High-temperature-resistant radiation-proof concrete and preparation method thereof

By optimizing the composition and preparation methods of radiation-proof concrete, the problem of degradation of radiation shielding performance and mechanical properties at high temperatures is solved, the safety of nuclear facilities is improved, and the theoretical basis for large-scale application of nuclear facilities is provided.

CN119019125AActive Publication Date: 2024-11-26SHANGHAI CONSTRUCTION GROUP CO LTD

Patent Information

Application Number
CN202411148720.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The existing radiation-proof concrete has degraded radiation shielding and mechanical properties under high temperature conditions, resulting in safety issues in nuclear facilities, especially in the case of core melting accidents in nuclear reactors, which require higher performance under the influence of heat and radiation.

Method used

By optimizing the composition and preparation method of radiation-proof concrete, the ratio of serpentine, snake-shaped sand, gelling materials, water and water reducing agents are adjusted, and the high-temperature water loss and mechanical properties attenuation coefficient are determined through high-temperature experiments, and the water-glue ratio is adjusted. and water-reducing dose, high-temperature radiation-resistant concrete is designed to improve its radiation shielding and mechanical properties at high temperatures.

Benefits of technology

It effectively improves the comprehensive performance of pit walls and near-core concrete, reduces nuclear radiation threats, ensures the ecological environment and personnel safety, and provides a theoretical basis for large-scale application of nuclear facilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019125A_ABST
    Figure CN119019125A_ABST
Patent Text Reader

Abstract

The invention relates to high-temperature-resistant radiation-proof concrete and a preparation method thereof. The concrete comprises the following components in percentage by mass (kg / m < 3 >): 600-700 parts of serpentine, 1000-1100 parts of serpentine sand, 500-600 parts of a cementing material, 200-230 parts of water and 8-9 parts of a water reducing agent. The high-temperature-resistant radiation-proof concrete is optimally designed, the neutron transmission resistance and the long-term mechanical property of the shielding concrete after high-temperature damage are considered at the same time, and the concrete is optimally designed at the beginning of mix proportion design, so that the comprehensive performance of the reactor pit wall and the near-reactor-core concrete under emergency conditions such as reactor core melting is effectively improved; by matching with bottom plate sacrifice concrete, the radiation shielding performance of the material after thermal damage can be effectively improved, the nuclear radiation threat is reduced, and the ecological environment safety and the personnel health are guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of radiation-proof concrete preparation, and particularly relates to high-temperature resistant radiation-proof concrete and a preparation method thereof. Background Art

[0002] At present, the global energy industry is transforming towards clean energy, and low-carbon emission energy such as nuclear energy will become an important solution to the future global increase in electricity demand. During the construction of nuclear power plants, radiation-proof concrete is mainly used for safety structures such as prestressed containment and nuclear island floor, which plays a role in shielding radiation and has high performance requirements. Unlike ordinary concrete, radiation-proof concrete not only has mechanical and construction performance requirements, but also has high requirements for the high-temperature performance and homogeneous performance of concrete. At present, the fourth-generation nuclear reactors, such as molten salt reactors, have a long-term working temperature of concrete above 150°C, which puts forward high requirements on the performance of pit wall concrete and near-core concrete. In addition, once a core melting accident occurs, the high-temperature performance requirements for radiation-proof concrete structures such as containment are higher, and the effects of heat and radiation need to be comprehensively considered.

[0003] Neutron radiation in nuclear radiation has strong penetrability. Neutrons scatter and collide with hydrogen nuclei, losing most of their energy. In engineering, materials with high crystalline water and high density are usually relied upon to slow down neutrons and absorb radiation. Aggregates are mainly barite, serpentine and limonite. Such aggregates usually have high density, large mass and high crystalline water content, so they have good radiation shielding capabilities. However, under the action of long-term neutron radiation and core thermal radiation, water is lost in concrete aggregates and cementitious materials, materials decompose, and thermal stress accumulates, resulting in a significant decrease in radiation protection capabilities and mechanical properties, causing safety issues.

