Microbial carbon sequestration reinforcement and mine filling utilization method of urban solid waste recycled aggregate

Through microbial carbon sequestration technology, CO2 is fixed to form calcium carbonate, which solves the problems of high water absorption rate and low density of urban solid waste recycled aggregates, improves its mechanical properties, meets the requirements of mine filling, and achieves carbon fixation and emission reduction. It has wide application prospects.

CN119019122APending Publication Date: 2024-11-26CHINA UNIV OF MINING & TECH (BEIJING) +1
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202411126280.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The water absorption rate and low density of urban solid waste recycled aggregates are difficult to meet the engineering application requirements of mine filling, and there are carbon emission problems.

Method used

Using microbial carbon fixation technology, carbonic anhydrase mineralized bacteria are used to fix CO2 to form calcium carbonate, and combined with urban solid waste recycled aggregate for soaking or spraying to form reinforced recycled aggregate, reducing water absorption and porosity, and improving density and mechanics. performance.

Benefits of technology

It effectively improves the density and mechanical properties of regenerated aggregates, meets the conveying and mechanical properties conditions of mine filling, and at the same time realizes the fixation and emission reduction of CO2, with wide applicability and engineering application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019122A_ABST
    Figure CN119019122A_ABST
Patent Text Reader

Abstract

The invention discloses a microbial carbon sequestration reinforcement and mine filling utilization method of urban solid waste recycled aggregate, which comprises the following steps: step S1, fully mixing a microbial bacterial solution, a pH buffer solution and a calcium source solution with the urban solid waste recycled aggregate by adopting a soaking method or a spraying method to obtain mixed recycled aggregate; s2, putting the mixed recycled aggregate obtained in the step S1 into a carbonization test box for carbon sequestration strengthening treatment to obtain strengthened recycled aggregate; s3, fully mixing the reinforced recycled aggregate obtained in the step S2 with a gelling agent and water to obtain a filling material; and S4, filling the filling material obtained in the step S3 into the goaf through a filling pipeline. According to the invention, the problems of high water absorption and low density of the urban construction waste recycled aggregate are effectively improved, and the conveying performance and mechanical property of the filling material prepared from the recycled aggregate are improved, so that the filling material can be better suitable for coal mine cemented filling, urban solid wastes are treated, and a solution is provided for the problem of insufficient coal mine filling aggregate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of solid waste resource utilization and mine filling, and particularly relates to a method for enhancing microbial carbon fixation of urban solid waste recycled aggregates and mine filling utilization. Background Art

[0002] With the acceleration of urbanization and the development of the construction industry, the amount of urban solid waste generated has increased year by year. In 2023, China's general industrial solid waste generation reached 4.28 billion tons, the comprehensive utilization was 2.57 billion tons, and the disposal was 870 million tons. There is still a large amount of solid waste to be utilized or disposed. According to statistics, about 105,000 mu of fertile land in my country is affected by urban solid waste pollution every year. The stacking and landfilling of urban solid waste occupy land resources and bring great pressure to the ecological environment. At present, the technology for preparing recycled aggregates from urban solid waste has gradually matured, and urban solid waste can be processed into recycled aggregates through screening, crushing, cleaning and other processes. However, the water absorption rate of recycled aggregates after urban solid waste treatment is between 3.6% and 8.0%, the apparent density is 90% of natural aggregates, and the bulk density is 85% of natural aggregates. There are generally problems of high water absorption and low density. The prepared filling slurry has poor flow properties and high compression rate, which is difficult to meet the actual application of engineering.

[0003] In 2023, China's CO2 emissions increased by 565 million tons to 12.6 billion tons. In order to achieve the goal of carbon peak in 2030 and carbon neutrality in 2060, my country's industrial development needs to achieve its own green and low-carbon transformation. As industries that emit a large amount of CO2, the coal industry and the cement industry also need effective carbon fixation technology to reduce their own carbon emissions. Carbonic anhydrase mineralizing bacteria are non-photosynthetic CO2 assimilating microorganisms that can directly convert CO2 gas into HCO3 by producing carbonic anhydrase themselves. - , achieving direct fixation of CO2 in the air and combining with Ca under alkaline conditions 2+ Calcium carbonate is formed. Calcium carbonate generated under bacterial induction has a gelling effect. General urban construction solid waste, such as concrete and mortar, is alkaline and has carbon fixation potential. Combined with the carbon fixation and calcium carbonate gelling effect of microorganisms such as carbonic anhydrase, it can enhance the mechanical properties and other properties of construction solid waste recycled aggregates. The enhanced construction solid waste can be used in mine filling scenarios. A large number of underground mining goafs are used as disposal spaces for carbonized construction solid waste. It has a good application prospect for treating a large amount of urban solid waste, achieving CO2 gas fixation, and enriching the source of mine filling materials. Summary of the invention

