more, more preferably 1; and / or density ρ is 3.60 g / cm 3Below, preferably 3.50g / cm 3 Below, more preferably 3.40g / cm 3 Below; and / or Knoop hardness H K 500×10 7 Pa or more, preferably 515×10 7 Pa or more, more preferably 530×10 7 Pa or more; and / or Young's modulus E is 7000×10 7 Pa or more, preferably 7300×10 7 Pa or more, more preferably 7600×10 7 Pa or above; and / or wear degree F A 200 or less, preferably 175 or less, more preferably 150 or less; and / or thermal expansion coefficient α 20 / 300℃ 90×10 -7 / K or less, preferably 50×10 -7 / K~85×10 -7 / K, more preferably 55×10 -7 / K~80×10 -7 / K, more preferably 60×10 -7 / K~72×10 -7 / K; and / or a high temperature viscosity of 60 dPaS or less at 1200°C, preferably 40 dPaS or less, more preferably 30 dPaS or less; and / or an anti-crystallization performance of B grade or above, preferably A grade.
[0017] (12) A glass preform made of the glass composition described in any one of (1) to (11).
[0018] (13) A glass element made of the glass composition described in any one of (1) to (11) or the glass preform described in (12).
[0019] (14) An optical instrument comprising the glass composition described in any one of (1) to (11), or comprising the glass element described in (13).
[0020] The beneficial effects of the present invention are: through reasonable component design, the glass composition obtained by the present invention has higher light transmittance and excellent abrasiveness. DETAILED DESCRIPTION
[0021] The embodiments of the glass composition of the present invention are described in detail below. However, the present invention is not limited to the embodiments described below, and can be implemented with appropriate changes within the scope of the purpose of the present invention. In addition, although the description of the repeated description may be appropriately omitted, the gist of the invention is not limited thereto. In the following content, the glass composition of the present invention is sometimes referred to as glass.
[0022] [Glass composition]
[0023] The range of each component of the glass composition of the present invention is described below. In this specification, unless otherwise specified, the content, total content, and total content of each component are all expressed as a weight percentage relative to the total amount of glass material in terms of oxide-converted composition. Here, the "composition converted to oxides" means that when oxides, complex salts, hydroxides, etc. used as raw materials for the glass composition of the present invention decompose and convert into oxides during melting, the total amount of the oxide material is taken as 100%.
[0024] Unless otherwise indicated in specific circumstances, the numerical ranges listed herein include upper and lower limits, "above" and "below" include the endpoints, and all integers and fractions included in the range, without being limited to the specific values listed when the range is defined. "And / or" referred to herein is inclusive, for example, "A and / or B" means only A, or only B, or both A and B.
[0025] <Essential Components and Optional Components>
[0026] SiO2 is the skeleton of the glass composition. As a glass network generator, it has the function of maintaining the chemical stability of the glass and improving the resistance to devitrification of the glass. If the SiO2 content is less than 17%, the above effect is not obvious, so the lower limit of the SiO2 content is 17%, preferably 21%, and more preferably 22%. If the SiO2 content is higher than 32%, the melting property of the glass decreases, the transition temperature and high temperature viscosity increase, which is not conducive to the improvement of the light transmittance of the glass. Therefore, the upper limit of the SiO2 content is 32%, preferably 30%, and more preferably 28%.
[0027] B2O3 is a component that forms a glass network structure and is an essential component of the glass of the present invention. By containing more than 18% of B2O3, the glass's meltability, resistance to devitrification and light transmittance can be improved. If the content of B2O3 exceeds 32%, the chemical stability of the glass deteriorates, the glass volatilization increases, which is not conducive to the stable control of optical constants, and the striation degree is easily deteriorated. Therefore, the content of B2O3 is 18-32%, preferably 21-30%, and more preferably 22-29%.
[0028] In some embodiments, the ratio B2O3 / SiO2 between the content of B2O3 and the content of SiO2 is controlled within the range of 0.7 to 1.7, which can reduce the high temperature viscosity of the glass while preventing the Young's modulus from decreasing. Therefore, preferably B2O3 / SiO2 is 0.7 to 1.7, and more preferably B2O3 / SiO2 is 0.75 to 1.5. Furthermore, controlling B2O3 / SiO2 within the range of 0.8 to 1.3 can further optimize the transmittance and thermal expansion coefficient of the glass. Therefore, it is further preferred that B2O3 / SiO2 is 0.8 to 1.3, and it is further preferred that B2O3 / SiO2 is 0.85 to 1.1.
[0029] La2O3 is an essential component of the glass of the present invention, which can increase the refractive index of the glass, improve the chemical stability and mechanical strength of the glass, and reduce the relative partial dispersion of the glass. In the present invention, the above effects are obtained by containing more than 7.5% La2O3, preferably more than 11% La2O3, and more preferably more than 12% La2O3. If the content of La2O3 exceeds 23%, the anti-crystallization property and thermal stability of the glass tend to deteriorate. Therefore, the content of La2O3 in the present invention is less than 23%, preferably less than 20%, and more preferably less than 18%.
