Ceramic material, ceramic slurry and preparation method and application thereof

By using ceramic solid solution and sintering additive formed by large and small ions rare earth ions and magnesium ions in ceramic capacitors, combined with MnO2 and V2O5, the problem of insufficient dielectric constant and reliability of ceramic capacitors is solved, and high dielectric constant and Comply with the temperature characteristics of EIA standard X7R.

CN119019170AActive Publication Date: 2024-11-26NANCHONG THREE CIRCLE ELECTRONICS +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411076882.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-26
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The dielectric constant of existing ceramic capacitors is difficult to meet the high capacity requirements, and there are high temperature coefficients and dielectric losses, as well as differences in DC bias characteristics.

Method used

A type of ceramic solid solution formed by large ion radius rare earth ions and magnesium ions and barium titanate, a type of ceramic solid solution formed by small ion radius rare earth ions and magnesium ions and barium titanate, combined with MnO2 and V2O5, by regulating rare earth ions and magnesium The amount of ions and the content of ceramic solid solution form ceramic materials to improve dielectric constant and reliability, and meet the EIA standard X7R characteristics.

Benefits of technology

It realizes high dielectric constant and high reliability of ceramic capacitors, and its temperature characteristics comply with EIA standard X7R, improving the performance and stability of the capacitor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004982567450000091
    Figure BDA0004982567450000091
  • Figure BDA0004982567450000101
    Figure BDA0004982567450000101
  • Figure BDA0004982567450000102
    Figure BDA0004982567450000102
Patent Text Reader

Abstract

The invention relates to a ceramic material, ceramic slurry and a preparation method and application thereof, and belongs to the technical field of capacitors. The ceramic material disclosed by the invention comprises a first-class ceramic solid solution (A1 < x > A < 2 > y > B < 1 > z > B < 2 > w O < 3 >), a second-class ceramic solid solution (A < 3 > B < 3 > alpha > B < 4 > beta > B < 5 > gamma O < 3 >), MnO2, V2O5 and a sintering aid (at least comprising CaO, Li2O and SiO2). According to the ceramic material, the ceramic capacitor has high dielectric constant and high reliability, and the temperature characteristic meets the EIA standard X7R characteristic.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of capacitors, and in particular to a ceramic material, a ceramic slurry, and a preparation method and application thereof. Background Art

[0002] Chip multilayer ceramic capacitors (MLCC) have the advantages of high precision, high integration, and low power consumption, and are widely used in consumer electronics, automobiles, home appliances, new energy and other fields. In recent years, with the miniaturization and high performance of electronic equipment, the demand for miniaturized and large-capacity multilayer ceramic capacitors has been increasing. At present, miniaturization and high capacity are mainly achieved by thinning the dielectric layer of MLCC and increasing the number of layers. Ceramic powder is the key material for preparing the dielectric layer, and barium titanate ceramic powder is currently widely used. Barium titanate (BaTiO3) is a typical ABO3 type perovskite structure. The Curie temperature of pure barium titanate is about 125°C. The dielectric constant of pure barium titanate with a particle size of about 200nm at room temperature is only about 1700. This dielectric constant is difficult to meet the use requirements of thin-film high-capacity products. Although the room temperature dielectric constant of barium titanate can be increased to more than 4000 through different synthesis methods and control of grain size, it still has defects such as high temperature coefficient, high dielectric loss and poor DC bias characteristics. Summary of the invention

[0003] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a ceramic material and a preparation method and application thereof.

[0004] To achieve the above object, the technical solution adopted by the present invention is:

[0005] In a first aspect, the present invention provides a ceramic material, which includes a first type of ceramic solid solution, a second type of ceramic solid solution, MnO2, V2O5 and a sintering aid;

[0006] The general chemical formula of the ceramic solid solution is A 1 x A 2 y B 1 z B 2 w O3,

[0007] Where 0.01≤x≤0.1, 0.005≤w≤0.02; A 1 is at least one of La, Gd, Pr, Sm, and Ce, A 2 for Ba,B 1 Ti, B 2 Mg;

[0008] The chemical formula of the second type of ceramic solid solution is A3 B 3 α B 4 β B 5 γ O3,

[0009] Where 0.005≤α≤0.05, 0.001≤β≤0.005; A 3 for Ba,B 3 is at least one of Er, Tm, Yb, Lu, and Sc, B 4 Mg, B 5 is Ti;

[0010] The sintering aid includes at least CaO, Li2O and SiO2.

