Plant asphalt matrix asphalt mixture and application thereof in semi-flexible pavement

By using a mixture of plant asphalt made of bioheavy oil, magnesium sulfate and magnesium oxide, combined with basalt and other stones, an excellent plant asphalt matrix asphalt mixture was prepared, and the adhesion of plant asphalt was solved by infusion of cement grouting materials. The limitations of this paper realize efficient and environmentally friendly semi-flexible pavement material preparation, with excellent road performance and environmental protection advantages.

CN119019116APending Publication Date: 2024-11-26湖南博研新材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411121365.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, plant asphalt has limitations in key properties such as adhesion, and it is difficult to completely replace petroleum asphalt. The hot mixing process leads to high energy consumption and high pollution. How to find a type of petroleum asphalt that has both the properties of petroleum asphalt and comes from renewable Alternative materials for resources have become a challenge in the field of road engineering.

Method used

Using a mixture of plant asphalt made of bioheavy oil and magnesium sulfate and magnesium oxide as a curing agent, combined with basalt and other stones, a plant asphalt matrix asphalt mixture with excellent mechanical strength and fluidity is prepared, and the filling of cement grouting material is carried out. , forming semi-flexible pavement materials.

Benefits of technology

Achieve a construction process without heating, reduces energy consumption and pollution emissions, improves the environmental protection properties and road performance of road materials, has good high temperature stability, water stability and anti-slip performance, high dynamic stability and residual stability The ratio of freeze-thaw splitting strength exceeds 84%, which promotes the sustainable development of the highway industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019116A_ABST
    Figure CN119019116A_ABST
Patent Text Reader

Abstract

The invention relates to a plant asphalt matrix asphalt mixture and application of the plant asphalt matrix asphalt mixture in a semi-flexible pavement. According to the invention, the plant asphalt is adopted as a cementing material, the coarse aggregate, the fine aggregate, the mineral powder and the curing agent in a proper ratio are added to prepare a large-gap matrix asphalt mixture, and the cement-based slurry is poured to realize effective combination with the plant asphalt matrix asphalt mixture, so that the innovative semi-flexible pavement material is formed. In the construction process, the plant asphalt matrix asphalt mixture does not need heating equipment, plant asphalt prepared from biological heavy oil is completely used, the plant asphalt matrix asphalt mixture has remarkable advantages in the aspects of reducing environmental pollution, reducing energy consumption and the like, and meanwhile, high efficiency and convenience of construction are achieved; the transformation of high-efficiency, energy-saving, durable and green development of the highway industry is promoted, and the application range of the plant asphalt is expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a plant asphalt matrix asphalt mixture and application thereof in a semi-flexible pavement, belonging to the technical field of pavement materials. Background Art

[0002] Common pavement forms are mainly divided into asphalt concrete pavement and cement concrete pavement. Due to the temperature sensitivity of asphalt materials, under the action of driving loads in high temperature environments in summer, asphalt pavements may undergo structural deformation due to reduced cohesion, resulting in permanent pavement diseases such as rutting and shifting. In contrast, although cement concrete pavements have a higher modulus, the problems they bring cannot be ignored. The high modulus of cement pavements leads to large rebound bumps, and the load, temperature, and dry and wet deformations are more significant. In addition, due to the large number of joints between the plates, the joints are very prone to damage, which not only increases the complexity of construction, but also affects the driving comfort in later use. In the face of the advantages and limitations of asphalt pavements and cement pavements, after the collective efforts and unremitting research of scientific researchers, a new pavement structure called semi-flexible pavement has been developed; semi-flexible pavement refers to a pavement structure formed by pouring cement slurry into a base asphalt mixture with a void ratio of 20%-28%. This pavement form effectively combines the flexibility of asphalt pavement and the rigidity of cement pavement, thus having the advantages of good high temperature stability and water stability. However, hot-mix petroleum asphalt mixture is usually used as the base material in its semi-flexible asphalt pavement, which has disadvantages such as high energy consumption, heavy pollution, and construction is restricted by climatic conditions.

[0003] At present, with the frequent development of road maintenance and construction activities, the demand for petroleum asphalt continues to rise. However, this demand growth trend is in sharp contrast to the current situation of global crude oil resources decreasing year by year. This series of factors together limit the supply of asphalt products in the downstream of the oil industry chain, posing a potential constraint on road infrastructure construction. Therefore, finding an alternative material with similar properties to petroleum asphalt and derived from renewable resources has become an urgent problem to be solved in the field of road engineering.

[0004] Due to the limitations of plant asphalt in key properties such as adhesion, plant asphalt made from bio-heavy oil is in a liquid state at room temperature and lacks the necessary mechanical strength. In particular, when the replacement ratio of plant asphalt is too high, it may have an adverse effect on the safety of road paving materials. Therefore, although the research progress of plant asphalt has brought hope for the sustainability and environmental friendliness of future road construction materials, it is still a challenge to completely replace petroleum asphalt. Finding a method to completely use plant asphalt as a road material has become an important research direction in the academic community. In the field of road construction, in order to meet the viscosity requirements of asphalt in construction, it needs to be heated to a higher temperature. This process inevitably leads to a series of problems, such as high energy consumption, large pollutant emissions, and complexity of the construction process. These problems are becoming more and more prominent in the production and application of petroleum asphalt, posing a major challenge to environmental sustainable development. As an alternative material to petroleum asphalt, plant asphalt is in a liquid state at room temperature, which means that it does not need to be heated during the construction process, thereby directly avoiding the high energy consumption and high pollution emissions faced by traditional hot mix asphalt. In addition, due to its similar chemical composition to petroleum asphalt, plant asphalt exhibits performance characteristics comparable to petroleum asphalt. However, in the prior art, only a small amount of plant asphalt is mixed into petroleum asphalt to partially replace petroleum asphalt. To achieve the goal of completely replacing petroleum asphalt with plant asphalt, there are still challenges. This is mainly due to the limitations of plant asphalt in key properties such as adhesion. Under normal temperature conditions, plant asphalt made from bio-heavy oil is in a liquid state and lacks the necessary mechanical strength. Especially when the replacement ratio of plant asphalt is too high, it may have an adverse effect on the safety of road paving materials. Therefore, although the research progress of plant asphalt has brought hope for the sustainability and environmental friendliness of future road construction materials, it is still a challenge to completely replace petroleum asphalt. Finding a method that can completely use plant asphalt as a road material has become an important research direction in the academic community.

[0005] Different types of asphalt binders have different effects on the base asphalt mixture, thereby affecting the water stability and high-temperature performance of semi-flexible pavement materials, especially the low-temperature crack resistance. How to overcome this problem is also a technical problem that semi-flexible pavement materials urgently need to solve. Summary of the invention

[0006] 1. Technical issues to be resolved

[0007] In order to solve the above problems in the prior art, the present invention provides a plant asphalt matrix asphalt mixture and its application in a semi-flexible pavement. The present invention also provides a plant asphalt semi-flexible pavement material for preparing a semi-flexible pavement.

[0008] (II) Technical solution

[0009] In order to achieve the above object, the main technical solutions adopted by the present invention include:

[0010] In a first aspect, the present invention provides a plant asphalt mortar for road materials, which includes plant asphalt and a curing agent, wherein the curing agent is a mixture of magnesium sulfate and magnesium oxide in a mass ratio of 1:2-3 (preferably 1:2.5), and the curing agent is added in an amount of 15-25% of the mass of the plant asphalt; the plant asphalt is a dark brown liquid made from biological heavy oil, which does not contain petroleum asphalt. Most preferably, the curing agent is added in an amount of 20%. Preferably, the curing agent is a mixture of magnesium sulfate and magnesium oxide in a mass ratio of 1:2.5

[0011] In a second aspect, the present invention further provides a plant asphalt-based asphalt mixture, which includes the above-mentioned plant asphalt mortar and stone, wherein the stone is composed of coarse aggregate, fine aggregate and mineral powder.

[0012] Furthermore, the coarse aggregate and the fine aggregate are basalt, and the mineral powder is lime powder mineral powder.

[0013] Preferably, in the stone, the mass proportion of coarse aggregate is 82.3%-89.1%, the mass proportion of fine aggregate is 14.7%-7.9% and the mass proportion of mineral powder is 3%; the amount of vegetable asphalt is 3%-5% of the total mass of the stone.

[0014] Furthermore, the void ratio of the plant asphalt matrix asphalt mixture is 20-28%.