[0030] In some embodiments, the ratio La2O3 / SiO2 between the content of La2O3 and the content of SiO2 is controlled within the range of 0.3 to 1.2, so that the glass can have excellent abrasion resistance while preventing the transition temperature from increasing. Therefore, La2O3 / SiO2 is preferably 0.3 to 1.2, and more preferably La2O3 / SiO2 is 0.35 to 1.0. Furthermore, controlling La2O3 / SiO2 within the range of 0.4 to 0.9 can further optimize the light transmittance of the glass. Therefore, La2O3 / SiO2 is further preferably 0.4 to 0.9, and even more preferably La2O3 / SiO2 is 0.45 to 0.8.
[0031] Gd2O3 can improve the refractive index and chemical stability of glass, but if its content is higher than 8%, the devitrification resistance and abrasion resistance of glass will deteriorate. Therefore, the content of Gd2O3 is 0 to 8%, preferably 0 to 5%, and more preferably 0 to 1.5%. In some embodiments, it is further preferred that Gd2O3 is not contained.
[0032] Y2O3 can increase the refractive index of glass, reduce density and upper crystallization temperature, but if its content is higher than 8%, the devitrification resistance and weather resistance of glass will deteriorate. Therefore, the content of Y2O3 in the present invention is 0-8%, preferably 0-5%, and more preferably 0-1.5%. In some embodiments, it is further preferred that Y2O3 is not contained.
[0033] Yb2O3 is also a component that gives glass high refractive and low dispersion properties. If its content exceeds 5%, the anti-crystallization performance of the glass deteriorates. Therefore, the content of Yb2O3 is 0-5%, preferably 0-3%, and more preferably 0-2%. In some embodiments, it is further preferred that Yb2O3 is not contained.
[0034] In some embodiments, the total content of La2O3, Gd2O3, Y2O3, and Yb2O3, Ln2O3, is controlled within the range of 7.5 to 28%, which can easily obtain the desired refractive index, improve chemical stability, and prevent the deterioration of the anti-crystallization performance of the glass. Therefore, the content of Ln2O3 is preferably 7.5 to 28%, more preferably 10 to 25%, and further preferably 11 to 20%.
[0035] ZrO2 can adjust the optical constants of glass, improve the resistance to devitrification and chemical stability. If its content exceeds 10%, the melting performance of the glass will decrease, the melting temperature will increase, and it will easily lead to inclusions inside the glass and its transmittance will decrease, and it will be difficult to maintain a low transition temperature. Therefore, the ZrO2 content is 0-10%, preferably 0.5-8%, and more preferably 1-7%.
[0036] In some embodiments, the ratio of ZrO2 to SiO2, ZrO2 / SiO2, is controlled within the range of 0.01 to 0.4, which can improve the hardness and chemical stability of the glass and prevent the deterioration of the anti-crystallization performance. Therefore, ZrO2 / SiO2 is preferably 0.01 to 0.4, more preferably ZrO2 / SiO2 is 0.05 to 0.35, and further preferably ZrO2 / SiO2 is 0.1 to 0.3.
[0037] Nb2O5 has the effect of increasing the refractive index and dispersion of glass, and can also improve the anti-devitrification and chemical stability of glass. If its content exceeds 5%, the dispersion of glass increases, and the optical properties of the glass of the present invention cannot be achieved. At the same time, the light transmittance of glass decreases. Therefore, the content of Nb2O5 is 0-5%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that Nb2O5 is not contained.
[0038] WO3 can improve the refractive index and dispersion of glass. If its content is too high, the light transmittance of the glass will decrease and the anti-crystallization performance will deteriorate. Therefore, the content of WO3 is 0-5%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that WO3 is not contained.
[0039] ZnO can lower the transition temperature of glass, improve the chemical stability of glass, and reduce the high temperature viscosity of glass. If the ZnO content is too high, the anti-crystallization performance of glass will deteriorate and the thermal expansion coefficient will increase. Therefore, the content of ZnO in the present invention is 0 to 4.5%, preferably 0 to 3%, and more preferably 0 to 2%. In some embodiments, it is further preferred that ZnO is not contained.
[0040] Alkali metal oxide Rn2O (Rn2O is one or more of Li2O, Na2O, K2O) can reduce the transition temperature of glass, adjust the optical constants and high temperature viscosity of glass, and improve the melting property of glass. However, when its content is high, the devitrification resistance and chemical stability of glass are reduced. Therefore, the content of Rn2O in the present invention is 0 to 6.5%, preferably 0 to 5%, and more preferably 0 to 2%.
[0041] Li2O can reduce the transition temperature of glass, but its high content is not good for the acid resistance stability and thermal expansion coefficient of glass, and it can corrode the melting container (such as platinum crucible). Therefore, the content of Li2O is 0-5%, preferably 0-3%, and more preferably 0-2%.
[0042] Na2O has the effect of improving the melting property of glass and lowering the glass transition temperature. When its content is too high, the chemical stability and weather resistance of glass are reduced. Therefore, the content of Na2O is 0 to 5%, preferably 0 to 3%, and more preferably 0 to 2%. In some embodiments, it is further preferred that Na2O is not contained.
[0043] K2O has the effect of improving the thermal stability and melting property of glass, but when the content of K2O exceeds 5%, the devitrification resistance of glass decreases. Therefore, the content of K2O is 0 to 5%, preferably 0 to 3%, and more preferably 0 to 2%. In some embodiments, it is further preferred that K2O is not contained.