[0004] The purpose of the present invention is to provide a method for enhancing carbon fixation by microorganisms of urban solid waste recycled aggregates and mine filling utilization, so as to solve the problems of high water absorption and low density of urban solid waste recycled aggregates.

[0005] To achieve the above object, the present invention adopts the following technical solution:

[0006] A method for enhancing carbon fixation of urban solid waste recycled aggregates by microorganisms and mine filling utilization comprises the following steps:

[0007] Step S1, using an immersion method or a spraying method to fully mix the microbial liquid, the pH buffer solution and the calcium source solution with the municipal solid waste recycled aggregate to obtain a mixed recycled aggregate;

[0008] Step S2, placing the mixed recycled aggregate obtained in step S1 into a carbonization test box for carbon fixation strengthening treatment to obtain strengthened recycled aggregate;

[0009] Step S3, fully mixing the reinforced recycled aggregate obtained in step S2 with a gelling agent and water to obtain a filling material;

[0010] Step S4, filling the filling material obtained in step S3 into the goaf through the filling pipeline.

[0011] In step S1, the specific steps of the immersion method are:

[0012] Step A1, preparing a microbial solution, wherein the volume ratio of the microbial solution to the calcium source solution is 1:1 to 4:1;

[0013] Step A2, preparing a pH buffer solution with a concentration of 0.5 to 1.5 mol / L and a volume ratio of 1:1 to 4:1 to the calcium source solution;

[0014] Step A3, preparing a calcium source solution with a concentration between 0.5 and 1.5 mol / L;

[0015] Step A4, mixing the microbial liquid obtained in step A1, the pH buffer solution obtained in step A2, and the calcium source solution obtained in step A3 to obtain a soaking solution;

[0016] Step A5, crushing and screening the construction waste by a crusher to obtain recycled aggregate, wherein the recycled aggregate with a particle size of 5 mm to 25 mm is used as recycled coarse aggregate, and the recycled aggregate with a particle size of less than 5 mm is used as recycled fine aggregate;

[0017] Step A6, according to the mass ratio of recycled aggregate to soaking liquid of 2:1, the recycled coarse aggregate and the recycled fine aggregate obtained in step A5 are respectively placed in the soaking liquid obtained in step A4 and soaked for 30 minutes.

[0018] In step S1, the specific steps of the spraying method are:

[0019] Step B1, preparing a microbial solution, wherein the volume ratio of the microbial solution to the calcium source solution is 1:1 to 4:1;

[0020] Step B2, preparing a pH buffer solution with a concentration of 0.5 to 1.5 mol / L and a volume ratio of 1:1 to 4:1 to the calcium source solution;

[0021] Step B3, preparing a calcium source solution with a concentration between 0.5 and 1.5 mol / L;

[0022] Step B4, mixing the microbial liquid obtained in step B1, the pH buffer solution obtained in step B2, and the calcium source solution obtained in step B3 to obtain a spray liquid, and adding the spray liquid to a spray gun pressure tank;

[0023] Step B5, crushing and screening the construction waste by a crusher to obtain recycled aggregate, wherein the recycled aggregate with a particle size of 5 mm to 25 mm is used as recycled coarse aggregate, and the recycled aggregate with a particle size of less than 5 mm is used as recycled fine aggregate;

[0024] Step B6, spraying the spraying liquid in the spray gun pressure tank of step B4 uniformly on the surface of the recycled coarse aggregate and recycled fine aggregate obtained in step B5 according to a certain mass ratio of aggregate to spraying liquid.