[0004] Therefore, it is necessary to optimize the design of radiation-proof concrete under high temperature conditions to meet the requirements of new core protection. Summary of the invention

[0005] The present invention provides a high temperature resistant radiation proof concrete and a preparation method thereof, taking the radiation shielding performance and mechanical performance requirements of the radiation proof concrete at high temperature as the starting point, optimizing the design of the high temperature radiation proof concrete, providing a new path for optimizing the performance of radiation shielding structural materials, and thus effectively ensuring the safety of nuclear facilities. This method will promote the research on the composition, structure and performance relationship of radiation shielding materials, provide a corresponding theoretical basis for the design and construction of concrete radiation shielding structures, and solve the demand problem of large-scale application of nuclear facilities.

[0006] In order to solve the above technical problems, the present invention includes the following technical solutions:

[0007] A high temperature resistant radiation proof concrete, wherein the components of the concrete are in a mass ratio of (kg / m 3 ):

[0008] Serpentine 600-700, serpentine sand 1000-1100, cementitious material 500-600, water 200-230, water reducing agent 8-9.

[0009] A method for preparing high temperature resistant radiation proof concrete, the method comprising the following steps:

[0010] Step S1, preparing radiation-proof concrete that meets the design requirements of nuclear facilities at room temperature, making concrete specimens, and embedding temperature sensors in the concrete specimens, the temperature sensors are used to monitor and display the internal temperature of the concrete, the concrete specimens are placed in a standard curing room for curing to 28 days after demoulding, the concrete specimens are taken out and placed in a dry and ventilated place to dry to constant weight, and the mass is recorded as m0;

[0011] Step S2, placing the concrete specimen in a muffle furnace, heating it from room temperature to a target temperature at a certain heating rate, wherein the target temperature, the constant temperature fixing time and the constant temperature duration are all determined by the concrete working conditions, and a CO2 sensor is installed on the muffle furnace for real-time detection of CO2 concentration changes in the environment;

[0012] Step S3, firstly measure the total mass of CO2 in the muffle furnace before heating, recorded as m1, and after the constant temperature is over, use the CO2 sensor to measure the total mass of CO2 in the muffle furnace at a fixed temperature, recorded as m2, and the mass of CO2 generated by the decomposition of CaCO3 in the concrete during the heating process, recorded as m3, then m3 = m2-m1;

[0013] Step S4: After the experiment is over, the concrete specimen is immediately taken out from the muffle furnace and weighed, recorded as m4. The calculation formula for the amount of water lost during the high temperature process is: m = m0-m4-m3.

[0014] Therefore, the calculation formula for the high-temperature water loss L of single cubic meter concrete is:

[0015] L = m / V; m is in kg; V is the volume of the cylindrical concrete specimen, in m 3 ;

[0016] Step S5, A is the long-term mechanical property attenuation coefficient after high temperature damage for 112 days, A=G / S, G is the strength of concrete at high temperature for 112 days, in MPa; S is the strength of concrete at room temperature for 112 days; calculate the undamaged strength Cz of concrete at room temperature, Cz=Gz / A, Gz is the expected target value of concrete strength at high temperature,

[0017] Step S6: Obtain the mapping relationship between the strength fc of concrete at each age at room temperature and M by fitting method: c=a·log M)+b, where fc is the compressive strength at maturity M; a and b are constants obtained by fitting; M is the maturity calculated by the Nurse-Saul equation;

[0018] Step S7: When the design strength of concrete is less than C60, the concrete mix strength is determined by the following formula:

[0019] f cu,0 ≥f cu,k +1.645δ;

[0020] When the design strength of concrete is greater than or equal to C60, the concrete mix strength is determined by the following formula:

[0021] f cu,0 ≥1.15f cu,k ;

[0022] Where, δ is the standard deviation of concrete strength;

[0023] Step S8: Determine the concrete water-cement ratio R at high temperature 高温 , In the formula, a a and a b are regression coefficients, f b It is the 28d mortar compressive strength of cementitious material;

[0024] Step S9: Adjust the mix ratio while keeping the original mass of the main aggregate of the radiation-proof concrete at room temperature unchanged. 高温 =W 常温 +L,C 高温 =W 高温 / R 高温 , where W 高温 W is the water consumption of high temperature radiation proof concrete; 常温 C is the water consumption of radiation-proof concrete at room temperature; 高温 The amount of cementitious materials used for high temperature radiation proof concrete;

[0025] Step S10, increasing the amount of concrete water reducing agent, the water reducing agent increasing interval is 0.1% of the amount of cementitious material, so as to obtain the final proportion of high temperature radiation proof concrete.