[0015] Furthermore, when the void ratio of the plant asphalt-based asphalt mixture is 20%, the coarse aggregate in the stone accounts for 84.2%, the fine aggregate accounts for 14.7% and the mineral powder accounts for 3%; the amount of plant asphalt used is 4.4%-4.6% of the mass of the stone, and the amount of curing agent used is 20% of the mass of the plant asphalt;

[0016] When the void ratio of the plant asphalt-based asphalt mixture is 23%, the coarse aggregate in the stone accounts for 84.9%, the fine aggregate accounts for 12.1% and the mineral powder accounts for 3%; the amount of plant asphalt used is 4.1%-4.3% of the mass of the stone, and the amount of curing agent used is 20% of the mass of the plant asphalt;

[0017] When the void ratio of the plant asphalt-based asphalt mixture is 25%, the coarse aggregate in the stone accounts for 86.1%, the fine aggregate accounts for 14.7% and the mineral powder accounts for 3%; the amount of plant asphalt used is 3.7%-3.9% of the mass of the stone, and the amount of curing agent used is 20% of the mass of the plant asphalt;

[0018] When the void ratio of the plant asphalt-based asphalt mixture is 28%, the coarse aggregate in the stone accounts for 89.1%, the fine aggregate accounts for 7.9% and the mineral powder accounts for 3%; the amount of plant asphalt used is 3.4%-3.6% of the stone mass, and the amount of curing agent used is 20% of the plant asphalt mass.

[0019] A plant asphalt semi-flexible pavement material comprises the plant asphalt matrix asphalt mixture as described above and cement grouting material, wherein the cement grouting material comprises cement, modifier, silica fume, mineral powder, sand and water reducing agent; preferably, the cement is P·O42.5 silicate cement, the modifier is styrene-butadiene rubber emulsion, the water reducing agent is polycarboxylic acid water reducing agent, and the mineral powder is limestone mineral powder.

[0020] As the plant asphalt semi-flexible pavement material described above, preferably, the modifier is 5-15% of the cementitious material, silica fume is 3-8% of the mass of cement, mineral powder is 5-15% of the cementitious material, sand is 10-20% of the cementitious material, and the water reducer is 0.3-1% of the mass of cement, wherein the cementitious material refers to silica fume and cement.

[0021] Furthermore, optimally, the modifier is 10% of the cementitious material, silica fume is 5% of the cement mass, mineral powder is 10% of the cementitious material, sand is 15% of the cementitious material, and the water reducer is 0.5% of the cement mass. Under this condition, the cement paste has good fluidity and mechanical properties under the optimal ratio, with a fluidity of 12.3s, a 7-day flexural strength and a compressive strength of 3.7MPa and 24.6MPa, respectively, and a 28-day flexural strength and a compressive strength of 5.8MPa and 38.6MPa, respectively.

[0022] As for the above-mentioned vegetable asphalt semi-flexible pavement material, preferably, when in use, water is added to the cement grouting material in an amount of 50-60% of the mass of the cementitious material. Further, preferably, water is added to the cement grouting material in an amount of 55% of the mass of the cementitious material.

[0023] The use of the plant asphalt-based asphalt mixture and the plant asphalt semi-flexible pavement material as described above in the preparation of semi-flexible pavement.

[0024] (III) Beneficial effects

[0025] The beneficial effects of the present invention are:

[0026] The plant asphalt mortar for road materials provided by the present invention is used as a substitute for petroleum asphalt, providing strong support for the sustainable development of transportation infrastructure construction. By introducing renewable resources, it not only improves the environmental protection properties of road materials, but also realizes the harmonious unity of effective resource utilization and environmental protection goals in road engineering practice.

[0027] The present invention adopts plant asphalt as a binder material to prepare a base asphalt mixture with large voids, and realizes effective combination with the plant asphalt base asphalt mixture by pouring cement-based slurry, thereby forming an innovative semi-flexible pavement material.

[0028] The present invention provides a gradation composition of a plant asphalt matrix asphalt mixture at four different target void ratios of 20%, 23%, 25% and 28%. The optimal asphalt dosage of the plant asphalt matrix asphalt mixture at each void ratio is determined by the Schellenberg leakage test and the Kentenberg dispersion test (4.5%, 4.2%, 3.8% and 3.5%). In addition, the injection rate of cement slurry into the plant asphalt matrix asphalt mixture is used as an evaluation index, and the injection rate of the slurry is determined to be above 88%, ensuring good injection performance. The road performance of plant asphalt semi-flexible pavement materials with different target void ratios is studied. The results show that the mixture has good high temperature stability, water stability and anti-skid performance, the dynamic stability exceeds 13,000 times / mm, the residual stability is not less than 94%, the freeze-thaw splitting strength ratio exceeds 84%, and the swing value exceeds 80. The mixture has good low-temperature crack resistance, and the maximum bending and tensile strain reaches 2134.50με.

[0029] The plant asphalt semi-flexible pavement material provided by the present invention combines the flexibility of plant asphalt-based materials with the rigidity advantages of cement-based materials to form a new type of pavement material with excellent road performance. No heating equipment is required during the construction process, and plant asphalt made entirely from bio-heavy oil is used, thereby showing significant advantages in reducing environmental pollution and energy consumption, while achieving high efficiency and convenience in construction. By using such environmentally friendly materials, it not only has excellent road performance, but also promotes the transformation of the highway industry to high efficiency, energy saving, durability and green development, expands the application scope of plant asphalt, and provides a relatively important theoretical basis and practical guide for future research in the road field. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is the penetration index result of the cured vegetable asphalt;

[0031] Figure 2 It is the result of the ductility index of the cured vegetable asphalt (5℃ water bath);

[0032] Figure 3 It is the softening point index result of the solidified plant asphalt;

[0033] Figure 4 This is the infrared spectrum test result of plant asphalt;

[0034] Figure 5 This is the infrared spectrum test result of cured plant asphalt;

[0035] Figure 6 It is the result between the complex shear modulus G* of plant asphalt and the temperature change;

[0036] Figure 7 It is the result between the phase angle (δ) of plant asphalt and the temperature change;

[0037] Figure 8 It is the result between the rutting factor (G* / sinδ) of plant asphalt and the temperature change;

[0038] Fig. 9 It is the result of the creep stiffness modulus of plant asphalt and temperature change;

[0039] Fig.10 is the result of creep rate and temperature change;

[0040] Fig.11 This is a test picture of the cured vegetable asphalt magnified 5000 times by scanning electron microscope;

[0041] Fig.12 This is a test picture of the cured vegetable asphalt magnified 10,000 times by scanning electron microscope;

[0042] Fig.13 TG curve and DTG curve of the solidified vegetable asphalt;

[0043] Fig.14 Marshall specimens of vegetable asphalt matrix asphalt mixture before and after cement paste pouring;

[0044] Fig.15 The rutting specimens of the plant asphalt matrix asphalt mixture before and after cement paste pouring;

[0045] Fig.16 The specimens of the plant asphalt matrix asphalt mixture beam before and after cement paste pouring;

[0046] Fig.17 It is the deformation curve of rutting depth. DETAILED DESCRIPTION

[0047] The present invention provides a plant asphalt-based asphalt mixture, in which an inorganic active powder curing agent is used as the raw material, which can undergo complex physical and chemical reactions with the plant asphalt, thereby forming a gelled network structure of the plant asphalt and achieving the curing of the plant asphalt.

[0048] The coarse and fine aggregates used in the present invention are both basalt. Studies have found that due to its high content of alkaline chemical components, basalt can produce a good reaction when mixed with acidic plant asphalt and can show better performance. The advantage of choosing this material is that its chemical properties can effectively react with plant asphalt, thereby improving the overall performance of the mixture. Fine aggregate is mainly used to fill the gaps in the skeleton structure.

[0049] As the largest particle size component in the grouting material of the plant asphalt semi-flexible pavement material, sand has significant particle size characteristics and has a significant impact on the smoothness of the grouting operation. Fineness modulus, as a key parameter to measure the particle size distribution and particle grading of sand particles, plays a decisive role in the suspension stability of sand in the slurry and the segregation performance of mortar. The segregation of mortar is directly related to whether it can be evenly and effectively filled into the voids inside the plant asphalt matrix asphalt mixture, thereby ensuring the ideal grouting effect.

[0050] The main function of the water reducer is to generate sufficient repulsive force between particles, thereby achieving effective dispersion of the particles. This dispersion effect not only reduces the agglomeration of particles, thereby significantly improving the fluidity of the cement paste and optimizing its overall working performance, but the polycarboxylic acid water reducer used in the present invention can effectively improve the rheological properties of cement-based materials and enhance their strength and durability. In the present invention, 5% silica fume is used to replace cement. Silica fume can reduce the yield stress and viscosity of cement-based materials. The reduction in yield stress means that cement-based materials are easier to flow and deform when subjected to external forces, while the reduction in viscosity improves the fluidity and processability of cement-based materials, thereby improving the working performance of cement paste; the use of silica fume is of great significance for improving the construction performance, mechanical properties and durability of materials.