[0025] The microorganisms in the microbial liquid are carbonic anhydrase mineralizing bacteria, such as Bacillus gelatinus. Such bacteria can directly fix CO2 in the air without providing light and hydrogen, and efficiently catalyze the rapid hydration of CO2 to form bicarbonate, which is further hydrolyzed in an alkaline environment to form carbonate, which combines with a calcium source to form calcium carbonate. In the process, a large amount of microbial polysaccharides are produced, and the polysaccharides and calcium carbonate form a co-cementing system, and finally calcium carbonate with filling and cementing effects is formed inside and on the surface of the solid waste aggregate to improve the strength and density of the recycled aggregate and reduce the permeability and water absorption of the recycled aggregate.

[0026] The pH buffer does not form an insoluble precipitate with calcium ions, has a pH between 7.5 and 9.5, and is one of a tris (trishydroxymethylaminomethane) buffer, a barbiturate buffer, an ammonium chloride buffer, a borax-calcium chloride buffer, and a boric acid-potassium chloride buffer.

[0027] The calcium source solution is a soluble calcium salt solution, and the soluble calcium salt is one or more of calcium chloride, calcium acetate, calcium nitrate, and calcium bicarbonate.

[0028] In step S2, the carbonization test box provides CO2, and the volume concentration of CO2 during carbonization is between 400ppm and 27%, the temperature is between 20 and 40°C, and the humidity is between 60 and 90%.

[0029] The urban solid waste recycled aggregate is obtained by crushing and screening construction waste through a crusher. The construction waste is one or more of slag, concrete blocks, crushed stones, brick and tile fragments, and waste mortar.

[0030] The gelling agent is a cement-based gelling agent, a microbial gelling agent, or a mixture of two or more thereof.

[0031] The principle of the present invention is to use carbonic anhydrase-producing microorganisms (such as Bacillus gelatinus) to directly fix CO2 in the air, efficiently catalyze the rapid hydration of CO2 to form bicarbonate, further hydrolyze in an alkaline environment to generate carbonate, and combine with a calcium source to form calcium carbonate. In the process, a large amount of microbial polysaccharides are produced, and the polysaccharides and calcium carbonate form a co-cementing system. Finally, calcium carbonate with filling and cementing effects is formed inside and on the surface of solid waste aggregates to improve the strength and density of recycled aggregates and reduce the permeability and water absorption of recycled aggregates.

[0032] Beneficial effects: Compared with the prior art, the present invention has the following advantages:

[0033] (1) Using microbial carbon fixation enhancement technology to enhance the modification of recycled aggregates can effectively reduce the water absorption and porosity of recycled aggregates from urban construction waste, improve the mechanical properties and density of recycled aggregates, and make them meet the transportation and mechanical properties conditions required for underground mine filling.

[0034] (2) In the process of treating recycled aggregates and CO2 using carbonic anhydrase-producing carbonic anhydrase mineralizing bacteria, carbonic anhydrase can promote carbon cycle, convert carbon dioxide into calcium carbonate precipitation, achieve carbon fixation and emission reduction, help reduce greenhouse gas emissions, and protect the environment.

[0035] (3) The use of microbial carbon fixation enhancement technology to strengthen recycled aggregates has wide applicability and engineering application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The present invention uses microbial carbon fixation enhancement technology to enhance the recycled aggregates of urban solid waste and prepare filling materials;

[0037] Figure 2 The present invention discloses a process for strengthening recycled aggregate and preparing filling materials by using an immersion method;

[0038] Figure 3 The present invention discloses a process for strengthening recycled aggregate and preparing filling materials by spraying. DETAILED DESCRIPTION

[0039] The present invention will be further explained below in conjunction with the accompanying drawings.

[0040] like Figure 1 As shown, a method for enhancing carbon fixation by microorganisms of urban solid waste recycled aggregates and mine filling utilization of the present invention comprises the following steps:

[0041] Step S1, using an immersion method or a spraying method to fully mix the microbial liquid, the pH buffer solution and the calcium source solution with the municipal solid waste recycled aggregate;

[0042] Step S2, placing the municipal solid waste recycled aggregate obtained in step S1 into a carbonization test box for carbon fixation strengthening treatment to obtain strengthened recycled aggregate;

[0043] Step S3, mixing the reinforced recycled aggregate obtained in step S2 with cement and water in proportion to obtain a filling material;

[0044] Step S4, filling the filling material obtained in step S3 into the goaf through the filling pipeline.