[0026] Further, the Nurse-Saul equation is as follows: In the formula, M is maturity (℃·h or ℃·d); T is the average temperature of concrete in the time interval △t (℃); T0 is the reference temperature (℃), which refers to the temperature at which the strength of concrete no longer increases with age, that is, the temperature at which the hydration reaction inside the concrete stops. In the calculation, -10℃ is taken. Substituting the undamaged strength of concrete at room temperature Cz into the logarithmic model, the corresponding standard value of concrete 28d compressive strength f can be obtained.cu,k .

[0027] Furthermore, the concrete specimen is a formed cylindrical concrete specimen.

[0028] Furthermore, the size of the concrete specimen is φ60×80 mm. At this time, the volume of the cylindrical concrete specimen is (π×0.03 2 ×0.08).

[0029] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0030] The present invention provides a high temperature resistant radiation proof concrete, wherein the components of the concrete are in a mass ratio of (kg / m 3 ): Serpentine 600-700, serpentine sand 1000-1100, cementitious material 500-600, water 200-230, water reducing agent 8-9.

[0031] The high-temperature resistant and radiation-proof concrete is optimized in design, and the neutron transmission resistance and long-term mechanical properties of the shielding concrete after high-temperature damage are taken into consideration. The concrete is optimized at the beginning of the mix design, which effectively improves the comprehensive performance of the pit wall and near-core concrete in emergency situations such as core melting. Combined with the sacrificial concrete of the bottom plate, it can effectively improve the radiation shielding performance of the material after thermal damage, reduce the threat of nuclear radiation, and ensure the safety of the ecological environment and the health of personnel. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 A schematic diagram of a high temperature thermal damage experiment of high temperature resistant and radiation proof concrete according to an embodiment of the present invention;

[0033] Figure 2 A schematic diagram of high temperature thermal damage of high temperature resistant and radiation proof concrete according to an embodiment of the present invention;

[0034] Figure 3 It is a schematic diagram of the growth law of concrete strength at room temperature according to an embodiment of the present invention;

[0035] Figure 4 This is a schematic diagram of a neutron shielding test of high temperature resistant radiation proof concrete according to an embodiment of the present invention. DETAILED DESCRIPTION

[0036] The following is a further detailed description of a high temperature resistant radiation proof concrete and a preparation method thereof provided by the present invention in conjunction with specific embodiments and drawings. The advantages and features of the present invention will become more apparent from the following description.

[0037] Design concept: The description of key indicators such as crystal water content, material composition, thermal stability, density, etc. is the basis for accurately analyzing the evolution of the shielding capacity of radiation-proof concrete at any time, and is also a powerful means to optimize the design of new radiation-proof concrete.

[0038] (1) Prepare radiation-proof concrete that meets the design requirements of nuclear facilities at room temperature, form cylindrical concrete specimens (φ60×80mm), and embed temperature sensors in the concrete specimens. The temperature sensors are used to monitor and display the internal temperature of the concrete. After demolding, the specimens are placed in a standard curing room for curing until the age of 28 days. The specimens are taken out and placed in a dry and ventilated place to dry to constant weight. The mass of the concrete specimen is recorded as m0.

[0039] (2) See Figure 1 , the prepared concrete specimens are placed in a muffle furnace and heated from room temperature to the target temperature (100℃, 200℃, 300℃, 400℃, 500℃, 600℃, 700℃, 800℃) at a certain heating rate. The target temperature, constant temperature fixing time and constant temperature duration are all determined by the concrete working conditions. A CO2 sensor is installed on the muffle furnace to detect the change of CO2 concentration in the environment in real time.