[0051] The study found that the selection of styrene-butadiene rubber latex as a modifier can effectively improve the low-temperature crack resistance of cement grouting materials and the bonding performance of the interface between cement paste and plant asphalt matrix mixture; it can also effectively enhance the interfacial bonding between cement mortar and plant asphalt mixture, and can effectively improve the overall performance and durability of the composite material. At the same time, by adjusting the dosage of styrene-butadiene rubber latex, the comprehensive performance of the grouting material can be further optimized to meet the needs of specific engineering applications.

[0052] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below in conjunction with the accompanying drawings through specific embodiments. The plant asphalt used in the following examples is a Class A liquid plant asphalt (excluding petroleum asphalt) made from bio-heavy oil by Hunan Boyan New Materials Co., Ltd., and its performance indicators are density 0.9g / mL, higher fatty acid content 79.1%, phytosterol content 9.1%, volatile organic matter VOCs (2.28%), moisture (0.4%), and acid value 46.1. The curing agent is a mixture of anhydrous magnesium sulfate and magnesium oxide in a mass ratio of 1:2-3, and the particle size distribution of the inorganic active powder curing agent is D90=40.10μm, D50=9.86μm, and D10=0.60μm. Both coarse and fine aggregates are basalt. Stones with a particle size of more than 2.36 mm are classified as coarse aggregates, while stones with a particle size equal to and less than 2.36 mm are considered fine aggregates. According to the test of "JTG E42-2005 Highway Engineering Aggregate Test Procedures", the basic physical performance indicators of basalt coarse aggregate are water absorption of 0.9%, firmness of 6%, stone crushing value of 15.6%, Los Angeles abrasion loss of 12.5%, and content of slender flat particles of 5.2%, which meet the technical standards for expressways and first-class highways; the fine aggregate is basalt fine aggregate. After testing, the performance indicators are sand equivalent of 69.1%, firmness of 16%, methylene blue value of 1.9g / kg, and angularity of 37s, which meet the technical standards for expressways and first-class highways. The performance of the selected limestone powder was tested according to the "JTG E42-2005 Highway Engineering Aggregate Test Procedure". The results showed that the water content was 0.39%, the particle size range <0.15mm was 95.4%, the particle size range <0.075mm was 87.4%, the hydrophilic coefficient was 0.733, and the plasticity index was 3, which met the technical standards for expressways and first-class highways. P·O 42.5 silicate cement came from Tuoda New Materials Technology Industry Group Co., Ltd.; the performance indicators of the sand used were tested in accordance with the "JGJ 52-2006 Standard for the Quality and Inspection Methods of Sand and Stone for Ordinary Concrete". The results showed that the firmness was 3%, the mud content was 0.4%, the water absorption rate was 1.8%, and the apparent density was 2.62g / cm 3 .

[0053] The polycarboxylate water reducer comes from Shandong Jinrong Chemical Technology Co., Ltd., and the silica fume comes from Hebei Zhengyu New Material Technology Co., Ltd. The basic mineral composition of silica fume is SiO2 90.26%, Na2O 0.86%, MgO 0.64%, Al2O3 0.32%, Fe2O3 0.08% and CaO 1.03%; the technical indicators of styrene-butadiene rubber latex are relative density (20°C) of 0.978, Ph (25°C) of 5.2, flash point of 145°C, surface tension of 65-75 (mN·m -1 ), viscosity (20℃) is 35-45 (mPa·s) and solid content is 66-67%.

[0054] Example 1

[0055] In order to determine the optimal dosage of the curing agent, which is a mixture of anhydrous magnesium sulfate and magnesium oxide in a mass ratio of 1:2.5, this experiment added five different mass ratios of curing agent, namely 10%, 15%, 20%, 25% and 30%, to the vegetable asphalt. The mixing process of vegetable asphalt and curing agent was carried out at room temperature using a JRJ300-S high-speed shear instrument. The shear process lasted for about 3 minutes, and the shear rate was controlled at 300 rpm. After the high-speed shearing was completed, the specimens were properly cured. Subsequently, a series of performance tests were carried out on these cured vegetable asphalt specimens to evaluate the effects of different dosages of curing agent on the performance of vegetable asphalt, so as to select the optimal curing agent dosage. According to the T0604, T0605 and T0606 operating steps in the "JTG E20-2011 Highway Engineering Asphalt and Asphalt Mixture Test Procedures", the cured vegetable asphalt specimens were tested respectively. Specifically: According to T0604, the cooled sample was placed in a constant temperature water tank at the specified test temperature for 1.5 hours, and then the needle penetration instrument was adjusted so that the needle tip was in contact with the sample surface, and then the standard needle was allowed to fall freely for penetration test. After the needle fell freely for 5 seconds, the reading was immediately recorded; the obtained needle penetration test results are as follows: Figure 1 As shown. According to T0605, first inject the asphalt sample into the mold, then use a hot scraper to scrape off the excess asphalt from the fully cooled specimen at room temperature, put the treated specimen into a water tank for 1.5 hours, start the ductility tester for testing, and record the relevant data; the ductility test results are as follows: Figure 2 As shown. According to T0606, the ring and ball method is used to measure the softening point of asphalt. The treated specimen is placed in a constant temperature water tank at 5°C for 15 minutes. At the same time, the pure water in the beaker is cooled to 5°C. The specimen is placed in the round hole of the beaker bracket and a positioning ring is put on. The beaker is heated. When the specimen softens and begins to fall until it contacts the bottom, the temperature at this time is immediately and accurately read. The softening point test result is as follows: Figure 3 shown.

[0056] As can be seen from the figure, the curing agent dosage is between 10% and 30%. As the dosage increases, the decrease in the penetration data gradually slows down and reaches the minimum when the dosage is 30%. This trend shows that the increase in curing agent effectively improves the consistency of plant asphalt, making it more resistant to stress or penetration. It can be seen that the high temperature performance of plant asphalt gradually improves with the increase in curing agent dosage. In addition, the ductility data of the specimens showed an increasing trend in the initial stage of the increase in curing agent dosage, but when the dosage reached a certain level, the ductility data began to gradually decrease. It is also worth noting that when the curing agent dosage is about 20%, the ductility data reaches its maximum value, and the low temperature performance of plant asphalt also reaches the best. The softening point data of the plant asphalt specimens show a gradually slowing upward trend with the increase in curing agent dosage, which is similar to the trend of the gradual decrease in penetration. The data reaches the maximum when the dosage is 30%. Both reflect the influence of curing agent dosage on the high temperature performance of plant asphalt, and also fully prove that the addition of curing agent helps to improve the high temperature performance of plant asphalt. The curing agent effectively improves the performance of asphalt by reacting with the molecules and groups in the plant asphalt. When the liquid molecules in the plant asphalt interact with the solid molecules of the inorganic active powder curing agent, the liquid molecules tend to adsorb on the surface of the solid molecules to form a stable interface layer, while maintaining a dynamic balance with the molecules inside the liquid. This interfacial effect not only enhances the binding force between the curing agent and the asphalt, but also promotes the chemical reaction between the two. When the curing agent is mixed with the plant asphalt, the active ingredients in the curing agent react chemically with functional groups such as carboxylic acids in the asphalt to form new chemical bonds. The formation of these chemical bonds not only enhances the interaction between asphalt molecules, but also increases the cross-linking density of the asphalt, making the asphalt harder and more stable, further improving the overall performance of the mixture.

[0057] The results of the external spectrum test of the vegetable asphalt before and after adding the curing agent using Nicolet iS50 infrared spectrometer show that Figure 4 and Figure 5 As shown in the figure, the results show that there are 10 obvious absorption peaks in the cured plant asphalt. Compared with the infrared test results of the original plant asphalt, it can be found that the absorption spectrum is basically similar, among which 1707.20cm -1 The transmittance of the absorption peak at 1563.10cm is greatly reduced, and the transmittance of other absorption peaks also changes. A new absorption peak appears at 1563.10cm -1 The absorption peaks at 1112.45 cm-1 are caused by the C=C stretching vibration on the benzene ring skeleton. -1The absorption peak caused by the ring vibration of cyclopropane verifies the chemical reaction between the plant asphalt and the curing agent. The organic macromolecules in the plant asphalt react well with the inorganic active powder curing agent elements. After curing, the C=C of the two molecules combined forms a strong absorption peak, forming a new olefin organic compound.

