Steel slag powder composite waste glass mortar and preparation method thereof
By mixing steel slag powder, waste glass powder, silicate cement, standard sand and red mud in a specific proportion, forming steel slag powder composite waste glass mortar, the problem of insufficient compressive and bending strength of existing waste glass mortar is solved, and the problem of insufficient compression and bending strength of existing waste glass mortar is achieved. It simplifies the preparation process and improves performance, and is suitable for cement mortar.
Patent Information
- Application Number
- CN202411162508.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-26
AI Technical Summary
The existing waste glass mortar has insufficient compressive and bending strength, and the preparation method is complex, the preparation environment is strict, and the expansion rate is high.
Steel slag powder, waste glass powder, silicate cement, standard sand and red mud are mixed in a specific proportion, and steel slag powder composite waste glass mortar is formed through stirring, simplifying the preparation process, improving compressive and bending strength, and reducing expansion rate.
The prepared steel slag powder composite waste glass mortar has excellent durability and mechanical properties, with improved compressive and flexural strength and reduced expansion rate. It is suitable for cement mortar, improving working performance and impermeability.
Smart Images

Figure CN119019136A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of concrete, and in particular to a steel slag powder composite waste glass mortar and a preparation method thereof. Background Art
[0002] Steel slag is an industrial solid waste produced during the steelmaking process, mainly composed of iron, calcium, magnesium, manganese and other components. Although the fineness of steel slag is difficult to meet the requirements of cement mortar materials, the dicalcium silicate and tricalcium silicate minerals therein are fully crystallized, and the grains are coarse and dense. Waste glass refers to glass, glass products and glass fibers that are no longer used and are discarded or abandoned. At present, there are many technologies for waste glass mortar. For example, Chinese invention patent CN 112979251 A discloses a waste glass mortar, which uses ordinary silicate cement, standard sand, glass powder, Na2SO4, mixed alkali, water and the like to prepare waste glass mortar. Due to the strict requirements of the alkaline environment conditions in its preparation process, this technology is limited by the influence of material composition and preparation environment. Chinese invention patent CN 113880515 A discloses a waste glass mortar and a preparation method. Its glass powder activation step and hydrothermal treatment conditions are complicated, and the compressive and flexural strengths of the waste glass mortar specimens need to be improved. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a steel slag powder composite waste glass mortar, which has good compressive and flexural strength and low expansion rate.
[0004] The technical problem to be solved by the present invention is also to provide a method for preparing steel slag powder composite waste glass mortar, which is simple and does not require complicated processing conditions. The prepared mortar has good compressive and flexural strength and a low expansion rate.
[0005] In order to solve the above problems, the present invention provides a steel slag powder composite waste glass mortar, which includes the following components in parts by weight: 3-7 parts of waste glass powder, 2-6 parts of steel slag powder, 8-10 parts of silicate cement, 16-20 parts of standard sand, 0.5-1.2 parts of red mud, and 4-6 parts of water.
[0006] Preferably, the following components are included in parts by weight: 4-6 parts of waste glass powder, 3-5 parts of steel slag powder, 8-9 parts of Portland cement, 17-19 parts of standard sand, 0.6-1 part of red mud, and 4-6 parts of water.
[0007] In some embodiments, the average particle size of the waste glass powder is 80 μm to 300 μm;
[0008] The SiO2 content of the waste glass powder is ≥60%.
[0009] In some embodiments, the average particle size of the steel slag powder is 0.8 μm to 12 μm;
[0010] The steel slag powder has a CaO content of ≥40%, a SiO2 content of ≥13%, a Fe2O3 content of ≥20%, and a free CaO content of ≤3.0%.
[0011] In some embodiments, the silicate cement is ordinary silicate cement.
[0012] In some embodiments, the total mass content of aluminum oxide and iron oxide in the red mud is ≥30%.
[0013] In order to solve the above problems, the present invention also provides a method for preparing steel slag powder composite waste glass mortar, comprising the following steps:
[0014] Mixing silicate cement, standard sand, waste glass powder and steel slag powder and stirring to obtain a dry material component;
[0015] The red mud and water are mixed and stirred to obtain a mixed liquid;
[0016] Pour the dry material components into the mixed liquid and stir evenly to obtain steel slag powder composite waste glass mortar.
[0017] In some embodiments, silicate cement, standard sand, waste glass powder, and steel slag powder are mixed and stirred for 200s to 300s to obtain a dry material component.