[0040] (3) First, measure the total mass of CO2 in the muffle furnace before heating, recorded as m1. After the constant temperature is over, use the CO2 sensor to measure the total mass of CO2 in the muffle furnace at a fixed temperature, recorded as m2. During the heating process, the mass of CO2 generated by the decomposition of CaCO3 in the concrete is recorded as m3, which can be calculated by the following formula:

[0041] m3=m2-m1

[0042] (4) After the experiment, the concrete specimen is immediately taken out of the muffle furnace and weighed, and the mass is recorded as m4. Therefore, the amount of water lost during the high temperature process m can be calculated by the following formula:

[0043] m=m0-m4-m3

[0044] Therefore, the high-temperature water loss L of single cubic meter concrete can be calculated by the following formula:

[0045] L = m / V, V is the volume of the cylindrical concrete specimen, that is, L = m / (π×0.03 2 ×0.08)

[0046] (5)Reference Figure 3 Under normal temperature conditions, the strength growth of concrete shows obvious regularity, that is, the early strength grows rapidly, and the medium and long-term strength grows slowly, and the growth law conforms to the logarithmic model. However, under high temperature conditions, the internal structure of concrete is destroyed by evaporating water vapor and CO2, and the decomposition of hydration products causes the bond strength of the aggregate interface to be destroyed, and the mechanical properties of concrete are destroyed, that is, thermal damage is formed. Typical reference Figure 2 .

[0047] Assume that the 112d strength of concrete at room temperature is S, and the 112d strength of concrete at high temperature is G, with the unit of MPa. According to the requirements of the project for radiation-proof concrete, the long-term mechanical property attenuation coefficient A after 112d high-temperature damage can be calculated, and the calculation formula is as follows: In this embodiment, the 112d strength of concrete is used as the main identification standard for thermal damage, and the appropriate age is also selected according to actual needs in actual projects.

[0048] A=G / S

[0049] Under the condition that the types of radiation-proof aggregate and cementitious materials are determined, the undamaged strength Cz of concrete at room temperature can be calculated from the expected target value Gz of concrete strength at high temperature. The calculation formula is as follows:

[0050] Cz=Gz / A

[0051] (6) The mapping relationship between the strength fc of concrete at each age at room temperature and M can be obtained through the fitting method, which is very close to the logarithmic function model relationship. a and b are fitting parameters. The formula is as follows:

[0052] f c =a·log M)+b, where fc is the compressive strength at maturity M; a and b are constants obtained by fitting; and M is the maturity calculated by the Nurse-Saul equation.

[0053] The Nurse-Saul equation is as follows: Where M is maturity, in units of ℃·h or ℃·d; T is the average temperature of concrete within the time interval △t, in units of ℃; T0 is the reference temperature, in units of ℃. The reference temperature refers to the temperature at which the strength of concrete no longer increases with age, that is, the temperature at which the hydration reaction inside the concrete stops. In the calculation, -10℃ is taken. Substituting the undamaged strength of concrete at room temperature Cz into the logarithmic model, the corresponding standard value of the concrete 28d compressive strength f can be obtained. cu,k .

[0054] (7) According to the national standard "Ordinary Concrete Mix Design Code" (JGJ 55-2011):

[0055] When the design strength of concrete is less than C60, the concrete mix strength is determined by the following formula:

[0056] f cu,0 ≥f cu,k +1.645δ;

[0057] When the design strength of concrete is greater than or equal to C60, the concrete mix strength is determined by the following formula:

[0058] fcu,0 ≥1.15f cu,k ;

[0059] Where δ is the standard deviation of concrete strength.

[0060] (8) According to the national standard "Ordinary Concrete Mix Design Code" (JGJ 55-2011), determine the concrete water-binder ratio R at high temperature. 高温 , In the formula, a a and a b are regression coefficients, f b It is the 28d compressive strength of cementitious material mortar.