[0011] The present invention combines a first type of ceramic solid solution formed by rare earth ions with large ionic radius and magnesium ions and barium titanate, a second type of ceramic solid solution formed by rare earth ions with small ionic radius and magnesium ions and barium titanate, and a specific sintering aid, and is matched with MnO2 and V2O5 to form a ceramic material. By regulating the amount of rare earth ions with large ionic radius and magnesium ions in the first type of ceramic solid solution, the amount of rare earth ions with small ionic radius and magnesium ions in the second type of ceramic solid solution, and the content of the first type of ceramic solid solution and the second type of ceramic solid solution in the ceramic material, a ceramic capacitor using the ceramic material as a ceramic dielectric raw material has both high dielectric constant and high reliability, and the temperature characteristics meet the EIA standard X7R characteristics.

[0012] The weight percentages of the first type of ceramic solid solution and the second type of ceramic solid solution in the ceramic material of the present invention play a key role in the dielectric constant, temperature characteristics and reliability of the ceramic capacitor; wherein, the substitution of rare earth ions for the B position (i.e., Ti position) of BaTiO3 will increase the volume of the BaTiO3 unit cell in the grain shell, and cause the grain shell to expand in volume relative to the grain core during the process of the sintering temperature dropping to room temperature, exerting tension on the grain core, thereby promoting the increase of the Curie temperature (Tc) point of the BaTiO3 grain core; and the substitution of rare earth ions for the A position (i.e., Ba position) of BaTiO3 will exert compressive stress on the BaTiO3 grain core, thereby lowering its Curie temperature point.

[0013] Rare earth ions with large ionic radius tend to replace the A position of BaTiO3, causing the Tc point of the ceramic solid solution to move to low temperature, thereby improving the dielectric constant of the ceramic solid solution at room temperature, but too much A-position substitution will lead to abnormal growth of grains and deterioration of the temperature stability characteristics of ceramic capacitors. Rare earth ions with small ionic radius tend to replace the B position of BaTiO3, causing the Tc point of the ceramic solid solution to move to high temperature, thereby improving the TCC of ceramic capacitors. In addition, due to the low diffusion rate of small-radius rare earth ions, they tend to be unevenly distributed in the grain boundaries and grain shell regions of the ceramic solid solution, thereby better preventing grain growth to increase the insulation breakdown time, thereby improving the reliability of ceramic capacitors.

[0014] The rare earth ions in the first type of ceramic solid solution or the second type of ceramic solid solution exist simultaneously in the grain boundaries and grains of the ceramic solid solution, thereby improving the life characteristics of the ceramic capacitor during high temperature loading to improve its reliability. However, when the content of rare earth ions in the ceramic solid solution is too small, it is difficult to fully improve the reliability of the ceramic capacitor; and when the content of rare earth ions in the ceramic solid solution is too high, the sintering characteristics of the ceramic solid solution during the sintering process will deteriorate, which will in turn reduce the reliability of the ceramic capacitor.

[0015] For a type of ceramic solid solution A 1 x A 2 y B 1 z B 2 w O3, large radius rare earth ion A 1 The diffusion rate in BaTiO3 is faster, which easily leads to grain growth; at the same time, it will diffuse deeply into the BaTiO3 grains, thereby destroying the formation of the grain shell and eventually becoming chemically uniform grains (i.e., unable to form a core-shell structure). Therefore, large-radius rare earth ions require more magnesium ions than small-radius rare earth ions to inhibit the growth of BaTiO3 grains and form a complete core-shell structure.