[0018] In some embodiments, the dry ingredients are poured into the mixed solution and stirred for 500s to 600s.
[0019] And, application of the steel slag powder composite waste glass mortar in cement mortar.
[0020] The implementation of the present invention has the following beneficial effects:
[0021] The present invention mixes waste glass powder, steel slag powder, silicate cement, standard sand, red mud and water, wherein the steel slag powder contains a large amount of substances such as iron oxide and silicon oxide, and has excellent durability and mechanical properties. The waste glass powder is used as a compensating material in cement mortar, which is beneficial to improving the strength and durability of the mortar. In addition, the oxides and silicates contained in the steel slag powder, waste glass and red mud react with the hydration products in the cement to form a dense gel system, which has a volcanic ash effect and helps to improve the working performance and anti-seepage performance of the cement mortar. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a process flow chart of the preparation method of the steel slag powder composite waste glass mortar provided by the present invention. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. In addition, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0024] In the description of the present invention, it is necessary to understand that the terms "length", "width", "up", "down", "left", "right", "horizontal", "top", "bottom", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0025] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0026] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or mutual communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0027] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.
[0028] The disclosure below provides many different embodiments or examples to realize different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the examples of various specific processes and materials provided by the present invention, but those of ordinary skill in the art can be aware of the application of other processes and / or the use of other materials.
[0029] In the present invention, "preferred" and "better" are only used to describe implementation methods or embodiments with better effects, and it should be understood that they do not constitute a limitation on the scope of protection of the present invention. In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features. In the present invention, when involving numerical ranges, unless otherwise specified, the two endpoints of the numerical range are included.
[0030] The invention provides a steel slag powder composite waste glass mortar, which comprises the following components in parts by weight: 3-7 parts of waste glass powder, 2-6 parts of steel slag powder, 8-10 parts of Portland cement, 16-20 parts of standard sand, 0.5-1.2 parts of red mud and 4-6 parts of water.
[0031] The present invention mixes waste glass powder, steel slag powder, silicate cement, standard sand, red mud and water, wherein the steel slag powder contains a large amount of substances such as iron oxide and silicon oxide, and has excellent durability and mechanical properties; the waste glass powder is used as a compensating material in cement mortar, which is beneficial to improving the strength and durability of the mortar. In addition, the oxides and silicates contained in the steel slag, waste glass and red mud react with the hydration products in the cement to form a dense gel system, which has a volcanic ash effect and helps to improve the working performance and anti-seepage performance of the cement mortar.
[0032] Specifically, waste glass powder refers to the product of waste glass after crushing and ball milling, and waste glass refers to glass, glass products and glass fibers that are no longer used and are discarded or abandoned. Exemplary weight parts of the waste glass powder are 3 parts, 4 parts, 5 parts, 6 parts, and 7 parts. Preferably, the weight parts of the waste glass powder are 4 to 6 parts. In some embodiments, the average particle size of the waste glass powder is 80μm to 300μm; preferably, the average particle size of the waste glass powder is 80μm to 100μm; it should be noted that when the waste glass powder is ground to the fineness within the above range, it will show volcanic ash activity, which enables the waste glass powder to replace part of the cement as an auxiliary cementitious material. In addition, the waste glass powder of the above particle size can improve the microstructure of cement mortar, thereby increasing its strength.
[0033] In some embodiments, the SiO2 content of the waste glass powder is ≥60%, which can improve the corrosion resistance and acid resistance of the mortar, thereby improving the durability of the mortar and resisting chemical erosion. Preferably, the waste glass powder includes the following chemical components in terms of mass percentage: SiO2 60-80%, Fe2O3 4-7%, Al2O3 6-11%, CaO 5-18%, MgO 1-5%. Among them, a high content of SiO2 can significantly improve the hardness and compressive strength of the mortar and provide a stable skeleton for the mortar. Alumina plays a reinforcing role in the mortar, which can improve the microstructure of the mortar and increase its density, thereby improving the compressive strength. An appropriate amount of calcium oxide can react with other components in the mortar (such as water, silicates, etc.) to generate hydration products, such as calcium hydroxide and calcium silicate gel, which help fill the pores in the mortar, improve the density, and thus enhance the compressive strength. However, too much CaO may cause the mortar to expand in volume and affect performance.