[0061] (9) Since the main water loss in concrete under high temperature is caused by the dehydration of calcium silicate gel, a cement hardening product, the mix ratio is adjusted while keeping the original mass of the main aggregates of the radiation-proof concrete at room temperature unchanged. Since the undamaged strength Cz of concrete at room temperature is higher than the strength of the mix ratio at room temperature, the calculated water-cement ratio is too small, so the total amount of concrete paste is adjusted to avoid the situation where the surface of the concrete aggregate is not covered with paste and water loss and cracking, thereby improving the stability of high-temperature radiation-proof concrete. The adjustment method is as follows:

[0062] W 高温 =W 常温 +L,C 高温 =W 高温 / R 高温 , where W 高温 The amount of water used for high temperature radiation proof concrete;

[0063] W 常温 C is the water consumption of radiation-proof concrete at room temperature; 高温 The amount of cementitious material used in high-temperature radiation-proof concrete.

[0064] (10) Given the high temperature water consumption W of high temperature radiation proof concrete 高温 , high temperature cementitious material dosage C 高温 , based on the amount of aggregate (using the original room temperature mix ratio), the amount of concrete water reducer is increased on the basis of the original room temperature mix ratio. After trial mixing, the concrete fluidity meets the specific construction requirements, thus obtaining the final mix ratio of high temperature radiation proof concrete. The water reducer is increased by 0.1% of the cementitious material dosage, thus obtaining the final mix ratio of high temperature radiation proof concrete.

[0065] During the design of nuclear-related structures, key design optimization parameters such as the high-temperature water loss L of concrete at the design temperature and the long-term mechanical properties attenuation coefficient A can be obtained from basic experiments, thereby deriving an optimized design scheme for high-temperature resistant and radiation-proof concrete.

[0066] The 28d performance data of concrete are all measured after the specimens are placed in a dry and ventilated place to cool to room temperature after thermal damage. The experimental heating rate is 4℃ / h and the constant temperature time is 2h.

[0067] The neutron flux after concrete shielding is measured by:

[0068] refer to Figure 4 The neutron shielding experiment uses the cylindrical concrete specimen of this embodiment.

[0069] The concrete sample is irradiated with a neutron source in the same energy range as the inner side of the molten salt reactor through the electron accelerator neutron source. The receiver can count the collected neutron energy, and the neutron shielding performance of the concrete can be calculated by using the ratio of the neutron flux after shielding to the neutron flux before shielding.

[0070] Example 1: The radiation protection concrete mix ratio at room temperature is as follows: (kg / m 3 )

[0071] Cementitious materials Serpentine Serpentine sand water Water reducing agent 400 690 1060 200 5.4

[0072] The mechanical properties and radiation shielding properties of concrete at room temperature are as follows:

[0073]

[0074] The mechanical properties and radiation shielding properties of concrete after 600℃ high temperature damage are as follows:

[0075]

[0076] After optimized design, the mix ratio of radiation protection concrete is as follows: (kg / m 3 )

[0077] Cementitious materials Serpentine Serpentine sand water Water reducing agent 532 690 1060 218 8.2

[0078] The mechanical properties and radiation shielding properties of concrete after high temperature damage are as follows:

[0079]

[0080] The mechanical properties and radiation shielding properties of concrete after 400℃ high temperature damage are as follows:

[0081]

[0082] After optimized design, the mix ratio of radiation protection concrete is as follows: (kg / m 3 )

[0083] Cementitious materials Serpentine Serpentine sand water Water reducing agent 508 690 1060 224 8.7

[0084] The mechanical properties and radiation shielding properties of concrete after high temperature damage are as follows:

[0085]

[0086] The above examples are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. The above embodiments only express several embodiments of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A high temperature resistant radiation proof concrete, characterized in that: The mass ratio of each component of the concrete is (kg / m 3 ): Serpentine 600-700, serpentine sand 1000-1100, cementitious material 500-600, water 200-230, water reducing agent 8-9.