[0044] MgO can reduce the melting temperature and relative partial dispersion of glass, but when the content of MgO is too high, the anti-devitrification performance and stability of glass decrease. Therefore, the content of MgO is 0-5%, preferably 0-3%, and more preferably 0-2%. In some embodiments, it is further preferred that MgO is not contained.
[0045] CaO helps to improve the density and processing performance of glass, but when the content of CaO is too much, it will make it difficult for the optical constants of the glass to meet the design requirements and the anti-crystallization performance will deteriorate. Therefore, the content of CaO is 0-4%, preferably 0-3%, and more preferably 0-2%. In some embodiments, it is further preferred that CaO is not contained.
[0046] In some embodiments, the ratio (ZnO+CaO+Rn2O) / La2O3 between the total content of ZnO, CaO, and Rn2O and the content of La2O3 is controlled to be below 1.0, which can improve the chemical stability and light transmittance of the glass and prevent the density and abrasiveness from deteriorating. Therefore, it is preferred that (ZnO+CaO+Rn2O) / La2O3 is below 1.0, more preferably (ZnO+CaO+Rn2O) / La2O3 is below 0.8, further preferably (ZnO+CaO+Rn2O) / La2O3 is below 0.5, and further preferably (ZnO+CaO+Rn2O) / La2O3 is below 0.3.
[0047] SrO can improve the devitrification resistance of glass and improve the melting performance of glass, but if its content is too high, the refractive index of glass will be difficult to meet the design requirements, and the cost of glass will also rise rapidly. Therefore, the content of SrO is 2-15%, preferably 3-13%, and more preferably 5.5-11%.
[0048] In some embodiments, the ratio of SrO to La2O3 is controlled within the range of 0.1 to 1.5, which can improve the chemical stability and Young's modulus of the glass and prevent the increase of the thermal expansion coefficient of the glass. Therefore, SrO / La2O3 is preferably 0.1 to 1.5, more preferably 0.2 to 1.2, further preferably 0.3 to 1.0, and further preferably 0.35 to 0.8.
[0049] In some embodiments, by controlling the ratio of the total content of Y2O3, Gd2O3, ZnO, CaO, and Rn2O Y2O3+Gd2O3+ZnO+CaO+Rn2O to the content of SrO (Y2O3+Gd2O3+ZnO+CaO+Rn2O) / SrO to below 1.0, the high temperature viscosity and transition temperature of the glass can be reduced while preventing the hardness from deteriorating. Therefore, it is preferred that (Y2O3+Gd2O3+ZnO+CaO+Rn2O) / SrO is less than 1.0, it is more preferred that (Y2O3+Gd2O3+ZnO+CaO+Rn2O) / SrO is less than 0.8, it is further preferred that (Y2O3+Gd2O3+ZnO+CaO+Rn2O) / SrO is less than 0.5, and it is further preferred that (Y2O3+Gd2O3+ZnO+CaO+Rn2O) / SrO is less than 0.3.
[0050] BaO has the function of adjusting the glass refractive index, improving the glass transmittance and devitrification resistance in the present invention, and can reduce the temperature coefficient of refractive index and thermal expansion coefficient of the glass. If its content is too high, the chemical stability of the glass will be reduced. Therefore, the content of BaO is 12 to 27.5%, preferably 15 to 25%, and more preferably 16 to 23%.
[0051] In some embodiments, the ratio of the total content of La2O3 and SrO La2O3+SrO to the content of BaO (La2O3+SrO) / BaO is controlled within the range of 0.5 to 2.5, which can reduce the thermal expansion coefficient and transition temperature of the glass while preventing the Young's modulus of the glass from decreasing. Therefore, preferably (La2O3+SrO) / BaO is 0.5 to 2.5, more preferably (La2O3+SrO) / BaO is 0.7 to 2.0, further preferably (La2O3+SrO) / BaO is 0.8 to 1.8, and further preferably (La2O3+SrO) / BaO is 0.9 to 1.5.
[0052] TiO2 has the effect of increasing the refractive index of glass and can participate in the formation of glass network. A proper amount of TiO2 can make the glass more stable, but too much content will reduce the light transmittance of the glass and cause obvious coloring of the glass. Therefore, the content of TiO2 in the present invention is 0-5%, preferably 0-3%, and more preferably 0-2%. In some embodiments, it is further preferred that TiO2 is not contained.
[0053] Al2O3 can improve the stability and resistance to devitrification of glass and increase the strength of glass. When its content exceeds 10%, the chemical stability and melting property of glass decrease. Therefore, the content of Al2O3 in the present invention is 0-10%, preferably 1-8%, and more preferably 2-7%.
[0054] In some embodiments, the ratio of Al2O3 content to ZrO2 content, Al2O3 / ZrO2, is controlled within the range of 0.2 to 8.0, which can reduce the high temperature viscosity of the glass while preventing the deterioration of the anti-crystallization performance of the glass. Therefore, Al2O3 / ZrO2 is preferably 0.2 to 8.0, and more preferably Al2O3 / ZrO2 is 0.5 to 6.0. Furthermore, by making Al2O3 / ZrO2 within the range of 0.8 to 4.0, the hardness and abrasiveness of the glass can be further optimized. Therefore, Al2O3 / ZrO2 is further preferably 0.8 to 4.0, and even more preferably Al2O3 / ZrO2 is 1.0 to 2.0.