[0058] According to the US Strategic Highway Research Program (SHRP), the effects of temperature and load were considered comprehensively, and the dynamic shear rheology test was used to evaluate the high temperature rheological properties of asphalt. The test results were also used to determine the optimal curing agent dosage. The results are as follows: Figure 6 , Figure 7 and Figure 8 .

[0059] Complex shear modulus (G*) is an important indicator for evaluating the ability of cured vegetable asphalt to resist deformation under repeated shear force. Figure 6 From the test data of the relationship between the change in G* of plant asphalt with different curing agent dosages and temperature, it was observed that as the test temperature increased, the shear modulus of plant asphalt with different curing agent dosages gradually decreased. In addition, by comparing the aged plant asphalt with the unaged original plant asphalt, it can be clearly seen that the shear modulus of the aged plant asphalt is higher. During the aging process, the molecular structure inside the plant asphalt may have been rearranged or cross-linked, resulting in an increase in its hardness. Figure 6 It can be seen from the data that the complex shear modulus of the plant asphalt with the addition of inorganic active powder curing agent is higher, indicating that it has a stronger ability to resist external deformation. This phenomenon is mainly attributed to the modification effect of the inorganic active powder curing agent, which significantly improves the modulus of the plant asphalt. Further comparison of the test results of plant asphalt with different amounts of curing agent shows that under the same temperature conditions, with the increase of the curing agent dosage, both the original plant asphalt and the aged plant asphalt, their complex shear modulus show different degrees of improvement. This observation shows that the addition of inorganic active powder curing agent can improve the shear deformation resistance of plant asphalt to a certain extent, which is of great significance for improving the performance of plant asphalt.

[0060] The phase angle (δ) value directly reflects the strength of the recovery ability of vegetable asphalt after deformation under high temperature conditions. Figure 7The changes in the δ value of plant asphalt with different curing agent dosages in the experiment showed that with the increase of temperature, the δ value of both the original plant asphalt and the aged plant asphalt showed a trend of gradual increase. This shows that plant asphalt tends to be more viscous under high temperature conditions. It is worth noting that at the same temperature, the δ value of the aged plant asphalt is generally smaller than that of the original asphalt. It can be seen that the aging process increases the elastic components in the plant asphalt. In addition, the experiment also found that under the same temperature conditions, the addition of curing agent has a significant effect on the δ value of plant asphalt, and this effect becomes more significant with the increase of curing agent dosage. This phenomenon may be due to the fact that the increase in temperature promotes the reaction between plant asphalt and inorganic active powder curing agent, which increases the viscosity of plant asphalt by physically or chemically combining with the adhesive substances in the asphalt. Therefore, these observations show that the addition of inorganic active powder curing agent can significantly improve the elastic properties of plant asphalt, which is of great significance for improving its performance at high temperatures.

[0061] By analyzing Figure 8 From the data of the aged plant asphalt, it was observed that the G* / sinδ value of the aged plant asphalt was higher than that of the unaged original plant asphalt. This result indicates that the aging process improves the high-temperature rutting resistance of the plant asphalt mixture. Under high temperature conditions, road materials are often prone to softening and deformation, leading to rutting and other problems. The aged plant asphalt can better resist these adverse factors and maintain the flatness and stability of the road due to its excellent high-temperature rutting resistance. Further analysis shows that in the two sets of data, with the increase of the amount of inorganic active powder curing agent, the G* / sinδ value shows an upward trend. This means that the more the curing agent is added, the shear strength and compressive strength of the asphalt mixture will be enhanced, enabling it to better withstand the vehicle load at high temperature, and the plant asphalt mixture will have a stronger high-temperature rutting resistance. This finding has important practical significance for guiding the design and application of plant asphalt mixtures, especially considering the road performance under high temperature conditions. Therefore, the addition of inorganic active powder curing agent not only improves the physical properties of plant asphalt, but also enhances its application potential under extreme temperature conditions.

[0062] In order to gain a deeper understanding of the low-temperature performance of cured vegetable asphalt and determine the optimal curing agent dosage, a bending beam rheological test was conducted on the cured vegetable asphalt. The test was conducted at three different temperatures: -18°C, -12°C and -6°C. The bending beam rheological test results are shown in Figure 2. Fig. 9 , Fig.10As shown. The results show that as the test temperature decreases, the creep stiffness modulus S of the plant asphalt containing different amounts of curing agent shows a continuous upward trend, while the creep rate m shows a gradually decreasing characteristic. Under low temperature conditions, the rheological properties of plant asphalt are more rigid and less deformable, which is closely related to the arrangement and interaction of its molecular structure. When the temperature drops, the molecular movement in the plant asphalt slows down, resulting in a higher stiffness of the material as a whole. In particular, under the same temperature conditions, the plant asphalt samples with a higher curing agent content show a higher creep stiffness modulus, indicating that with the increase of the curing agent content, the mixing uniformity of the plant asphalt and the curing agent decreases, resulting in different degrees of agglomeration in the plant asphalt. This agglomeration effect makes the plant asphalt material gradually become more brittle and hard, and loses its original stress relaxation properties. Taking -12℃ as an example, only when the curing agent content is less than or equal to 20%, the creep stiffness modulus of the plant asphalt remains below 300MPa, and the creep rate is greater than or equal to 0.3, which meets the low temperature performance level of PG-12. In addition, due to the decrease in temperature, the proportion of free asphalt in the plant asphalt decreases, resulting in the saturation of the interaction ability between the plant asphalt and the curing agent. This saturation phenomenon leads to a decrease in the rheological properties of the plant asphalt. It can be seen from the above that when the amount of inorganic active powder curing agent is small, the low-temperature performance of the plant asphalt is significantly improved, but correspondingly, its high-temperature performance is insufficient. On the contrary, when the curing agent dosage is high, the high-temperature performance of the plant asphalt is significantly enhanced, and it can better resist deformation and flow at high temperatures. However, too high a curing agent dosage will lead to a decrease in the low-temperature performance of the asphalt, that is, its crack resistance is weakened. When the inorganic active powder curing agent accounts for 20% of the mass of the plant asphalt, through the three major index tests of the plant asphalt, the dynamic shear rheology test, and the bending beam rheology test, it can be found that its high-temperature performance and low-temperature performance are both excellent, which can not only ensure the stability of the plant asphalt at high temperatures, but also maintain its crack resistance at low temperatures. Therefore, the optimal curing agent dosage of the plant asphalt was selected as 20%. At this dosage, the cured plant asphalt showed relatively excellent performance.

[0063] The Zeiss Merlin Compact scanning electron microscope was used to observe the plant asphalt mixed with 20% curing agent. The results are as follows: Fig.11 The test image of the cured vegetable asphalt magnified 5000 times by scanning electron microscope; Fig.12This is a test image of the cured plant asphalt under a scanning electron microscope at 10,000 times magnification. After 5,000 times magnification, it can be seen that some wrinkles appear on the surface of the cured plant asphalt, but no stratification occurs, due to the fine particle size and excellent dispersion performance of the curing agent particles. During the mixing process, the curing agent particles can be evenly dispersed in the matrix of the plant asphalt, avoiding agglomeration and local excessive concentration. At the same time, the coating effect of the plant asphalt on the inorganic active powder curing agent is very sufficient, thanks to the viscosity and wetting properties of the asphalt. The asphalt can tightly wrap the curing agent particles to form a uniform covering layer, ensuring a close bond between the curing agent and the asphalt. This good coating effect further enhances the wetting effect, allowing the curing agent particles to better interact with the asphalt matrix. The wetting effect is significant, which not only increases the contact area between the curing agent and the asphalt, but also promotes the interfacial reaction between the two. After 10,000 times magnification, fine particles coated with plant asphalt can be seen, which are presumed to be the reaction residues of the inorganic active powder curing agent. The reaction products with "volcanic ash effect" are interwoven in the plant asphalt mortar to form a unique network skeleton structure, which significantly improves the mechanical properties of the plant asphalt. The cured plant asphalt shows good viscoelasticity and can maintain good deformation recovery ability when subjected to external forces. In addition, this network skeleton structure also helps to reduce the voids and defects inside the plant asphalt, further improving its density and durability.