[0016] The study found that A 1 x A 2 y B 1 z B 2 wThe appropriate value range of x in O3 is 0.01≤x≤0.1. When x<0.01, it is not conducive to the solid dissolution of rare earth ions into BaTiO3 to form a complete shell, thereby accelerating the deterioration of the life of the ceramic capacitor; when x>0.1, too much rare earth ions will be dissolved into BaTiO3, resulting in a decrease in the dielectric constant of the ceramic solid solution and a decrease in sintering activity. Optionally, the above x can be 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09.

[0017] A 1 x A 2 y B 1 z B 2 w The appropriate value range of w in O3 is 0.005≤w≤0.02. When w<0.005, it is impossible to inhibit the diffusion of rare earth ions into the interior of BaTiO3, which results in the inability of the ceramic solid solution to form a complete core-shell structure, and further leads to the deterioration of the TCC of the ceramic capacitor; when w>0.02, excessive magnesium content strongly inhibits grain growth, which is not conducive to the sintering and densification of the ceramic solid solution. Optionally, the above w can be 0.006, 0.007, 0.008, 0.009, 0.01, 0.011, 0.012, 0.013, 0.014, 0.015, 0.016, 0.017, 0.018, 0.019.

[0018] In addition, A 1 x A 2 y B 1 z B 2 w In O3, z and w satisfy: z+w=1, x and y satisfy: 0.96≤x+y≤1.015; optionally, the value range of y can be 0.86-1.005, specifically 0.865, 0.895, 0.915, 0.93, 0.935, 0.94, 0.945, 0.955, 0.98, 0.985, 0.99, 0.995, 1; the value range of z can be 0.98-0.995, specifically 0.982, 0.984, 0.986, 0.988, 0.99, 0.992, 0.994.

[0019] For the second type of ceramic solid solution A 3 B 3 α B 4 β B 5 γO3, rare earth ion B with small ionic radius 3 And magnesium ions replace the B-site of BaTiO3 to become acceptor ions. The addition of acceptor ions can improve the reduction resistance, but excessive acceptor ions will form a large number of oxygen vacancies. The electrical migration of these charged oxygen vacancies under high temperature and high pressure will lead to a decrease in insulation, thereby deteriorating the reliability of ceramic capacitors.

[0020] The study found that A 3 B 3 α B 4 β B 5 γ The appropriate value range of α in O3 is 0.005≤α≤0.05. When α<0.005, it is not conducive to the formation of a complete shell of the ceramic solid solution, and it is difficult for small-radius rare earth ions to effectively dissolve into BaTiO3, which has a poor effect on improving the TCC of ceramic capacitors; when α>0.05, excessive acceptor ions will form a large number of oxygen vacancies, which will lead to the deterioration of the insulation resistance and reliability of ceramic capacitors under high temperature and high pressure. Optionally, the above α can be 0.01, 0.015, 0.02, 0.025, 0.03, 0.035, 0.04, 0.045.

[0021] A 3 B 3 α B 4 β B 5 γ The appropriate value range of β in BaTiO3 is 0.001≤β≤0.005. When β<0.001, the diffusion of rare earth ions into BaTiO3 cannot be suppressed, resulting in the inability of the ceramic solid solution to form a complete core-shell structure, which in turn leads to the deterioration of the TCC of the ceramic capacitor; when β>0.005, the diffusion of magnesium ions and rare earth ions with small ion radius in BaTiO3 is relatively slow, and since magnesium ions diffuse into BaTiO3 before rare earth ions with small ion radius during the solid solution process, excessive magnesium ions will cause the rare earth ions with small radius to be unable to be completely dissolved into BaTiO3, which in turn leads to poor improvement of the TCC of the ceramic capacitor. Optionally, the above β can be 0.002, 0.003, or 0.004.

[0022] In addition, the above A 3 B 3 α B 4 β B 5 γIn O3, α, β and γ satisfy: (1+α) / (β+γ)=1.006~1.090; optionally, the value range of γ is 0.96~0.9958, specifically 0.961, 0.962, 0.969, 0.977, 0.99, 0.991, 0.9915, 0.992, 0.9938.

[0023] Optionally, the weight percentage of the first type of ceramic solid solution in the above-mentioned ceramic material is 50% to 85%, and the weight percentage of the second type of ceramic solid solution is 12% to 35%; the above-mentioned sintering aid includes at least CaO, Li2O and SiO2, and may also include aluminum oxide, boron oxide, etc.