[0034] Steel slag powder refers to the product of steel slag after crushing and ball milling. Steel slag refers to steel slag, which is an industrial solid waste produced during the steelmaking process. The exemplary weight parts of the steel slag powder are 2 parts, 3 parts, 4 parts, 5 parts, and 6 parts. Preferably, the weight parts of the waste glass powder are 3 to 5 parts. In some embodiments, the average particle size of the steel slag powder is 0.8 μm to 12 μm; preferably, the average particle size of the steel slag powder is 1 μm to 10 μm; steel slag powder within the above-mentioned fineness range is beneficial to improving the fluidity, strength and durability of the mortar.
[0035] In some embodiments, the CaO content of the steel slag powder is ≥40%, the SiO2 content is ≥13%, the Fe2O3 content is ≥20%, and the free CaO content is ≤3.0%, so that the content of substances such as iron oxide and silicon oxide in the steel slag powder can be guaranteed. In addition, the presence of free calcium oxide has an adverse effect on the performance of cement mortar. On the one hand, it may lead to poor stability of cement mortar, because free calcium oxide will continue to react with water after the cement hardens to generate calcium hydroxide, accompanied by volume expansion, thereby destroying the structure of cement stone and reducing its strength. On the other hand, free calcium oxide will also affect the properties of cement such as setting time and strength development. Therefore, the present invention controls the free CaO content of the steel slag powder within 3.0%.
[0036] Preferably, the steel slag powder includes the following chemical components in terms of mass percentage: SiO2 13-27%, Fe2O3 20-30%, Al2O3 2-5%, CaO 40-55%, MgO 2-3%. The CaO content of the steel slag powder is relatively high, which can improve the compressive strength of the mortar. The combination of an appropriate amount of SiO2 helps to form a dense mortar structure. The hydrated calcium silicate gel generated by the reaction of SiO2 and CaO is one of the main sources of mortar strength. In addition, the iron oxide content is relatively high. Although it does not directly participate in the hydration reaction, it can be used as a filler to improve the microstructure of the mortar and to improve the density and compressive strength of the mortar to a certain extent.
[0037] Portland cement is a Portland cement clinker mainly composed of calcium silicate. The exemplary weight parts of the Portland cement are 8 parts, 8.5 parts, 9 parts, 9.5 parts, and 10 parts. Preferably, the weight parts of the Portland cement are 8 to 9 parts. In some embodiments, the Portland cement is ordinary Portland cement. Preferably, the Portland cement is ordinary Portland cement, and the strength grade is 42.5. The use of PO 42.5 cement not only ensures a certain physical strength, but also has fast early strength development and good durability, and is conducive to simplifying the preparation method of steel slag powder composite waste glass mortar without the need for complex equipment and technical support.
[0038] Red mud is the waste residue produced in the process of producing alumina from bauxite. It has a complex chemical composition, mainly including aluminum oxide, iron oxide, titanium oxide, calcium oxide, silicon dioxide and sodium oxide. In addition, it also contains some rare metal elements, such as scandium, gallium, vanadium, etc. The exemplary weight parts of the red mud are 0.6 parts, 0.8 parts, 1.0 parts, and 1.2 parts. Preferably, the weight parts of red mud are 0.6 to 1 parts. In some embodiments, the total mass content of aluminum oxide and iron oxide in the red mud is ≥30%. The oxides contained in the red mud react with the hydration products in the cement to form a dense gel system with a volcanic ash effect, which helps to improve the working performance and impermeability of cement mortar.
[0039] The standard sand is quartz sand, and the exemplary weight parts of the standard sand are 16 parts, 17 parts, 18 parts, 19 parts, and 20 parts. Preferably, the weight parts of the standard sand are 17 to 19 parts. The particle size distribution of the standard sand is uniform, the particle shape is good, the surface roughness is low, the density is large, the wear resistance is good, and it has certain strength, flexibility and stability. Adding an appropriate amount of standard sand is conducive to improving the physical strength of the finished product.
[0040] Finally, a certain amount of water is added to ensure uniform mixing and chemical reaction during the preparation process, and exemplary weight parts of water are 4 parts, 5 parts, and 6 parts, preferably, the weight part of water is 5 parts. Adding water within the above range can promote the hydration reaction of cement, improve the workability and fluidity of mortar, and improve preparation efficiency.
[0041] Accordingly, the present invention also provides a method for preparing steel slag powder composite waste glass mortar, such as Figure 1 As shown, the following steps are included:
[0042] S1, mixing silicate cement, standard sand, waste glass powder and steel slag powder and stirring to obtain a dry material component;
[0043] The amounts of silicate cement, standard sand, waste glass powder and steel slag powder added are as described above and will not be repeated here.