[0064] Thermogravimetric analysis (TG) can measure the mass loss of materials at different temperatures, and then infer the thermal decomposition temperature, thermal stability and possible components of the material, so as to reveal the thermal decomposition law of the solidified plant asphalt. The German NETZSCH synchronous thermal analyzer STA 449C was selected, with N2 as the atmosphere, the temperature range was room temperature-900℃, and the test results of plant asphalt with a curing agent content of 20% were as follows Fig.13As shown. According to the comprehensive change trend of the TG curve and the DTG curve in the figure, before 340℃, the weight loss of plant asphalt is decreasing slowly, which is mainly due to the gradual evaporation of water and other evaporable substances in the plant asphalt during the heating process. Between 340℃ and 460℃, the weight loss rate of plant asphalt increases rapidly, indicating that a more violent reaction occurs inside the plant asphalt within this temperature range. The materials that constitute the main body of asphalt, such as organic polymer compounds, begin to suffer a large amount of pyrolysis loss. These compounds decompose at high temperatures to produce gas and liquid products, resulting in a rapid decrease in the weight of plant asphalt. After 460℃, the weight loss of plant asphalt gradually stabilizes, the pyrolysis reaction inside the plant asphalt has been basically completed, and the remaining components have high thermal stability, and are not prone to significant pyrolysis losses. They are the solidified products generated by the reaction of plant asphalt and inorganic active powder, which shows that the addition of inorganic active powder curing agent can greatly improve the thermal stability of plant asphalt. The results show that after the plant asphalt is cured, when the test temperature reaches 340℃, the thermogravimetric loss rate is only 14.5%, and the cured plant asphalt has excellent thermal stability.

[0065] Example 2 Study on Optimization of Cement Paste Mix Ratio

[0066] In order to improve the low-temperature crack resistance of cement grouting materials and the bonding performance at the interface between cement slurry and plant asphalt-based asphalt mixture, the present invention found that adding styrene-butadiene rubber emulsion as a modifier into cement mortar can effectively improve the overall performance of cement slurry, especially the crack resistance under low temperature conditions and the bonding effect between different materials.

[0067] In this embodiment, P·O 42.5 cement is used as the main component, and is matched with styrene-butadiene rubber emulsion, mineral powder, sand, etc. to ensure that the basic performance of the grouting material is stable and reliable and can adapt to more changing environments. Through orthogonal experiments, fluidity, compressive strength, and flexural strength are selected as evaluation indicators, and the effects of different material dosages on grouting performance are systematically studied. Through a large number of experimental tests, a large amount of data is collected and analyzed and calculated to determine the optimal dosage of each material to determine the optimal composition design that meets the needs of plant asphalt semi-flexible pavement material grouting materials. Specifically, by adopting the orthogonal experimental design method, it is possible to systematically study the effects of multiple factors on a certain performance, while ensuring the independence of each factor.

[0068] By adjusting the amount of water in the mix, the working performance of the cement grouting material is optimized to ensure that it can be smoothly poured into the plant asphalt matrix asphalt mixture, that is, the determination of the water (emulsion) dosage. The setting of the water (emulsion) dosage is that the water accounts for 50%, 55%, and 60% of the mass of the cementitious material (silica fume and cement, where silica fume is 5% of the mass of cement). By adjusting the proportion of styrene-butadiene rubber emulsion, it accounts for 15%, 10%, and 5% of the mass of the cementitious material (where silica fume is 5% of the mass of cement). The specific design type is shown in Table 1.

[0069] Table 1 Water (milk) dosage

[0070]

[0071] The amount of water (emulsion) will directly affect the fluidity, strength and other properties of the slurry, so the amount of water (emulsion) (a, b, c) is set. The addition of sand can change the particle grading and density of the grouting material, thereby affecting its mechanical properties and durability. In order to find the best sand content range, the sand content is set (10%, 15%, 20% of the total mass of cement and silica fume). The addition of mineral powder can not only improve the workability of the grouting material, but also improve its crack resistance and durability. The amount of mineral powder is set (5%, 10%, 15% of the total mass of cement and silica fume). The amount of water reducer is low, which is 0.5% (the ratio of water reducer to the total mass of cement and silica fume), so its effect on cement paste is not considered. The specific orthogonal test is shown in Table 2. The fluidity test was conducted according to T508-2005 cement paste fluidity determination method in the specification "JTGE30-2005 highway engineering cement and cement concrete test procedures"; the flexural strength and compressive strength of cement paste were determined according to T506-2005 cement mortar strength test method (ISO method) in the specification "JTGE30-2005 highway engineering cement and cement concrete test procedures". The test results of the compressive strength (7d) and flexural strength (7d) of cement paste and the fluidity of cement paste are shown in Table 3.

[0072] Table 2 Orthogonal test table

[0073]

[0074] Table 3 Orthogonal test results

[0075]

[0076]

[0077] SPSSAU data processing software was used to analyze the test results of the orthogonal test. First, the test data of the orthogonal test were sorted using SPSSAU. Then, the range analysis method in the software was used to rank the parameters. By sorting and numbering the data, the relative size and importance of different parameters can be intuitively compared. After calculation and processing by SPSSAU, the ranking results of each parameter were obtained, and the results are shown in Tables 4-6.

[0078] Table 4 Compressive strength range analysis table

[0079]

[0080] Note: “-” in the table means there is no data at that level

[0081] The results show that the range of the water-binder ratio is as high as 3.40, which significantly highlights the dominant role of water (emulsion) content in affecting the compressive strength of cement paste. The extreme value differences of mineral powder content and sand content are 0.93 and 0.53, respectively, which indicates that under the current test conditions, the impact on the 7-day compressive strength of cement paste is relatively small. When the water (emulsion) content type is a, the mineral powder content is 10%, and the sand content is 20%, the 7-day compressive strength of cement paste reaches the optimal value. However, this set of optimal component content did not appear in the nine sets of orthogonal experiments we designed previously, indicating the emergence of new potential optimal combinations.

[0082] Table 5 Analysis of the range of flexural strength

[0083]

[0084]

[0085] Note: “-” means there is no data at that level

[0086] The above results show that among the factors affecting the 7d flexural strength of cement paste, the range of water (emulsion) content reached 1.10, which is the same as the 7d compressive strength, and both are decisive factors, while the mineral powder content and sand content are the weaker ones. Based on the above range, we can clearly conclude that the factors positively correlated with the 7d flexural strength of cement paste are ranked as follows: water (emulsion) content (A) > mineral powder content (B) > sand content (C). Further analysis of the optimal level combination shows that when the water (emulsion) content is a, the mineral powder content is 10%, and the sand content is 20%, the 7-day flexural strength of cement paste reaches the optimal level. This group of content ratios is the same as the 7d compressive strength of the above cement paste, and it does not appear in the orthogonal table of the above nine groups of tests.

[0087] Table 6 Fluidity range analysis table

[0088]

[0089] Note: “-” in the table means there is no data at that level

[0090] As can be seen from Table 6, the range of water (emulsion) content reached 3.03, which is significantly higher than other factors, showing the dominant role of water (emulsion) content in determining the fluidity of cement paste. The range of sand content is closely followed, which is 1.87, indicating that sand content also has a certain influence on fluidity. In contrast, the range of mineral powder content is smaller, which is 0.43, indicating that its influence on fluidity is relatively small. However, the quality of fluidity is inversely related to the range value: a lower fluidity value means better flow performance. Therefore, using the fluidity of cement paste as an evaluation index is exactly the opposite of the fluidity range analysis table. Therefore, the water-cement ratio is c, the mineral powder content is 10%, and the sand content is 10%. At this time, the fluidity of cement paste is optimal.

[0091] Therefore, when fluidity is used as an evaluation index, the optimal mix ratio should be: water (emulsion) content c, mineral powder content 10%, sand content 10%. At the same time, based on the range analysis of 7-day compressive strength and flexural strength, the optimal cement paste mix ratio previously determined is: water (emulsion) content a, mineral powder content 10%, sand content 20%. This is different from the results obtained from the range analysis of fluidity. In view of the fact that the base asphalt mixture grouting material must not only meet the mechanical performance requirements, but also consider fluidity, after many tests, the final cement paste formula was selected as follows: water (emulsion) content: b (water accounts for 55% of the cementitious material, styrene-butadiene rubber emulsion accounts for 10% of the cementitious material, mineral powder content: 10% of the cementitious material, sand content: 15% of the cementitious material, the cementitious material is cement and silica fume, and silica fume is 5% of the mass of cement. The performance test results are shown in Table 7 below.

[0092] Table 7 Test results

[0093]

[0094] From the above, it can be seen that the mechanical properties and fluidity of the cement paste at this dosage are relatively excellent. The cement paste that not only meets the mechanical performance requirements but also has good fluidity can fully meet the requirements for grouting material application.