[0024] As a preferred embodiment of the ceramic material of the present invention, the ceramic material includes the following components, calculated by weight percentage: 50% to 85% of a type I ceramic solid solution, 12% to 35% of a type II ceramic solid solution, 0.1% to 5% of MnO2, 0.1% to 3% of V2O5, and 2.4% to 15% of a sintering aid.

[0025] Optionally, the weight percentage of the first type of ceramic solid solution can be 55%, 57%, 60%, 63%, 65%, 67%, 70%, 72%, 75%, 78%, 80%; the weight percentage of the second type of ceramic solid solution can be 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28%, 30%, 32%, 34%; the weight percentage of MnO2 can be 0.5%. , 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%; the weight percentage of V2O5 can be specifically 0.3%, 0.6%, 0.9%, 1.2%, 1.5%, 1.8%, 2.1%, 2.4%, 2.7%; the weight percentage of sintering aid can be specifically 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%.

[0026] As a preferred embodiment of the ceramic material of the present invention, the ceramic material includes the following components by weight percentage: 60% to 75% of a type I ceramic solid solution, 18% to 30% of a type II ceramic solid solution, 0.5% to 3.5% of MnO2, 0.8% to 2% of V2O5, and 6% to 10% of a sintering aid.

[0027] More preferably, the ceramic material comprises the following components by weight: 70% of a first type of ceramic solid solution, 20% of a second type of ceramic solid solution, 1.5% of MnO2, 1.2% of V2O5 and 7.3% of a sintering aid.

[0028] As a preferred embodiment of the ceramic material of the present invention, the CaO accounts for 10% to 30% of the total weight of the sintering aid, and the Li2O accounts for 10% to 30% of the total weight of the sintering aid.

[0029] The CaO in the above sintering aid has the function of regulating A(Ca,Ba) / B(Ti). Properly increasing the ratio of A / B is beneficial to improving the insulation resistance of ceramic capacitors, but too high a ratio of A / B will lead to too high a sintering temperature of the ceramic material; while Li2O and SiO2 are easy to form a liquid phase during the sintering process of the ceramic material, which can reduce the sintering temperature. When the weight percentage of CaO in the sintering aid is too large, the sintering temperature of the ceramic material is too high, and when its weight percentage is too small, it is difficult to play the role of regulating A(Ca,Ba) / B(Ti); when the weight percentage of Li2O in the sintering aid is too small, the sintering characteristics of the ceramic material will deteriorate, and when the weight percentage is too large, Li2O is easy to react with Mg in the ceramic solid solution to produce a secondary phase.

[0030] Preferably, SiO2 in the above sintering aid accounts for 40% to 80% of the total weight of the sintering aid. When the weight percentage of SiO2 is within this range, it can not only better reduce the sintering temperature of the ceramic material, but also more effectively prevent the ceramic material from generating secondary phases.

[0031] Optionally, the weight percentage of CaO in the above-mentioned sintering aid can be 15%, 20%, or 25%, the weight percentage of Li2O can be 15%, 20%, or 25%, and the weight percentage of SiO2 can be 45%, 50%, 55%, 60%, 65%, 70%, or 75%.

[0032] As a preferred embodiment of the ceramic material of the present invention, the ceramic solid solution is prepared by the following preparation method: 1 x A 2 y B 1 z B 2 w The stoichiometric ratio of each element in O3 is 1 Oxide, B 2 The oxide and BaTiO3 are ball-milled for 15 to 20 hours, and then calcined at 1000 to 1050° C. for 3 to 5 hours in an air atmosphere. Optionally, the ball-milling time can be 16 hours, 17 hours, 18 hours, or 19 hours, the calcination temperature can be 1010° C., 1020° C., 1030° C., or 1040° C., and the calcination time can be 3.5 hours, 4 hours, or 4.5 hours.