[0055] In some embodiments, the ratio of Al2O3 to B2O3 is controlled within the range of 0.01 to 0.45, which can reduce the thermal expansion coefficient of the glass while preventing the glass transition temperature from increasing and improving the light transmittance of the glass. Therefore, Al2O3 / B2O3 is preferably 0.01 to 0.45, more preferably 0.05 to 0.4, and further preferably 0.1 to 0.3.
[0056] In some embodiments, the ratio of the total content of BaO and SrO BaO+SrO to the total content of ZrO2 and Al2O3 ZrO2+Al2O3 (BaO+SrO) / (ZrO2+Al2O3) is controlled within the range of 1.0 to 15.0, which can optimize the abrasiveness of the glass while reducing the density of the glass. Therefore, it is preferred that (BaO+SrO) / (ZrO2+Al2O3) is 1.0 to 15.0, and it is more preferred that (BaO+SrO) / (ZrO2+Al2O3) is 1.5 to 10.0. Furthermore, by controlling (BaO+SrO) / (ZrO2+Al2O3) within the range of 2.0 to 8.0, the high temperature viscosity of the glass can be further optimized. Therefore, it is more preferred that (BaO+SrO) / (ZrO2+Al2O3) is 2.0 to 8.0, and it is further preferred that (BaO+SrO) / (ZrO2+Al2O3) is 2.5 to 5.0.
[0057] Ta2O5 has the effect of increasing the refractive index of glass and improving the resistance of glass to devitrification, but if its content is too high, the thermal stability of the glass will decrease and the density will increase; on the other hand, compared with other components, Ta2O5 is very expensive. From the perspective of practicality and cost, its usage should be minimized. Therefore, the content of Ta2O5 in the present invention is limited to 0-5%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that Ta2O5 is not contained.
[0058] P2O5 can improve the devitrification resistance of glass, but if its content is too high, the chemical stability of glass will deteriorate. Therefore, the content of P2O5 is 0 to 4%, preferably 0 to 2%, and more preferably 0 to 1%. In some embodiments, it is further preferred that P2O5 is not contained.
[0059] In the present invention, by containing 0-1% of one or more components of Sb2O3, SnO2, SnO, and CeO2 as clarifiers, the clarification effect of the glass and the bubble degree of the glass can be improved. The preferred content of the clarifier is 0-0.5%, and the more preferred content of the clarifier is 0-0.2%.
[0060] F can be used to adjust the refractive index of glass and reduce the temperature coefficient of refractive index. However, its volatilization during the production process creates environmental load problems. At the same time, it will volatilize from the glass surface in the molding operation temperature range to form an inhomogeneous part, reducing the glass quality and consistency of optical constants. Therefore, the content of F is 0-5%, preferably 0-3%, and more preferably 0-2%. In some embodiments, it is further preferred that F is not contained.
[0061] <Components that should not be contained>
[0062] In the glass of the present invention, even if oxides of transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo are contained alone or in combination in small amounts, the glass will be colored and absorption will occur at specific wavelengths in the visible light region, thereby weakening the property of the present invention of improving the visible light transmittance. Therefore, it is preferred that the glass composition, especially for glass compositions requiring transmittance at wavelengths in the visible light region, substantially contain no oxides of transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo.
[0063] In recent years, the use of oxides of Th, Cd, Tl, Os, Be and Se has tended to be regulated as harmful chemical substances, and environmental protection measures are necessary not only in the manufacturing process of glass, but also in the processing process and the disposal after productization. Therefore, in the case of paying attention to the impact on the environment, it is preferred that they are substantially not contained except for the inevitable mixing. As a result, the glass composition does not substantially contain substances that pollute the environment. Therefore, even without taking special environmental countermeasures, the glass composition of the present invention can be manufactured, processed and discarded.
[0064] In order to achieve environmental friendliness, the glass composition of the present invention preferably does not contain As2O3 and PbO. Although As2O3 has the effect of eliminating bubbles and preventing glass from being colored, the addition of As2O3 will increase the platinum corrosion of the glass on the furnace, especially on the platinum furnace, causing more platinum ions to enter the glass, which has an adverse effect on the service life of the platinum furnace.
[0065] The "does not contain" and "0%" recorded in this article mean that the compound, molecule or element is not intentionally added as a raw material to the glass composition of the present invention; however, as raw materials and / or equipment for producing the glass composition, there may be certain impurities or components that are not intentionally added, which may be contained in a small amount or trace amount in the final glass composition, and this situation is also within the scope of protection of the patent of this invention.
[0066] Next, the properties of the glass composition of the present invention will be described.
[0067] <Refractive Index and Abbe Number>
[0068] The refractive index of the glass composition (n d ) and the Abbe number (νd ) Tested according to the method specified in GB / T 7962.1-2010.
[0069] In some embodiments, the refractive index (n d ) has an upper limit of 1.66, a preferred upper limit of 1.65, and a more preferred upper limit of 1.64.
[0070] In some embodiments, the refractive index (n d ) has a lower limit of 1.59, a preferred lower limit is 1.60, and a more preferred lower limit is 1.61.
[0071] In some embodiments, the Abbe number (ν d ) has an upper limit of 61, a preferred upper limit of 60, and a more preferred upper limit of 59.
[0072] In some embodiments, the Abbe number (ν d ) has a lower limit of 55, a preferred lower limit of 56, and a more preferred lower limit of 57.