[0095] Example 3 Plant asphalt semi-flexible pavement material

[0096] The design concept of the plant asphalt semi-flexible pavement material provided by the present invention is based on a skeleton-compacted structure, in which a large-void plant asphalt matrix asphalt mixture provides a stable skeleton structure, and cement grouting is then poured into it to achieve structural compaction.

[0097] 1. Gradation design of plant asphalt matrix asphalt mixture

[0098] The volume method is used to design the gradation of large-void plant asphalt matrix asphalt mixture to ensure that the void ratio of the final plant asphalt matrix asphalt mixture meets the requirements of cement slurry injection while maintaining the structural stability and mechanical properties of the mixture. The design index parameters of the matrix asphalt mixture are shown in Table 8.

[0099] Table 8 Design index parameters of base asphalt mixture

[0100]

[0101] The volume method is used to design the gradation of large-void plant asphalt-based asphalt mixture, which specifically includes the following steps:

[0102] (1) Determine the main structure gradation composition and fine aggregate gradation composition of plant asphalt matrix asphalt mixture.

[0103] (2) Determine the packed density of coarse aggregate, the apparent density of coarse aggregate, the bulk density of fine aggregate, and the bulk density of mineral powder.

[0104] (3) Calculate the void ratio of the main structure of the base asphalt mixture.

[0105]

[0106] Where: V VC is the void ratio of the main structure of the base asphalt mixture (%);

[0107] ρ SC is the packing density of the main structure of the base asphalt mixture (g / cm 3 );

[0108] ρt C is the apparent density of the main structure of the base asphalt mixture (g / cm 3 );

[0109] (4) Determine the amount of vegetable asphalt and mineral powder.

[0110] (5) Determine the target void ratio of the plant asphalt matrix asphalt mixture.

[0111] (6) Based on the material parameters, use equations (2) and (3) to solve the coarse and fine aggregate dosages and determine the gradation composition.

[0112] q f +q c +q p =100 (2)

[0113]

[0114] Where: q fis the fine aggregate content (%);

[0115] q c is the coarse aggregate content (%);

[0116] q p is the mineral powder content (%);

[0117] q a is the vegetable asphalt content (%);

[0118] ρ f is the bulk density of fine aggregate (g / cm 3 );

[0119] ρ p is the bulk density of mineral powder (g / cm 3 );

[0120] ρ sc is the compact density of coarse aggregate (g / cm 3 );

[0121] ρ a is the density of plant asphalt (g / cm 3 );

[0122] ρ f is the bulk density of fine aggregate (g / cm 3 );

[0123] ρ f is the bulk density of fine aggregate (g / cm 3 );

[0124] V vs Design target void ratio (%) for base asphalt mixture.

[0125] (7) Determine the optimal amount of vegetable asphalt.

[0126] (8) Determine the grading composition of plant asphalt matrix asphalt mixture at different void ratios.

[0127] Four different void ratio levels of 20%, 23%, 25%, and 28% were selected to construct different gradation combinations. The test was conducted in accordance with the "JTG E42-2005 Highway Engineering Aggregate Test Procedures" and the following data were obtained:

[0128] Packing density of coarse aggregate ρ sc =1.602g / cm 3 ;

[0129] Apparent density of coarse aggregate ρ tc =2.768g / cm 3 ;

[0130] Bulk density of fine aggregate ρ f =2.794g / cm 3 ;

[0131] Bulk density of mineral powder ρ p =2.695g / cm 3 ;

[0132] Density of vegetable asphalt ρ a =0.9g / cm 3 .

[0133] In this embodiment, a plant asphalt-based asphalt mixture with a porosity of 25% is taken as an example, and the proportion of mineral powder is 3%. Different amounts of plant asphalt are selected, which are 3.0%, 3.5%, 4.0%, 4.5% and 5.0% (of the total mass of coarse aggregate, fine aggregate and mineral powder), respectively. Formulas (1), (2) and (3) are combined to obtain the amounts of coarse aggregate and fine aggregate at different plant asphalt amounts, as shown in Table 8 below.

[0134] Table 8 Proportion results of asphalt mixture based on plant asphalt under the condition of 25% void ratio

[0135]

[0136] According to the ratio of coarse and fine aggregates when the void ratio of plant asphalt matrix asphalt mixture is 25% in Table 8, through experiments and calculations, the mix ratio of plant asphalt matrix asphalt mixture is obtained as shown in Table 9.

[0137] Table 9 Calculation table of base asphalt mixture proportions at various asphalt dosages under the condition of a void ratio of 25%

[0138]

[0139] 2. Determination of the optimal asphalt dosage

[0140] Two test methods specified in the "JTG E20-2011 Highway Engineering Asphalt and Asphalt Mixture Test Procedure" were used to determine the optimal amount of vegetable asphalt. The Schellenberg leakage test (T 0732-2011) and the Kentenberg dispersion test (T 0733-2011) were used to determine the maximum and minimum asphalt amounts of the vegetable asphalt-based asphalt mixture. The Schellenberg leakage test ensures that no leakage occurs when the asphalt dosage is too high, thereby maintaining the stability and durability of the mixture. The Kentenberg dispersion test ensures that the asphalt dosage is not too low, which will lead to a decrease in the bonding strength between aggregates and affect the overall performance of the mixture. Finally, we took the average of these two values ​​as the optimal asphalt dosage of the vegetable asphalt-based asphalt mixture. The results are shown in Table 10.

[0141] Table 10 Optimal asphalt dosage under various designed void ratios

[0142]

[0143] 3. Grading composition of plant asphalt matrix asphalt mixture

[0144] By using the optimal asphalt dosage of vegetable asphalt at each void ratio in Table 10 above, and combining formulas (1), (2), and (3), the amount of coarse aggregate and fine aggregate at each void ratio is solved as shown in Table 11 below.

[0145] Table 11 Proportion results of asphalt mixture based on plant asphalt under different void ratio conditions

[0146]

[0147] According to the T 0709-2011 standard in the "JTG E20-2011 Highway Engineering Asphalt and Asphalt Mixture Test Procedure", the Marshall stability test was carried out on the plant asphalt-based asphalt mixture with different void ratios. It should be noted that the optimal amount of asphalt refers to the percentage amount of plant asphalt based on the total mass of coarse aggregate, fine aggregate and mineral powder, and a curing agent of 20% of the mass of plant asphalt is also required. In the plant asphalt-based asphalt mixture, the distribution of voids is mainly composed of closed voids, semi-open voids and fully open voids. In addition to closed voids, semi-open voids and fully open voids can allow cement paste to be poured smoothly. Therefore, when evaluating the void ratio of the plant asphalt-based asphalt mixture, the sum of the void ratios of semi-open voids and fully open voids is regarded as the effective void ratio. The results are shown in Table 12.

[0148] Table 12 Performance index of base asphalt mixture

[0149]

[0150] 4. Research on the injection of plant asphalt semi-flexible pavement material specimens

[0151] The vibrating sinking method was used to prepare the specimens of the semi-flexible pavement material of plant asphalt. The preparation of the specimens of the plant asphalt-based asphalt mixture followed the T0702-2011 and T 0703-2011 standards in the "JTG E20-2011 Highway Engineering Asphalt and Asphalt Mixture Test Procedure". According to these regulations, standard plant asphalt-based asphalt mixture Marshall specimens and standard plant asphalt rutting plate specimens were prepared respectively. In the process of preparing the semi-flexible pavement material of plant asphalt, the cured Marshall specimens were sealed with plastic wrap and tape at the bottom of the test mold. Since there was oil paper and test mold under the rutting specimen, there was no need to use plastic wrap and tape, but it was necessary to wrap plastic wrap and tape around to prevent side leakage. Then the treated Marshall specimens and rutting specimens were placed on the vibration table. When placing the specimens, ensure that the specimens were in close and stable contact with the vibration table to avoid shaking or displacement during the vibration process. Then, the vibration table was started. As the vibration table vibrated, cement slurry was added from above the specimen to fill the gaps between the base asphalt mixture. The vibration time and intensity were ensured to be moderate, so that the cement slurry could fully penetrate without damaging the specimen. At the same time, we also continuously added cement slurry during the vibration process to keep the slurry inside the specimen sufficient and uniform until the grouting was completed. The grouting specimen was placed in a curing room with a humidity of not less than 90% and a temperature of 20℃±3℃ for curing until the standard time. The finished product is as follows: Figure 14-16 As shown, the left side of the figure is a plant asphalt-based asphalt mixture specimen, and the right side is a plant asphalt-based asphalt mixture specimen poured with cement slurry. The cement slurry is the formula determined in Example 2: the water (emulsion) content is b (water accounts for 55% of the cementitious material, and the styrene-butadiene rubber emulsion accounts for 10% of the cementitious material), the mineral powder content is 10% of the cementitious material, the sand content is 15% of the cementitious material, and the silica fume content is 5% of the cement mass.