[0044] In some embodiments, silicate cement, standard sand, waste glass powder, and steel slag powder are mixed and stirred for 200s to 300s to obtain a dry material component.
[0045] S2, mixing red mud and water and stirring to obtain a mixed solution;
[0046] The amounts of red mud and water added are as described above and will not be repeated here.
[0047] S3, pouring the dry material components into the mixed liquid and stirring evenly to obtain steel slag powder composite waste glass mortar.
[0048] In some embodiments, the dry ingredients are poured into the mixed solution and stirred for 500s to 600s.
[0049] The preparation method provided by the present invention has a simple process, and the implementation process does not require complicated equipment and technical support. After the steel slag powder composite waste glass mortar is prepared, a cube axial compressive strength test, a flexural strength test, and an expansion rate test are carried out. Among them, the compressive strength test makes the mortar into a test block of 50mm*50mm*50mm, the flexural strength test makes the mortar into a test block of 40mm*40mm*160mm, and the expansion rate test makes the mortar into a test piece of 25mm*25mm*280mm. The prepared mortar has good compressive and flexural strength, and a low expansion rate. It shows that the steel slag powder composite waste glass mortar can be used in cement mortar.
[0050] The present invention is further described below with reference to specific embodiments.
[0051] Example 1
[0052] The present embodiment provides a steel slag powder composite waste glass mortar, which includes the following components in parts by weight: 5 parts of waste glass powder, 1.5 parts of steel slag powder, 10 parts of silicate cement, 18 parts of standard sand, 0.5 parts of red mud, and 5 parts of water.
[0053] The average particle size of the waste glass powder is 80 μm, and the average particle size of the steel slag powder is 5 μm.
[0054] The method for preparing the steel slag powder composite waste glass mortar in this embodiment comprises the following steps:
[0055] S1. Mix ordinary Portland cement, standard sand, waste glass powder and steel slag powder according to the above weight parts, and stir for 200 seconds to obtain a dry material component;
[0056] S2, mixing red mud and water in the above parts by weight to obtain a mixed solution;
[0057] S3. Pour the dry material components into the mixed liquid and stir evenly for 500 seconds to obtain steel slag powder composite waste glass mortar.
[0058] Example 2
[0059] The present embodiment provides a steel slag powder composite waste glass mortar, which includes the following components in parts by weight: 5 parts of waste glass powder, 4.5 parts of steel slag powder, 10 parts of silicate cement, 18 parts of standard sand, 1 part of red mud, and 5 parts of water.
[0060] The average particle size of the waste glass powder is 80 μm, and the average particle size of the steel slag powder is 4 μm.
[0061] The method for preparing the steel slag powder composite waste glass mortar in this embodiment comprises the following steps:
[0062] S1. Mix ordinary Portland cement, standard sand, waste glass powder and steel slag powder according to the above weight parts, and stir for 250 seconds to obtain a dry material component;
[0063] S2, mixing red mud and water in the above parts by weight to obtain a mixed solution;
[0064] S3. Pour the dry material components into the mixed liquid and stir evenly for 550 seconds to obtain steel slag powder composite waste glass mortar.
[0065] Example 3
[0066] The present embodiment provides a steel slag powder composite waste glass mortar, which includes the following components in parts by weight: 5 parts of waste glass powder, 5.5 parts of steel slag powder, 10 parts of silicate cement, 18 parts of standard sand, 0.5 parts of red mud, and 5 parts of water.
[0067] The average particle size of the waste glass powder is 80 μm, and the average particle size of the steel slag powder is 4 μm.
[0068] The method for preparing the steel slag powder composite waste glass mortar in this embodiment comprises the following steps:
[0069] S1. Mix ordinary Portland cement, standard sand, waste glass powder and steel slag powder according to the above weight parts, and stir for 300 seconds to obtain a dry material component;
[0070] S2, mixing red mud and water in the above parts by weight to obtain a mixed solution;
[0071] S3. Pour the dry material components into the mixed liquid and stir evenly for 600 seconds to obtain steel slag powder composite waste glass mortar.
[0072] Example 4
[0073] The present embodiment provides a steel slag powder composite waste glass mortar, which includes the following components in parts by weight: 5 parts of waste glass powder, 3.5 parts of steel slag powder, 10 parts of silicate cement, 16 parts of standard sand, 0.5 parts of red mud, and 5 parts of water.