[0073] <Transition Temperature>
[0074] The transition temperature (T g ) Tested according to the method specified in GB / T7962.16-2010.
[0075] In some embodiments, the transition temperature (T g ) is 650°C or less, preferably 600 to 650°C, more preferably 605 to 645°C, and further preferably 610 to 640°C.
[0076] <Water resistance stability>
[0077] Water resistance stability of glass composition (D W ) (Powder method) Tested in accordance with the method specified in GB / T 17129.
[0078] In some embodiments, the water resistance stability (D W ) is 3 or more types, preferably 2 or more types, and more preferably 1 type.
[0079] <density>
[0080] The density (ρ) of the glass composition is tested according to the method specified in GB / T7962.20-2010.
[0081] In some embodiments, the density (ρ) of the glass composition of the present invention is 3.60 g / cm 3Below, preferably 3.50g / cm 3 Below, more preferably 3.40g / cm 3 the following.
[0082] <Knoop hardness>
[0083] Knoop hardness of glass composition (H K ) Tested according to the method specified in GB / T7962.18-2010.
[0084] In some embodiments, the Knoop hardness (H) of the glass composition of the present invention is K ) is 500×10 7 Pa or more, preferably 515×10 7 Pa or more, more preferably 530×10 7 Pa or above.
[0085] <Young's modulus>
[0086] The Young's modulus (E) of the glass composition is calculated by ultrasonic testing of its longitudinal wave velocity and transverse wave velocity according to the following formula:
[0087]
[0088] G=V S 2 ρ
[0089] Where: E is Young's modulus, Pa;
[0090] G is the shear modulus, Pa;
[0091] V T is the shear wave velocity, m / s;
[0092] V S is the longitudinal wave velocity, m / s;
[0093] ρ is the glass density, g / cm 3 .
[0094] In some embodiments, the Young's modulus (E) of the glass composition of the present invention is 7000×10 7 Pa or more, preferably 7300×10 7 Pa or more, more preferably 7600×10 7 Pa or above.
[0095] <Abrasion>
[0096] The abrasiveness of the glass composition (F A) refers to the value obtained by multiplying the ratio of the wear volume of the sample to the wear volume (volume) of the standard sample (H-K9 glass) under exactly the same conditions by 100, and is expressed by the following formula:
[0097]
[0098] Where: V—volume wear of the sample being tested;
[0099] V0—Volume loss of standard sample;
[0100] W—mass wear loss of the sample being tested;
[0101] W0—standard sample mass wear;
[0102] ρ—density of the sample being tested;
[0103] ρ0—standard sample density.
[0104] In some embodiments, the abrasiveness (F A ) is 200 or less, preferably 175 or less, and more preferably 150 or less.
[0105] <Coefficient of Thermal Expansion>
[0106] The thermal expansion coefficient of the glass composition (α 20 / 300℃ ) Test data at 20-300℃ according to the method specified in GB / T7962.16-2010.
[0107] In some embodiments, the coefficient of thermal expansion (α 20 / 300℃ ) is 90×10 -7 / K or less, preferably 50×10 -7 / K~85×10 -7 / K, more preferably 55×10 -7 / K~80×10 -7 / K, more preferably 60×10 -7 / K~72×10 -7 / K.
[0108] <Anti-crystallization performance>
[0109] The test method for the anti-crystallization performance of the glass composition is as follows: the sample glass is cut into a size of 20×20×10 mm and placed in a g Keep the glass in a muffle furnace at +200℃ for 60 minutes, take it out and cool it down, and then observe whether there is devitrification or crystal particles on the surface and inside of the glass. If the glass sample has no devitrification and crystal particles, the glass has excellent anti-crystallization performance.
[0110] According to the above test method, glass with no devitrification or crystal grains on the surface and no crystal particles inside is recorded as "A", glass with no crystal grains inside but devitrification or crystal grains on the surface is recorded as "B", glass with 1 to 10 crystal particles inside is recorded as "C", glass with 10 to 20 crystal particles inside is recorded as "D", and glass with more than 20 densely packed crystal particles inside is recorded as "×".
[0111] In some embodiments, the anti-devitrification performance of the glass composition of the present invention is B grade or above, preferably A grade.
[0112] <High temperature viscosity>
[0113] The high temperature viscosity of the glass composition is tested by the following method: using a THETA Rheotronic II high temperature viscometer with a rotation method, the numerical unit is dPaS (poise), the smaller the value, the lower the viscosity.
[0114] In some embodiments, the glass composition of the present invention has a high temperature viscosity at 1200° C. of 60 dPaS or less, preferably a high temperature viscosity at 1200° C. of 40 dPaS or less, and more preferably a high temperature viscosity at 1200° C. of 30 dPaS or less.
[0115] <400~800nm average light transmittance>
[0116] Average light transmittance of glass composition at 400-800nm (τ 400~800nm ) Tested according to the method specified in GB / T7962.12-2010. The higher the average light transmittance at 400-800nm, the smaller the average light transmission loss of the glass composition.
[0117] In some embodiments, the average light transmittance (τ 400~800nm ) is 99.0% or more, preferably 99.5% or more, and more preferably 99.7% or more.