[0045] Among them, the microorganisms in the microbial liquid are carbonic anhydrase mineralizing bacteria, such as Bacillus gelatinus. This type of bacteria can directly fix CO2 in the air without providing light and hydrogen, and efficiently catalyze the rapid hydration of CO2 to form bicarbonate, which is further hydrolyzed in an alkaline environment to form carbonate, which combines with a calcium source to form calcium carbonate. In the process, a large amount of microbial polysaccharides are produced, and the polysaccharides and calcium carbonate form a co-cementing system, and finally calcium carbonate with filling and cementing effects is formed inside and on the surface of the solid waste aggregate to improve the strength and density of the recycled aggregate and reduce the permeability and water absorption of the recycled aggregate.

[0046] The pH buffer does not form an insoluble precipitate with calcium ions, and the pH is between 7.5 and 9.5. The pH buffer is a tris (tris(hydroxymethylaminomethane)) buffer, a barbiturate buffer, an ammonium chloride buffer, a borax-calcium chloride buffer, or a boric acid-potassium chloride buffer.

[0047] The calcium source solution is a soluble calcium salt solution, and the soluble calcium salt is one or more of calcium chloride, calcium acetate, calcium nitrate, and calcium bicarbonate.

[0048] The gelling agent may be one or more gelling agent materials such as a cement-based gelling agent and a microbial gelling agent.

[0049] The carbonization test box provides CO2. The CO2 concentration during carbonization is between 400ppm and 27%, the temperature is between 20 and 40°C, and the humidity is between 60 and 90%.

[0050] Urban solid waste recycled aggregate is obtained by crushing and screening construction waste through a crusher. Construction waste is one or more of slag, concrete blocks, crushed stones, brick and tile fragments, and waste mortar.

[0051] The present invention will be further described below in conjunction with the embodiments.

[0052] Example 1

[0053] In this embodiment, the recycled aggregate of construction waste is strengthened by soaking method and used as mine filling raw material. Figure 2 As shown, the specific steps are as follows:

[0054] (1) preparing a microbial solution with a volume ratio of 1:1 to a calcium source solution;

[0055] (2) preparing a pH buffer solution with a concentration of 0.5 mol / L and a volume ratio of 1:1 with the calcium source solution;

[0056] (3) preparing a calcium source solution with a concentration of 0.5 mol / L;

[0057] (4) mixing the microbial solution obtained in step (1), the pH buffer solution obtained in step (2), and the calcium source solution obtained in step (3) to obtain a soaking solution;

[0058] (5) crushing and screening the construction waste by a crusher to obtain recycled aggregate, wherein the recycled aggregate with a particle size of 5 mm to 25 mm is used as recycled coarse aggregate, and the recycled aggregate with a particle size of less than 5 mm is used as recycled fine aggregate;

[0059] (6) placing the regenerated coarse aggregate and the regenerated fine aggregate obtained in step (5) into the soaking solution obtained in step (4) for 30 minutes in a mass ratio of the regenerated aggregate to the soaking solution of 2:1, and then placing them in a carbonization test chamber for microbial carbon fixation enhancement treatment to obtain enhanced regenerated coarse aggregate and enhanced regenerated fine aggregate;

[0060] (7) preparing a filling material by mixing the reinforced recycled coarse aggregate, reinforced recycled fine aggregate, cement and water obtained in step (6) in a mass ratio of 5:2:1:2;

[0061] (8) Fill the filling material obtained in step (7) into the goaf through a filling pipeline.

[0062] Through the above steps (1) to (7), this embodiment also obtains a kind of urban solid waste recycled aggregate filling material, whose raw materials are composed of reinforced recycled coarse aggregate, reinforced recycled fine aggregate, cement and water; the mass ratio of reinforced recycled coarse aggregate, reinforced recycled fine aggregate, cement and water is 5:2:1:2.