[0033] As a preferred embodiment of the ceramic material of the present invention, the second type of ceramic solid solution is prepared by the following preparation method: according to the chemical formula A 3 B 3 α B 4 β B 5 γ The stoichiometric ratio of each element in O3 is 3 Oxide, B 4 The oxide and BaTiO3 are ball-milled for 15 to 20 hours, and then calcined at 1050 to 1100° C. for 3 to 5 hours in an air atmosphere. Optionally, the ball-milling time can be 16 hours, 17 hours, 18 hours, or 19 hours, the calcination temperature can be 1060° C., 1070° C., 1080° C., or 1090° C., and the calcination time can be 3.5 hours, 4 hours, or 4.5 hours.

[0034] The ball milling in the preparation method of the first type of ceramic solid solution or the second type of ceramic solid solution refers to wet grinding using a ball mill. In addition, the first type of ceramic solid solution or the second type of ceramic solid solution obtained by roasting in the above preparation method can be further wet-milled using a ball mill, and the ball milling time is 20 to 30 hours and the ball milling speed is 100 to 150 rpm.

[0035] In a second aspect, the present invention provides a method for preparing the above-mentioned ceramic material, which comprises the following steps: uniformly mixing a type I ceramic solid solution, a type II ceramic solid solution, MnO2, V2O5 and a sintering aid to obtain a ceramic material.

[0036] In a third aspect, the present invention provides a ceramic slurry, which includes ceramic powder, an organic solvent and a binder, wherein the ceramic powder is the above-mentioned ceramic material.

[0037] As a preferred embodiment of the ceramic slurry of the present invention, the weight percentage of the organic solvent relative to the ceramic powder is 80% to 85%; the weight percentage of the binder relative to the ceramic powder is 7% to 9%.

[0038] As a preferred embodiment of the ceramic slurry of the present invention, the organic solvent includes at least one of toluene and ethanol; the binder includes at least one of polyvinyl butyral and polyacrylic acid.

[0039] As a preferred embodiment of the ceramic slurry described in the present invention, the ceramic slurry can be prepared by the following preparation method: ceramic powder, organic solvent and binder are added into a ball mill for wet mixing and dispersion to obtain ceramic slurry; wherein, the ball milling time is about 40 to 50 hours, the ball milling rate is 150 to 200 rpm, and the ball milling medium is zirconia balls (with a diameter of 2 to 4 mm and an addition amount of 10 to 12 times the mass of the ceramic powder).

[0040] In a fourth aspect, the present invention provides a chip-type multilayer ceramic capacitor including a ceramic dielectric made from the above ceramic slurry.

[0041] Compared with the prior art, the present invention has the following beneficial effects:

[0042] The present invention combines a first type of ceramic solid solution formed by rare earth ions with large ionic radius and magnesium ions and barium titanate, a second type of ceramic solid solution formed by rare earth ions with small ionic radius and magnesium ions and barium titanate, and a specific sintering aid, and is matched with MnO2 and V2O5 to form a ceramic material. By regulating the amount of rare earth ions with large ionic radius and magnesium ions in the first type of ceramic solid solution, the amount of rare earth ions with small ionic radius and magnesium ions in the second type of ceramic solid solution, and the content of the first type of ceramic solid solution and the second type of ceramic solid solution in the ceramic material, a ceramic capacitor using the ceramic material as a ceramic dielectric raw material has both high dielectric constant and high reliability, and the temperature characteristics meet the EIA standard X7R characteristics. DETAILED DESCRIPTION

[0043] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0044] Unless otherwise specified, other materials, reagents, etc. used in the examples and comparative examples can be obtained from commercial sources.

[0045] 1. A type of ceramic solid solution (A 1 x A 2 y B 1 z B 2 w O3, A 1 A is a rare earth element. 2 for Ba,B 1 Ti, B 2 Mg)

[0046] Table 1A 1 x A 2 y B 1 z B 2 w Rare Earth Element A in O3 1 The type and values ​​of x, y, z, and w