[0118] The thickness of the glass composition is preferably 1 to 12 mm, more preferably 2 to 12 mm, further preferably 5 to 10 mm, and further preferably 2 mm, 5 mm, 8 mm, or 10 mm.
[0119] <400nm light transmittance>
[0120] 400nm light transmittance of glass composition (τ 400nm ) Tested in accordance with the method specified in GB / T 7962.12-2010. The higher the 400nm light transmittance, the lower the blue band light absorption of the glass composition, and the closer the lighting effect is to white light.
[0121] In some embodiments, the 400 nm light transmittance (τ 400nm ) is 99.0% or more, preferably 99.5% or more, and more preferably 99.7% or more.
[0122] The thickness of the glass composition is preferably 1 to 12 mm, more preferably 2 to 12 mm, further preferably 5 to 10 mm, and further preferably 2 mm, 5 mm, 8 mm, or 10 mm.
[0123] [Manufacturing method]
[0124] The manufacturing method of the glass composition of the present invention is as follows: the glass of the present invention is produced using conventional raw materials and processes, including but not limited to using oxides, hydroxides, fluorides, various salts (carbonates, nitrates, sulfates, phosphates, metaphosphates), boric acid, etc. as raw materials, and after mixing according to conventional methods, the prepared furnace materials are put into a melting furnace (such as platinum, gold or platinum alloy crucible) at 1000-1400° C. for melting, and after clarification and homogenization, a homogeneous molten glass without bubbles and undissolved substances is obtained, and the molten glass is cast in a mold and annealed. Those skilled in the art can appropriately select raw materials, process methods and process parameters according to actual needs.
[0125] [Glass preforms and glass elements]
[0126] The glass preform can be produced from the produced glass composition by means of grinding, or by means of press molding such as re-hot pressing, precision stamping, etc. That is, the glass preform can be produced by mechanical processing such as grinding and polishing the glass composition, or by producing a preform for press molding from the glass composition, re-hot pressing the preform and then grinding the preform to produce the glass preform, or by precision stamping the preform produced by grinding.
[0127] It should be noted that the means for preparing a glass preform is not limited to the above means. As described above, the glass composition of the present invention is useful for various glass elements and optical designs, and it is particularly preferred to form a preform from the glass composition of the present invention, and use the preform to perform re-hot press molding, precision stamping molding, etc. to produce glass elements such as lenses and prisms.
[0128] The glass preform and glass element of the present invention are both formed from the glass composition of the present invention. The glass preform of the present invention has the excellent properties of the glass composition; the glass element of the present invention has the excellent properties of the glass composition, and can provide various glass elements such as lenses and prisms with high optical value.
[0129] Examples of the lens include various lenses having spherical or aspherical lens surfaces, such as a concave meniscus lens, a convex meniscus lens, a biconvex lens, a biconcave lens, a plano-convex lens, and a plano-concave lens.
[0130] The glass composition of the present invention can be used to draw glass components such as optical fibers.
[0131] [Optical instruments]
[0132] The glass components formed from the glass composition of the present invention can be used to manufacture optical instruments such as photographic equipment, video equipment, endoscopes, display equipment, and monitoring equipment.
[0133] Example
[0134] <Glass Composition Example>
[0135] In order to further clearly illustrate and describe the technical solution of the present invention, the following non-limiting examples are provided.
[0136] In this embodiment, the above-mentioned method for manufacturing the glass composition is used to obtain a glass composition having the composition shown in Tables 1 to 3. In addition, the properties of each glass are measured by the test method described in the present invention, and the measurement results are shown in Tables 1 to 3. In the following embodiments, the average light transmittance (τ 400~800nm ) and 400nm light transmittance (τ 400nm ) is the test result of glass composition with a thickness of 10 mm.
[0137] Table 1.
[0138]
[0139]
[0140] Table 2.
[0141]
[0142]
[0143]
[0144] Table 3.
[0145]
[0146]
[0147] <Glass Preform Example>
[0148] The glasses obtained from glass composition examples 1 to 24 are used, for example, by grinding processing, or by molding methods such as re-hot pressing, precision stamping, etc., to make preforms of various lenses, prisms, etc., such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses.
[0149] <Glass Element Example>
[0150] The preforms obtained in the above-mentioned glass preform embodiments are annealed to reduce the deformation inside the glass and perform fine adjustments so that the optical properties such as the refractive index reach the desired values.
[0151] Next, each preform is ground and polished to produce various lenses and prisms such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses. The surface of the obtained glass element may be coated with an anti-reflection film.
[0152] <Optical Instrument Embodiment>
[0153] The glass elements made from the above-mentioned glass element embodiments are optically designed to form optical components or optical assemblies using one or more glass elements, and can be used in, for example, imaging equipment, sensors, microscopes, medical technology, digital projection, communications, optical communication technology / information transmission, optics / lighting in the automotive field, photolithography technology, excimer lasers, wafers, computer chips, and integrated circuits and electronic devices including such circuits and chips, or in camera equipment and devices in the automotive field.
Claims
1. A glass composition, characterized in that: Its components, expressed in weight percentage, contain: SiO2: 17-32%; B2O3: 18-32%; BaO: 12-27.5%; SrO: 2-15%; Ln2O3: 7.5-28%, wherein La2O3 / SiO2 is 0.3-1.2, and the Ln2O3 is the total content of La2O3, Gd2O3, Y2O3 and Yb2O3.