[0063] Example 2

[0064] In this embodiment, the recycled aggregate of urban construction waste is strengthened by spraying and used as mine filling raw materials. Figure 3 As shown, the specific steps are as follows:

[0065] (1) preparing a microbial solution with a volume ratio of 1:1 to a calcium source solution;

[0066] (2) preparing a pH buffer solution with a concentration of 1.5 mol / L and a volume ratio of 1:1 with the calcium source solution;

[0067] (3) preparing a calcium source solution with a concentration of 1.5 mol / L;

[0068] (4) mixing the microbial liquid obtained in step (1), the pH buffer solution obtained in step (2), and the calcium source solution obtained in step (3) to obtain a spray liquid, and adding the spray liquid to a spray gun pressure tank;

[0069] (5) crushing and screening the construction waste by a crusher to obtain recycled aggregate, wherein the recycled aggregate with a particle size of 5 mm to 25 mm is used as recycled coarse aggregate, and the recycled aggregate with a particle size of less than 5 mm is used as recycled fine aggregate;

[0070] (6) spraying the spray liquid in the spray gun pressure tank of step (4) uniformly on the surface of the recycled coarse aggregate and the recycled fine aggregate obtained in step (5) at a mass ratio of aggregate to spray liquid of 4:1, and placing the recycled coarse aggregate and the recycled fine aggregate in a carbonization test chamber for microbial carbon fixation enhancement treatment to obtain enhanced recycled coarse aggregate and enhanced recycled fine aggregate;

[0071] (7) preparing a filling material by mixing the reinforced recycled coarse aggregate, reinforced recycled fine aggregate, cement and water obtained in step (6) in a mass ratio of 5:2:1:2;

[0072] (8) Fill the filling material obtained in step (7) into the goaf through a filling pipeline.

[0073] Through the above steps (1) to (7), this embodiment also obtains a kind of urban solid waste recycled aggregate filling material, whose raw materials are composed of reinforced recycled coarse aggregate, reinforced recycled fine aggregate, cement and water; the mass ratio of reinforced recycled coarse aggregate, reinforced recycled fine aggregate, cement and water is 5:2:1:2.

[0074] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for enhancing carbon fixation by microorganisms of recycled aggregates from municipal solid waste and mine filling, characterized in that: The following steps are involved: Step S1, using an immersion method or a spraying method to fully mix the microbial liquid, the pH buffer solution and the calcium source solution with the municipal solid waste recycled aggregate to obtain a mixed recycled aggregate; Step S2, placing the mixed recycled aggregate obtained in step S1 into a carbonization test box for carbon fixation strengthening treatment to obtain strengthened recycled aggregate; Step S3, fully mixing the reinforced recycled aggregate obtained in step S2 with a gelling agent and water to obtain a filling material; Step S4, filling the filling material obtained in step S3 into the goaf through the filling pipeline.

2. The method for enhancing carbon fixation by microorganisms and utilizing mine filling of urban solid waste recycled aggregates according to claim 1 is characterized in that: In step S1, the specific steps of the immersion method are: Step A1, preparing a microbial solution, wherein the volume ratio of the microbial solution to the calcium source solution is 1:1 to 4:1; Step A2, preparing a pH buffer solution with a concentration of 0.5 to 1.5 mol / L and a volume ratio of 1:1 to 4:1 to the calcium source solution; Step A3, preparing a calcium source solution with a concentration between 0.5 and 1.5 mol / L; Step A4, mixing the microbial liquid obtained in step A1, the pH buffer solution obtained in step A2, and the calcium source solution obtained in step A3 to obtain a soaking solution; Step A5, crushing and screening the construction waste by a crusher to obtain recycled aggregate, wherein the recycled aggregate with a particle size of 5 mm to 25 mm is used as recycled coarse aggregate, and the recycled aggregate with a particle size of less than 5 mm is used as recycled fine aggregate; Step A6, according to the mass ratio of recycled aggregate to soaking liquid of 2:1, the recycled coarse aggregate and the recycled fine aggregate obtained in step A5 are respectively placed in the soaking liquid obtained in step A4 and soaked for 30 minutes.