[0152] The filling degree of cement paste, i.e., the injection rate, is quantitatively characterized by calculating the ratio of the injected slurry volume to the volume of the connected voids in the plant asphalt matrix asphalt mixture. The results are shown in Table 13.

[0153] Table 13 Perfusion test results

[0154]

[0155] From the above test results, it can be observed that the actual void ratio and the connected void ratio test values ​​under different void ratio conditions are lower than the pre-designed void ratio. This phenomenon may be caused by several factors: First, there may be dust attached to the surface of the aggregate, which will affect the measurement of the void ratio. Second, the mineral powder and the inorganic active powder curing agent may not be fully mixed during the mixing process, thereby blocking the voids between the mixtures. In addition, the analysis results based on the three evaluation parameters of calculated grouting volume, actual grouting volume and grouting rate show that the cement paste has not been completely filled into every void of the plant asphalt matrix asphalt mixture. Under various void ratio conditions, the grouting rate of the cement paste has reached more than 88%, which means that the cement paste has successfully filled most of the voids in the plant asphalt matrix asphalt mixture, forming a tight and strong structure. This good combination not only significantly enhances the density of the mixture, making it have higher compressive strength and stability, but also improves the durability of the mixture and reduces damage caused by factors such as moisture intrusion and temperature changes. In addition, cement paste helps improve the cohesion and internal friction angle of the mixture, further enhancing its overall performance.

[0156] Example 4 Study on road performance of plant asphalt semi-flexible pavement material

[0157] 1. Study on high temperature stability of plant asphalt semi-flexible pavement materials

[0158] According to the plant asphalt base asphalt mixture at each void ratio in Table 12, basalt coarse and fine aggregates, limestone mineral powder, plant asphalt, and 20% of the mass of the plant asphalt are added with a curing agent, and plant asphalt semi-flexible pavement material rutting plate specimens with void ratios of 20%, 23%, 25%, and 28% are prepared according to "JTG E20-2011 Highway Engineering Asphalt and Asphalt Mixture Test Procedure" T 0719-2011. The formula of cement paste is: water (emulsion) content is b (water accounts for 55% of the cementitious material, styrene-butadiene rubber emulsion accounts for 10% of the cementitious material), mineral powder content is 10% of the cementitious material, sand content is 15% of the cementitious material, and silica fume is 5% of the cement mass. The grouting specimens were placed in a curing room with a humidity of not less than 90% and a temperature of 20℃±3℃ for curing to the standard time. After the curing was completed, the plant asphalt semi-flexible pavement material rutting plate specimens and their test molds were kept warm in a constant temperature room, and the wheel pressure load was set according to the test specifications. The results are shown in Table 14 and Fig.17 .

[0159] Table 14 Rutting test results

[0160]

[0161] The test results show that with the increase of the porosity of the plant asphalt semi-flexible pavement material, the deformation of the plant asphalt semi-flexible pavement material gradually decreases. With the gradual increase of the internal porosity of the mixture, the higher grouting amount increases the mass of the cement paste in the mixture, successfully fills most of the voids in the mixture, forms a tight and strong structure, and leads to a reduction in deformation in the rutting test. The dynamic stability of the rutting specimen with a porosity of 28% is as high as 19091 times / mm, far exceeding the requirements of JT / T1238-2019 Cement-based grouting materials for semi-flexible pavement materials for semi-flexible pavement materials. The specimens with other porosity also meet the requirements of the specification for the dynamic stability of semi-flexible pavement materials of 10,000 times / mm. The damage of the wheel pressure of the rutting test to the plant asphalt semi-flexible pavement material is largely resisted due to the filling effect of the cement paste, which makes it have higher compressive strength and stability. At the same time, the cement paste also helps to improve the cohesion and internal friction angle of the mixture, so that the plant asphalt semi-flexible pavement material can better resist vehicle loads.

[0162] from Fig.17 It can be seen that with the increase of loading time, the rutting depth of the plant asphalt semi-flexible pavement material is gradually increasing. The rutting change of the specimens with a void ratio of 25% and 28% is smaller than that of the specimens with a void ratio of 20% and 23%. When the test time reaches 40 minutes, the semi-flexible materials with a void ratio of 28% and 25% show a stable deformation, while the samples with a void ratio of 20% and 23% fail to show an obvious stable trend within the 60-minute test time. This indicates that under these lower void ratio conditions, the structure of the plant asphalt semi-flexible pavement material may be more sensitive to changes in external conditions and it takes longer to reach a stable state. Further analysis shows that the difference in cement paste grouting volume and void ratio causes the plant asphalt semi-flexible pavement material under the conditions of 20% and 23% void ratio to show more flexible characteristics, indicating that the plant asphalt semi-flexible pavement material has certain creep characteristics.

[0163] From the above rutting test results of plant asphalt semi-flexible pavement materials, it can be seen that plant asphalt semi-flexible pavement materials have significant advantages in high temperature stability. Especially under the condition of continuous high temperature, plant asphalt semi-flexible pavement materials show excellent heat resistance and deformation resistance. This material can still maintain its structural integrity and stability, and effectively resist the occurrence of rutting and sliding. Therefore, the excellent high temperature stability of plant asphalt semi-flexible pavement materials is of great significance for extending the service life of the pavement and reducing maintenance costs.

[0164] 2. Study on low temperature crack resistance of plant asphalt semi-flexible pavement materials

[0165] The small beam bending test was used to cut the vegetable asphalt semi-flexible pavement material into standard small beam specimens for the low temperature bending test. During the test, a load was applied to the middle section of the small beam specimen. As the load increased, the small beam specimen gradually bent and deformed. The various data during the test were recorded. The results are shown in Table 15.

[0166] Table 15 Beam bending test results

[0167]

[0168] When the void fraction is 20%, the average value of the maximum bending strain is 1967.10με, and as the void fraction increases to 23%, this value significantly increases to 2134.50με, reaching the maximum value among the four void fractions. However, when the void fraction further increases to 25% and 28%, the average value of the maximum bending strain decreases to 2053.80με and 1832.40με, respectively.

[0169] This trend of change shows that in the preparation process of plant asphalt semi-flexible pavement materials, the more cement paste is added, the better. In fact, there is an optimal cement paste addition, which makes the material show the best low-temperature bending and tensile deformation resistance at a specific void ratio. In this test, this optimal addition appeared near a void ratio of 23%. The reason for this phenomenon is that as the void ratio increases, the filling amount of cement paste also increases accordingly. When styrene-butadiene rubber emulsion is added to the cement paste, this emulsion can effectively improve the brittleness of the cement material and enhance its flexibility. At the same time, this improvement also significantly improves the low-temperature relaxation performance of the plant asphalt semi-flexible pavement material, making the material more "flexible" overall. This enhanced flexibility enables the material to better resist bending deformation under low temperature conditions, thereby exhibiting good low-temperature crack resistance.

[0170] 3. Study on water stability of plant asphalt semi-flexible pavement materials

[0171] According to the T0709-2011 standard in the "JTG E20-2011 Highway Engineering Asphalt and Asphalt Mixture Test Procedure", the Marshall specimens of the plant asphalt semi-flexible pavement material were tested after 7 days of maintenance. In order to accurately evaluate the water stability of the plant asphalt semi-flexible pavement material, the specimens were carefully divided into two test groups and different immersion test processes were performed. The first group of specimens was immersed in a 60°C water bath for 30 to 40 minutes, and then the Marshall stability was immediately measured. The stability value recorded at this time was recorded as MS. The second group of specimens was immersed in the same temperature conditions for 48 hours, and the Marshall stability was measured and recorded as MS1. The residual stability MS0 was calculated by MS1 / MS×100%. Using the residual stability MS0 as an evaluation index, the stability performance of the plant asphalt semi-flexible pavement material after long-term water immersion can be quantitatively analyzed, thereby objectively evaluating its water stability. The results are shown in Tables 16 and 17.