2. The glass composition according to claim 1, characterized in that Its components, expressed in weight percentage, also contain: Al2O3: 0-10%; and / or ZrO2: 0-10%; and / or Nb2O5: 0-5%; and / or WO3: 0-5%; and / or ZnO: 0-4.5%; and / or Rn2O: 0-6.5%; and / or MgO: 0-5%; and / or CaO: 0-4%; and / or TiO2: 0-5%; and / or Ta2O5: 0-5%; and / or P2O5: 0-4%; and / or F: 0-5%; and / or clarifier: 0-1%, wherein Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO2, SnO, and CeO2.
3. A glass composition, characterized in that: The components include SiO2, B2O3, BaO, SrO and La2O3, and the components are expressed in weight percentage, wherein La2O3 / SiO2 is 0.3 to 1.2, and the abrasiveness of the glass composition is F A Below 200.
4. The glass composition according to claim 3, characterized in that Its components, expressed in weight percentage, contain: SiO2: 17-32%; and / or B2O3: 18-32%; and / or BaO: 12-27.5%; and / or SrO: 2-15%; and / or Ln2O3: 7.5-28%; and / or Al2O3: 0-10%; and / or ZrO2: 0-10%; and / or Nb2O5: 0-5%; and / or WO3: 0-5%; and / or ZnO: 0-4.5%; and / or Rn2O: 0-6.5%; and / or MgO: 0-5%; and / or CaO: 0-4%; and / or TiO2: 0-5%; and / or Ta2O5: 0-5%; and / or P2O5: 0-4%; and / or F: 0-5%; and / or clarifier: 0-1%, wherein Ln2O3 is the total content of La2O3, Gd2O3, Y2O3, and Yb2O3, Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO2, SnO, and CeO2.
5. The glass composition according to any one of claims 1 to 4, characterized in that , whose components are expressed in weight percentage, wherein: B2O3 / SiO2 is 0.7-1.7, preferably B2O3 / SiO2 is 0.75-1.5, more preferably B2O3 / SiO2 is 0.8-1.3, and further preferably B2O3 / SiO2 is 0.85-1.1; and / or (La2O3+SrO) / BaO is 0.5-2.5, preferably (La2O3+SrO) / BaO is 0.7-2.0, more preferably (La2O3+SrO) / BaO is 0.8-1.8, and further preferably (La2O3+SrO) / BaO is 0.9-1.5; and / or SrO / La2O3 is 0.1-1.5, preferably SrO / La2O3 is 0.2-1.2, More preferably, SrO / La2O3 is 0.3 to 1.0, and further preferably, SrO / La2O3 is 0.35 to 0.8; and / or La2O3 / SiO2 is 0.35 to 1.0, and preferably, La2O3 / SiO2 is 0.4 to 0.9, and more preferably, La2O3 / SiO2 is 0.45 to 0.8; and / or (BaO+SrO) / (ZrO2+Al2O3) is 1.0 to 15.0, and preferably, (BaO+SrO) / (ZrO2+Al2O3) is 1.5 to 10.0, and more preferably, (BaO+SrO) / (ZrO2+Al2O3) is 2.0 to 8.0, and further preferably, (BaO+SrO) / (ZrO2+Al2O3) is 2.5 to 5.
0.
6. The glass composition according to any one of claims 1 to 4, characterized in that , the components are expressed in weight percentage, wherein: Al2O3 / B2O3 is 0.01-0.45, preferably Al2O3 / B2O3 is 0.05-0.4, more preferably Al2O3 / B2O3 is 0.1-0.3; and / or ZrO2 / SiO2 is 0.01-0.4, preferably ZrO2 / SiO2 is 0.05-0.35, more preferably ZrO2 / SiO2 is 0.1-0.3; and / or Al2O3 / ZrO2 is 0.2-8.0, preferably Al2O3 / ZrO2 is 0.5-6.0, more preferably Al2O3 / ZrO2 is 0.8-4.0, further preferably Al2O3 / ZrO2 is 1.0-2.0; and / or (Y2O3+Gd2O3+ZnO+CaO+Rn2O) / SrO is 1. 0 or less, preferably (Y2O3+Gd2O3+ZnO+CaO+Rn2O) / SrO is 0.8 or less, more preferably (Y2O3+Gd2O3+ZnO+CaO+Rn2O) / SrO is 0.5 or less, and further preferably (Y2O3+Gd2O3+ZnO+CaO+Rn2O) / SrO is 0.3 or less; and / or (ZnO+CaO+Rn2O) / La2O3 is 1.0 or less, preferably (ZnO+CaO+Rn2O) / La2O3 is 0.8 or less, more preferably (ZnO+CaO+Rn2O) / La2O3 is 0.5 or less, and further preferably (ZnO+CaO+Rn2O) / La2O3 is 0.3 or less, and the Rn2O is one or more of Li2O, Na2O, and K2O.