3. The method for enhancing carbon fixation by microorganisms and utilizing mine filling of urban solid waste recycled aggregates according to claim 1, characterized in that: In step S1, the specific steps of the spraying method are: Step B1, preparing a microbial solution, wherein the volume ratio of the microbial solution to the calcium source solution is 1:1 to 4:1; Step B2, preparing a pH buffer solution with a concentration of 0.5 to 1.5 mol / L and a volume ratio of 1:1 to 4:1 to the calcium source solution; Step B3, preparing a calcium source solution with a concentration between 0.5 and 1.5 mol / L; Step B4, mixing the microbial liquid obtained in step B1, the pH buffer solution obtained in step B2, and the calcium source solution obtained in step B3 to obtain a spray liquid, and adding the spray liquid to a spray gun pressure tank; Step B5, crushing and screening the construction waste by a crusher to obtain recycled aggregate, wherein the recycled aggregate with a particle size of 5 mm to 25 mm is used as recycled coarse aggregate, and the recycled aggregate with a particle size of less than 5 mm is used as recycled fine aggregate; Step B6, spraying the spraying liquid in the spray gun pressure tank of step B4 evenly on the surface of the recycled coarse aggregate and recycled fine aggregate obtained in step B5 according to a certain ratio of aggregate to spraying liquid.

4. The method for enhancing carbon fixation by microorganisms and utilizing mine filling of urban solid waste recycled aggregates according to any one of claims 1 to 3, characterized in that: The microorganisms in the microbial liquid are carbonic anhydrase mineralizing bacteria. The carbonic anhydrase mineralizing bacteria can efficiently catalyze the rapid hydration of CO2 to form bicarbonate without providing light and hydrogen, directly fix CO2 in the air, and further hydrolyze in an alkaline environment to form carbonate, which combines with a calcium source to form calcium carbonate. In the process, a large amount of microbial polysaccharides are produced, and the polysaccharides and calcium carbonate form a co-cementing system, and finally calcium carbonate with filling and cementing effects is formed inside and on the surface of the solid waste aggregate.

5. The method for enhancing carbon fixation by microorganisms and utilizing mine filling of urban solid waste recycled aggregates according to any one of claims 1 to 3, characterized in that: The pH buffer does not form an insoluble precipitate with calcium ions, has a pH between 7.5 and 9.5, and is one of a tris buffer, a barbiturate buffer, an ammonium chloride buffer, a borax-calcium chloride buffer, and a boric acid-potassium chloride buffer.

6. The method for enhancing carbon fixation by microorganisms and utilizing mine filling of urban solid waste recycled aggregates according to any one of claims 1 to 3, characterized in that: The calcium source solution is a soluble calcium salt solution, and the soluble calcium salt is one or more of calcium chloride, calcium acetate, calcium nitrate, and calcium bicarbonate.

7. The method for enhancing carbon fixation by microorganisms and utilizing mine filling of urban solid waste recycled aggregates according to any one of claims 1 to 3, characterized in that: In step S2, the carbonization test box provides CO2, and the volume concentration of CO2 during carbonization is between 400ppm and 27%, the temperature is between 20 and 40°C, and the humidity is between 60 and 90%.

8. The method for enhancing carbon fixation by microorganisms and utilizing mine filling of urban solid waste recycled aggregates according to any one of claims 1 to 3, characterized in that: The urban solid waste recycled aggregate is obtained by crushing and screening construction waste through a crusher. The construction waste is one or more of slag, concrete blocks, crushed stones, brick and tile fragments, and waste mortar.

9. The method for enhancing carbon fixation by microorganisms and utilizing mine filling of urban solid waste recycled aggregates according to any one of claims 1 to 3, characterized in that: The gelling agent is a cement-based gelling agent, a microbial gelling agent, or a mixture of two or more thereof.

Citation Information

Cited By

  • Recycled aggregate synergistically enhanced by two-step mineralization method and grain shape optimization method and preparation method thereof

    CN119638240A

  • A recycled aggregate synergistically enhanced by a two-step mineralization method and a particle shape optimization method and a preparation method thereof

    CN119638240B

  • Method for preparing mine negative carbon filling material based on solid waste-based carbonized aggregate

    CN120136468A

  • Underground cavern group construction waste residue in-situ curing and recycling process

    CN121088458A

  • Solid waste filling method based on MICP technology and carbon dioxide mineralization cooperation

    CN121676014A