[0074] The average particle size of the waste glass powder is 80 μm, and the average particle size of the steel slag powder is 4 μm.
[0075] The SiO2 content of the waste glass powder is ≥60%, the CaO content of the steel slag powder is ≥40%, the SiO2 content is ≥13%, the Fe2O3 content is ≥20%, and the free CaO content is ≤3.0%.
[0076] The method for preparing the steel slag powder composite waste glass mortar in this embodiment comprises the following steps:
[0077] S1. Mix ordinary Portland cement, standard sand, waste glass powder and steel slag powder according to the above weight parts, and stir for 200 seconds to obtain a dry material component;
[0078] S2, mixing red mud and water in the above parts by weight to obtain a mixed solution;
[0079] S3. Pour the dry material components into the mixed liquid and stir evenly for 500 seconds to obtain steel slag powder composite waste glass mortar.
[0080] Example 5
[0081] The present embodiment provides a steel slag powder composite waste glass mortar, which includes the following components in parts by weight: 5 parts of waste glass powder, 3.5 parts of steel slag powder, 10 parts of silicate cement, 16 parts of standard sand, 1 part of red mud, and 5 parts of water.
[0082] The average particle size of the waste glass powder is 80 μm, and the average particle size of the steel slag powder is 4 μm.
[0083] The method for preparing the steel slag powder composite waste glass mortar in this embodiment comprises the following steps:
[0084] S1. Mix ordinary Portland cement, standard sand, waste glass powder and steel slag powder according to the above weight parts, and stir for 250 seconds to obtain a dry material component;
[0085] S2, mixing red mud and water in the above parts by weight to obtain a mixed solution;
[0086] S3. Pour the dry material components into the mixed liquid and stir evenly for 550 seconds to obtain steel slag powder composite waste glass mortar.
[0087] Example 6
[0088] The present embodiment provides a steel slag powder composite waste glass mortar, which includes the following components in parts by weight: 5 parts of waste glass powder, 5.5 parts of steel slag powder, 10 parts of silicate cement, 16 parts of standard sand, 0.5 parts of red mud, and 5 parts of water.
[0089] The average particle size of the waste glass powder is 80 μm, and the average particle size of the steel slag powder is 4 μm.
[0090] The method for preparing the steel slag powder composite waste glass mortar in this embodiment comprises the following steps:
[0091] S1. Mix ordinary Portland cement, standard sand, waste glass powder and steel slag powder according to the above weight parts, and stir for 300 seconds to obtain a dry material component;
[0092] S2, mixing red mud and water in the above parts by weight to obtain a mixed solution;
[0093] S3. Pour the dry material components into the mixed liquid and stir evenly for 600 seconds to obtain steel slag powder composite waste glass mortar.
[0094] Example 7
[0095] The present embodiment provides a steel slag powder composite waste glass mortar, which includes the following components in parts by weight: 5 parts of waste glass powder, 4.5 parts of steel slag powder, 10 parts of silicate cement, 18 parts of standard sand, 0.5 parts of red mud, and 5 parts of water.
[0096] The average particle size of the waste glass powder is 300 μm, and the average particle size of the steel slag powder is 4 μm.
[0097] The method for preparing the steel slag powder composite waste glass mortar in this embodiment comprises the following steps:
[0098] S1. Mix ordinary Portland cement, standard sand, waste glass powder and steel slag powder according to the above weight parts, and stir for 200 seconds to obtain a dry material component;
[0099] S2, mixing red mud and water in the above parts by weight to obtain a mixed solution;
[0100] S3. Pour the dry material components into the mixed liquid and stir evenly for 500 seconds to obtain steel slag powder composite waste glass mortar.
[0101] Comparative Example 1
[0102] This comparative example provides a mortar, which includes the following components by weight: 10 parts of Portland cement, 18 parts of standard sand, and 5 parts of water. The preparation method thereof includes the following steps:
[0103] S1. Mix ordinary Portland cement and standard sand according to the above weight parts, stir for 200 seconds, and obtain a dry material component;
[0104] S3. Pour the dry components into water and stir evenly for 500 seconds to obtain mortar.
[0105] According to the Standard for Test Methods for Mechanical Properties of Ordinary Concrete (GB / T 50081-200), the mortars prepared in Examples 1 to 7 and Comparative Example 1 were subjected to cube axial compressive strength tests, flexural strength tests, and expansion rate tests. For the compressive strength test, the mortar was made into a 50mm*50mm*50mm test block, for the flexural strength test, the mortar was made into a 40mm*40mm*160mm test block, and for the expansion rate test, the mortar was made into a 25mm*25mm*280mm test piece. The results of the compressive test, flexural test, and expansion rate test of the mortars prepared in Examples 1 to 7 of the present invention and Comparative Example 1 are shown in Table 1.