7. The glass composition according to any one of claims 1 to 4, characterized in that , the components are expressed in weight percentage, wherein: SiO2: 21-30%, preferably SiO2: 22-28%; and / or B2O3: 21-30%, preferably B2O3: 22-29%; and / or Ln2O3: 10-25%, preferably Ln2O3: 11-20%; and / or BaO: 15-25%, preferably BaO: 16-23%; and / or SrO: 3-13%, preferably SrO: 5.5-11%; and / or Al2O3: 1 ~8%, preferably Al2O3: 2~7%; and / or ZrO2: 0.5~8%, preferably ZrO2: 1~7%; and / or Nb2O5: 0~3%, preferably Nb2O5: 0~1%, more preferably no Nb2O5; and / or WO3: 0~3%, preferably WO3: 0~1%, more preferably no WO3; and / or ZnO: 0~3%, preferably ZnO: 0~2%, more preferably no ZnO; and / or Rn2O: 0~5%, preferably Rn 2O: 0-2%; and / or MgO: 0-3%, preferably MgO: 0-2%, more preferably no MgO; and / or CaO: 0-3%, preferably CaO: 0-2%, more preferably no CaO; and / or TiO2: 0-3%, preferably TiO2: 0-2%, more preferably no TiO2; and / or Ta2O5: 0-3%, preferably Ta2O5: 0-1%, more preferably no Ta2O5; and / or P2O5: 0-2%, preferably P2 O5: 0-1%, more preferably no P2O5; and / or F: 0-3%, preferably F: 0-2%, more preferably no F; and / or clarifier: 0-0.5%, preferably clarifier: 0-0.2%, the Ln2O3 is the total content of La2O3, Gd2O3, Y2O3, and Yb2O3, Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO2, SnO, and CeO2.
8. The glass composition according to any one of claims 1 to 4, characterized in that , the components are expressed in weight percentage, wherein: La2O3: 7.5-23%, preferably La2O3: 11-20%, more preferably La2O3: 12-18%; and / or Gd2O3: 0-8%, preferably Gd2O3: 0-5%, more preferably Gd2O3: 0-1.5%, further preferably no Gd2O3; and / or Y2O3: 0-8%, preferably Y2O3: 0-5%, more preferably Y2O3: 0-1.5%, further preferably no Y2O3; and / or Yb2O3: 0 ~5%, preferably Yb2O3: 0~3%, more preferably Yb2O3: 0~2%, further preferably contains no Yb2O3; and / or Li2O: 0~5%, preferably Li2O: 0~3%, more preferably Li2O: 0~2%; and / or Na2O: 0~5%, preferably Na2O: 0~3%, more preferably Na2O: 0~2%, further preferably contains no Na2O; and / or K2O: 0~5%, preferably K2O: 0~3%, more preferably K2O: 0~2%, further preferably contains no K2O.
9. The glass composition according to any one of claims 1 to 4, characterized in that , Average light transmittance τ of glass composite with thickness below 12mm at 400~800nm 400~800nm 99.0% or more, preferably 99.5% or more, more preferably 99.7% or more; and / or the 400nm light transmittance τ of the glass composition with a thickness of 12 mm or less 400nm It is 99.0% or more, preferably 99.5% or more, and more preferably 99.7% or more.
10. The glass composition according to claim 9, characterized in that The thickness of the glass composition is 1 to 12 mm, preferably 2 to 12 mm, more preferably 5 to 10 mm, and further preferably 2 mm, 5 mm, 8 mm or 10 mm.
11. The glass composition according to any one of claims 1 to 4, characterized in that , the refractive index n of the glass composition d 1.59 to 1.66, preferably 1.60 to 1.65, more preferably 1.61 to 1.64; and / or Abbe number ν d 55 to 61, preferably 56 to 60, more preferably 57 to 59; and / or transition temperature T g 650°C or less, preferably 600-650°C, more preferably 605-645°C, and further preferably 610-640°C; and / or water resistance stability D W 3 or more, preferably 2 or more, more preferably 1; and / or density ρ is 3.60 g / cm 3 Below, preferably 3.50g / cm 3 Below, more preferably 3.40g / cm 3 Below; and / or Knoop hardness H K 500×10 7 Pa or more, preferably 515×10 7 Pa or more, more preferably 530×10 7 Pa or more; and / or Young's modulus E is 7000×10 7 Pa or more, preferably 7300×10 7 Pa or more, more preferably 7600×10 7 Pa or above; and / or wear degree F A 200 or less, preferably 175 or less, more preferably 150 or less; and / or thermal expansion coefficient α 20 / 300℃ 90×10 -7 / K or less, preferably 50×10 -7 / K~85×10 -7 / K, more preferably 55×10 -7 / K~80×10 -7 / K, more preferably 60×10 -7 / K~72×10 -7 / K; and / or a high temperature viscosity of 60 dPaS or less at 1200°C, preferably 40 dPaS or less, more preferably 30 dPaS or less; and / or an anti-crystallization performance of B grade or above, preferably A grade.
12. A glass preform, characterized in that , made of the glass composition described in any one of claims 1 to 11.
13. A glass element, characterized in that , made of the glass composition according to any one of claims 1 to 11 or the glass preform according to claim 12.
14. An optical instrument, characterized in that , containing the glass composition according to any one of claims 1 to 11, or containing the glass element according to claim 13.
Citation Information
Patent Citations
Optical glass and core material for optical fiber
CN103466936A
Super wear-resistant glazed brick glaze, preparation method thereof, glazed brick and preparation method thereof
CN115385575A
Optical glass
CN102311228A
Optical glass having negative anomalous dispensability
JP1998265238A
Electric motor driver, compressor drive device, and compressor
JP2009044873A