[0172] Table 16 Marshall test results of vegetable asphalt base asphalt mixture

[0173]

[0174] Table 17 Marshall test results of plant asphalt semi-flexible pavement materials

[0175]

[0176] The results show that the standard Marshall test values ​​of all four different void ratios exceed the design requirements for the base asphalt mixture in "JT / T1238-2019 Cement-based Grouting Materials for Semi-flexible Pavement Materials", which is a minimum strength standard of 3.0kN. The main reason for this result is a series of physical and chemical reactions between the inorganic active powder curing agent and the plant asphalt. The interfacial chemical effect of plant asphalt on volcanic ash is manifested at the molecular level of the contact interface between the two, and a close bond on the interface is achieved through charge transfer, chemical bonding, etc. This combination not only enhances the bonding properties of asphalt, but also enhances the overall stability of the mixture and lays the foundation for its performance improvement. This promotes a close bond between the two. The further addition of inorganic active powder not only promotes the chemical reaction with plant asphalt, but also generates a large amount of inorganic hydration products, thereby improving the strength of the plant asphalt matrix asphalt mixture. However, with the increase of the void ratio of the mixture, the Marshall stability and water-immersion Marshall stability of the plant asphalt matrix asphalt mixture are decreasing, showing a downward trend, which means that the deformation resistance and bearing capacity of the mixture are gradually weakening. Excessive void ratio not only weakens the overall strength of the mixture, but also makes its interior more susceptible to the influence of the external environment and load.

[0177] From the above test results, it can be seen that the Marshall stability and water-immersion Marshall stability of plant asphalt semi-flexible pavement materials are superior to those of plant asphalt-based asphalt mixtures. The injection of cement slurry fills most of the voids in the mixture, forming a tight and strong structure. The residual stability of the semi-flexible material at all void ratios is greater than or equal to 94%. This good combination not only significantly enhances the density of the mixture, giving it higher compressive strength and stability, but also proves that the coagulation and hardening effect of the cement slurry significantly improves the water stability of the semi-flexible pavement material.

[0178] 4. Freeze-thaw splitting test of plant asphalt semi-flexible pavement materials

[0179] According to T0729-2011 of "JTG E20-2011 Test Procedure for Asphalt and Asphalt Mixtures for Highway Engineering", the splitting tensile strength test of the cured vegetable asphalt semi-flexible material specimens was carried out, and the results are shown in Table 18.

[0180] Table 18 Freeze-thaw splitting test results

[0181]

[0182] From the above results, it can be seen that as the cement paste can fully infuse and fill the internal voids of the asphalt mixture, the strength of the plant asphalt semi-flexible pavement material shows a significant upward trend. The freeze-thaw splitting percentages of the plant asphalt semi-flexible pavement material specimens with four different void ratios all exceed 84%. When the void ratio is 25%, the freeze-thaw splitting strength ratio reaches 88.3%, which is the highest data under the four void ratios. This further confirms the positive effect of cement paste in improving the water stability and mechanical properties of plant asphalt matrix asphalt mixtures. Compared with the standard requirements for the water stability of traditional asphalt mixtures in the "JTG F40-2004 Highway Asphalt Pavement Construction Technical Specifications" (the highest standard is 80%), the plant asphalt semi-flexible pavement materials used in this study can meet these standard values. This result clearly shows that the plant asphalt semi-flexible pavement material has excellent water stability under ice and snow cold weather conditions, greatly reducing the risk of pavement damage caused by insufficient water stability.

[0183] 5. Study on the anti-skid performance of plant asphalt semi-flexible pavement materials

[0184] According to the specification of "T 0964-2008 Test method for determining the friction coefficient of road surface by pendulum instrument", three tests were conducted and the results were averaged to ensure the reliability of the data. When conducting the test, the indoor temperature was 30℃. The results are shown in 19.

[0185] Table 19 Friction coefficient BPN test results

[0186]

[0187] From the above results, it can be seen that the BPN of the semi-flexible pavement materials with four target porosity ratios is higher than 45, indicating that this material can provide a stable and efficient friction coefficient, ensuring that the vehicle can firmly grip the ground when driving at high speed or in emergency braking, avoiding slipping due to insufficient braking performance.

[0188] From the above, it can be seen that the present invention provides a plant asphalt mortar as a road material, which includes plant asphalt and a curing agent. When the curing agent is added in an amount of 20%, it can not only ensure the stability of the plant asphalt at high temperatures, but also maintain its anti-cracking performance at low temperatures.

[0189] The gradation composition and optimal asphalt dosage of the plant asphalt semi-flexible pavement material provided by the present invention are tested on the performance of the plant asphalt-based asphalt mixture, including indicators such as Marshall stability, flow value, and void ratio. The test results show that the plant asphalt-based asphalt mixture exhibits excellent performance at different void ratios of 20%, 23%, 25%, and 28%. The infusion rates of the laboratory specimens of the plant asphalt semi-flexible pavement material at the four void ratios all reach more than 88%. The high infusion rate means that the cement slurry can fully penetrate into the voids of the mixture and form a good combination with the plant asphalt-based asphalt mixture.

[0190] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any person skilled in the art can use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.

Claims

1. A plant asphalt mortar for road materials, characterized in that: It includes plant asphalt and a curing agent, wherein the curing agent is a mixture of magnesium sulfate and magnesium oxide in a mass ratio of 1:2-3, and the curing agent is added in an amount of 15-25% of the mass of the plant asphalt; the plant asphalt is a dark brown liquid made from biological heavy oil and does not contain petroleum asphalt.

2. A plant asphalt matrix asphalt mixture, characterized in that: It comprises the plant asphalt mortar as claimed in claim 1 and stone, wherein the stone consists of coarse aggregate, fine aggregate and mineral powder.

3. The plant asphalt matrix asphalt mixture according to claim 2, characterized in that: The coarse aggregate and fine aggregate are basalt, and the mineral powder is lime powder.

4. The plant asphalt matrix asphalt mixture according to claim 2, characterized in that: Among the stone materials, the mass proportion of coarse aggregate is 82.3%-89.1%, the mass proportion of fine aggregate is 14.7%-7.9% and the mass proportion of mineral powder is 3%; The dosage of vegetable asphalt is 3%-5% of the total mass of the stone.

5. The plant asphalt matrix asphalt mixture according to claim 2, characterized in that: The void ratio of plant asphalt matrix asphalt mixture is 20-28%.

6. The plant asphalt matrix asphalt mixture according to claim 5, characterized in that: When the void ratio of the plant asphalt-based asphalt mixture is 20%, the coarse aggregate in the stone accounts for 84.2%, the fine aggregate accounts for 14.7% and the mineral powder accounts for 3%; the amount of plant asphalt used is 4.4%-4.6% of the mass of the stone, and the amount of curing agent used is 20% of the mass of the plant asphalt; When the void ratio of the plant asphalt-based asphalt mixture is 23%, the coarse aggregate in the stone accounts for 84.9%, the fine aggregate accounts for 12.1% and the mineral powder accounts for 3%; the amount of plant asphalt used is 4.1%-4.3% of the mass of the stone, and the amount of curing agent used is 20% of the mass of the plant asphalt; When the void ratio of the plant asphalt-based asphalt mixture is 25%, the coarse aggregate in the stone accounts for 86.1%, the fine aggregate accounts for 14.7% and the mineral powder accounts for 3%; the amount of plant asphalt used is 3.7%-3.9% of the mass of the stone, and the amount of curing agent used is 20% of the mass of the plant asphalt; When the void ratio of the plant asphalt-based asphalt mixture is 28%, the coarse aggregate in the stone accounts for 89.1%, the fine aggregate accounts for 7.9% and the mineral powder accounts for 3%; the amount of plant asphalt used is 3.4%-3.6% of the stone mass, and the amount of curing agent used is 20% of the plant asphalt mass.

7. A plant asphalt semi-flexible pavement material, characterized in that: It comprises a plant asphalt-based asphalt mixture and a cement grouting material as described in any one of claims 2 to 6, wherein the cement grouting material comprises cement, a modifier, silica fume, mineral powder, sand and a water reducer; the cement is P·O42.5 silicate cement, the modifier is styrene-butadiene rubber emulsion, the water reducer is a polycarboxylic acid water reducer, and the mineral powder is limestone mineral powder.

8. The vegetable asphalt semi-flexible pavement material according to claim 7, characterized in that: The modifier is 5-15% of the cementitious material, silica fume is 3-8% of the cement mass, mineral powder is 5-15% of the cementitious material, sand is 10-20% of the cementitious material, and the water reducer is 0.3-1% of the cement mass, wherein the cementitious material refers to silica fume and cement.

9. The vegetable asphalt semi-flexible pavement material according to claim 7, characterized in that: When in use, water is added to the cement grouting material in an amount of 50-60% of the mass of the cementitious material.

10. Use of the plant asphalt-based asphalt mixture according to any one of claims 2 to 6 and the plant asphalt semi-flexible pavement material according to any one of claims 7 to 9 in the preparation of a semi-flexible pavement.