[0106] Table 1 Compression test, flexural test and expansion rate test results of mortar prepared in Examples 1 to 7 and Comparative Example 1
[0107]
[0108] As shown in Table 1, Example 4 exhibits the best comprehensive strength and durability. According to the preparation method of Example 4, the prepared mortar sample has a compressive strength of 36.28 MPa, a flexural strength of 8.93 MPa, and an expansion rate of 0.0594% at 28 days.
[0109] The results of the comparative experiment show that the compressive and flexural strengths of the mortar sample of Example 1 are improved compared with those of Comparative Example 1, and the expansion rate is lower than the standard threshold. The oxides and silicates contained in steel slag, waste glass and red mud react with the hydration products in cement to form a dense gel system with a volcanic ash effect, thereby improving the compressive and flexural strengths of the mortar.
[0110] By comparing the test data of Example 1 and Example 7, it is found that under the same dosage of chemical reagent, the bending and compressive strengths of the mortar are improved and the expansion rate is reduced when 80 micron glass powder is added than when 300 micron glass powder is added.
[0111] In addition, Examples 1 to 3 show that the waste glass mortar prepared by the scheme of the present invention has good compressive and flexural strength, and the expansion rate is lower than the standard threshold. In these experiments, the mortar prepared by Example 4 showed the best comprehensive strength and durability, highlighting the environmental significance and practicality of the method of the present invention.
[0112] In the description of this specification, the description with reference to the terms "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiments or examples are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0113] The above disclosure is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.
Claims
1. A steel slag powder composite waste glass mortar, characterized in that: The invention comprises the following components in parts by weight: 3-7 parts of waste glass powder, 2-6 parts of steel slag powder, 8-10 parts of silicate cement, 16-20 parts of standard sand, 0.5-1.2 parts of red mud and 4-6 parts of water.
2. The steel slag powder composite waste glass mortar according to claim 1, characterized in that: The invention comprises the following components in parts by weight: 4-6 parts of waste glass powder, 3-5 parts of steel slag powder, 8-9 parts of silicate cement, 17-19 parts of standard sand, 0.6-1 part of red mud and 4-6 parts of water.
3. The steel slag powder composite waste glass mortar according to claim 1, characterized in that: The average particle size of the waste glass powder is 80 μm to 300 μm; The SiO2 content of the waste glass powder is ≥60%.
4. The steel slag powder composite waste glass mortar according to claim 1, characterized in that: The average particle size of the steel slag powder is 0.8 μm to 12 μm; The steel slag powder has a CaO content of ≥40%, a SiO2 content of ≥13%, a Fe2O3 content of ≥20%, and a free CaO content of ≤3.0%.
5. The steel slag powder composite waste glass mortar according to claim 1, characterized in that: The silicate cement is ordinary silicate cement.
6. The steel slag powder composite waste glass mortar according to claim 1, characterized in that: The total mass content of aluminum oxide and iron oxide in the red mud is ≥30%.
7. A method for preparing steel slag powder composite waste glass mortar according to any one of claims 1 to 6, characterized in that: The following steps are involved: Mixing silicate cement, standard sand, waste glass powder and steel slag powder and stirring to obtain a dry material component; The red mud and water are mixed and stirred to obtain a mixed liquid; Pour the dry material components into the mixed liquid and stir evenly to obtain steel slag powder composite waste glass mortar.
8. The method for preparing the steel slag powder composite waste glass mortar according to claim 7, characterized in that: The silicate cement, standard sand, waste glass powder and steel slag powder are mixed and stirred for 200s to 300s to obtain a dry material component.
9. The method for preparing the steel slag powder composite waste glass mortar according to claim 7, characterized in that: Pour the dry ingredients into the mixed liquid and stir for 500s to 600s.
10. Use of the steel slag powder composite waste glass mortar as claimed in any one of claims 1 to 6 in cement mortar.
Citation Information
Patent Citations
Waste glass mortar and preparation method thereof
CN112979251A
Preparation method of waste glass mortar and waste glass mortar
CN113880515A
Cited By
Ceramsite with core-shell structure as well as preparation method and application of ceramsite
CN120518344A