2. The method for preparing high temperature resistant and radiation proof concrete according to claim 1, characterized in that: The steps include: Step S1, preparing radiation-proof concrete that meets the design requirements of nuclear facilities at room temperature, making concrete specimens, and embedding temperature sensors in the concrete specimens, the temperature sensors are used to monitor and display the internal temperature of the concrete, the concrete specimens are placed in a standard curing room for curing to 28 days after demoulding, the concrete specimens are taken out and placed in a dry and ventilated place to dry to constant weight, and the mass is recorded as m0; Step S2, placing the concrete specimen in a muffle furnace, heating it from room temperature to a target temperature at a certain heating rate, wherein the target temperature, the constant temperature fixing time and the constant temperature duration are all determined by the concrete working conditions, and a CO2 sensor is installed on the muffle furnace for real-time detection of CO2 concentration changes in the environment; Step S3, firstly measure the total mass of CO2 in the muffle furnace before heating, recorded as m1, and after the constant temperature is over, use the CO2 sensor to measure the total mass of CO2 in the muffle furnace at a fixed temperature, recorded as m2, and the mass of CO2 generated by the decomposition of CaCO3 in the concrete during the heating process, recorded as m3, then m3 = m2-m1; Step S4: After the experiment is over, the concrete specimen is immediately taken out from the muffle furnace and weighed, recorded as m4. The calculation formula for the amount of water lost during the high temperature process is: m = m0-m4-m3. Therefore, the calculation formula for the high-temperature water loss L of single cubic meter concrete is: L = m / V; m is in kg; V is the volume of the cylindrical concrete specimen, in m 3 ; Step S5, A is the long-term mechanical property attenuation coefficient after high temperature damage for 112 days, A=G / S, G is the strength of concrete at high temperature for 112 days, in MPa; S is the strength of concrete at room temperature for 112 days; calculate the undamaged strength Cz of concrete at room temperature, Cz=Gz / A, Gz is the expected target value of concrete strength at high temperature; Step S6: Obtain the mapping relationship between the strength fc of concrete at each age at room temperature and M by fitting method: c =a·log(M)+b, where fc is the compressive strength at maturity M; a and b are constants obtained by fitting; M is the maturity calculated by the Nurse-Saul equation; Step S7: When the design strength of concrete is less than C60, the concrete mix strength is determined by the following formula: f cu,0 ≥f cu,k +1.645s; When the design strength of concrete is greater than or equal to C60, the concrete mix strength is determined by the following formula: f u,0 ≥1.15f cu,k ; Where, δ is the standard deviation of concrete strength; Step S8: Determine the concrete water-cement ratio R at high temperature 高温 , In the formula, a a and a b are regression coefficients, f b It is the 28d mortar compressive strength of cementitious material; Step S9: Adjust the mix ratio while keeping the original mass of the main aggregate of the radiation-proof concrete at room temperature unchanged. 高温 =W 常温 +L,C 高温 =W 高温 / R 高温 , where W 高温 W is the water consumption of high temperature radiation proof concrete; 常温 C is the water consumption of radiation-proof concrete at room temperature; 高温 The amount of cementitious materials used for high temperature radiation proof concrete; Step S10, increasing the amount of concrete water reducing agent, the water reducing agent increasing interval is 0.1% of the amount of cementitious material, so as to obtain the final proportion of high temperature radiation proof concrete.

3. The preparation method according to claim 2, characterized in that: The Nurse-Saul equation is as follows: Where M is maturity, in units of ℃·h or ℃·d; T is the average temperature of concrete within the time interval △t, in units of ℃; T0 is the reference temperature, in units of ℃. The reference temperature refers to the temperature at which the strength of concrete no longer increases with age, that is, the temperature at which the hydration reaction inside the concrete stops. In the calculation, -10℃ is taken. Substituting the undamaged strength of concrete at room temperature Cz into the logarithmic model, the corresponding standard value of the concrete 28d compressive strength f can be obtained. cu,k .

4. The preparation method according to claim 3, characterized in that: The concrete specimen is a formed cylindrical concrete specimen.

5. The preparation method according to claim 4, characterized in that: The size of the concrete specimen is φ60×80mm.

Citation Information

Patent Citations

  • High-fluidity neutron-radiation-resistant concrete and preparation method thereof

    CN112079603A

  • Radiation-proof concrete composition, preparation method and prefabricated container

    CN112551951A

  • Method for detecting property degradation of concrete after high temperature action

    CN1945322A

Cited By

  • Device and method for measuring concrete volume change caused by long-term neutron irradiation

    CN120490162A

  • A device and method for measuring long-term neutron irradiation-induced volume change of concrete

    CN120490162B

  • Corrosion-resistant concrete formula optimization method and device and storage medium

    CN122314179A