[0047] serial number <![CDATA[A 1 ]]> x y z w C1 La 0.01 1.005 0.98 0.02 C2 La 0.01 0.99 0.995 0.005 C3 La 0.01 1 0.985 0.015 C4 La 0.01 0.995 0.99 0.01 C5 La 0.02 0.98 0.99 0.01 C6 La 0.05 0.935 0.99 0.01 C7 La 0.1 0.86 0.99 0.01 C8 La 0.08 0.895 0.985 0.015 C9 La 0.02 0.985 0.985 0.015 C10 La 0.05 0.94 0.985 0.015 C11 La 0.1 0.865 0.985 0.015 C12 La 0.05 0.945 0.98 0.02 C13 La 0.05 0.93 0.995 0.005 C14 La 0.02 0.99 0.98 0.02 C15 La 0.06 0.915 0.995 0.005 C16 La 0.04 0.955 0.985 0.015 C17 La 0 1.015 0.985 0.015 C18 La 0.5 0.265 0.985 0.015 C19 La 0.01 0.985 1 0 C20 La 0.01 1.035 0.95 0.05 C21 G 0.05 0.94 0.985 0.015 C22 Pr 0.05 0.94 0.985 0.015 C23 Sm 0.05 0.94 0.985 0.015 C24 Ce 0.05 0.94 0.985 0.015

[0048] The preparation method of the above-mentioned ceramic solid solution comprises the following steps:

[0049] According to the ratio in Table 1, 1 Oxide, B 2 The oxide and BaTiO3 ceramic powder are wet-mixed by ball milling for about 15 hours, dried, calcined at 1000°C in air for 4 hours, and then wet-milled by a ball mill for about 20 hours (the ball milling speed is 110 rpm) to obtain a type of ceramic solid solution powder.

[0050] 2. Type II ceramic solid solution (A 3 B 3 α B 4 β B 5 γ O3, A 3 for Ba,B 3 For rare earth elements, B 4 Mg, B 5 Ti

[0051] Table 2A 3 B 3 α B 4 β B 5 γ Rare earth element B in O3 3 The type and value of α, β and γ

[0052] serial number <![CDATA[B 3 ]]> α β γ E1 Lu 0.005 0.005 0.9938 E2 Lu 0.05 0.001 0.9620 E3 Lu 0.01 0.001 0.9920 E4 Lu 0.03 0.001 0.9770 E5 Lu 0.04 0.002 0.9690 E6 Lu 0.01 0.003 0.9910 E7 Lu 0.01 0.005 0.9900 E8 Lu 0.01 0.002 0.9915 E9 Lu 0.05 0.003 0.9610 E10 Lu 0.005 0.001 0.9958 E11 Lu 0.05 0.005 0.9600 E12 Lu 0 0.003 0.9985 E13 Lu 0.08 0.003 0.9385 E14 Lu 0.03 0 0.9775 E15 Lu 0.03 0.01 0.9725 E16 Tm 0.01 0.003 0.9910 E17 Yb 0.01 0.003 0.9910 E18 Er 0.01 0.003 0.9910 E19 Sc 0.01 0.003 0.9910

[0053] The preparation method of the above two types of ceramic solid solutions comprises the following steps:

[0054] According to the ratio in Table 2, 3 Oxide, B 4 The oxide and BaTiO3 ceramic powder are wet-mixed by ball milling for about 15 hours, dried, calcined at 1050°C in air for 4 hours, and then wet-milled by a ball mill for about 25 hours (the ball milling speed is 110 rpm) to obtain the second type of ceramic solid solution powder.

[0055] 3. Sintering aid (aCaO-bLi2O-cSiO2, a is the weight percentage of CaO in the sintering aid, b is the weight percentage of Li2O in the sintering aid, c is the weight percentage of SiO2 in the sintering aid)

[0056] Table 3 Weight percentage of CaO, Li2O and SiO2 in sintering aids

[0057] serial number a / % b / % c / % F1 10 10 80 F2 20 20 60 F3 30 30 40 F4 20 30 50 F5 15 15 70 F6 / 20 80 F7 5 30 65 F8 40 10 50 F9 20 / 80 F10 30 5 65 F11 10 40 50 F12 50 50 / F13 / / 100

[0058] The preparation method of the sintering aid comprises the following steps:

[0059] According to the ratio in Table 3, CaO, Li2O and SiO2 are mixed evenly to obtain a sintering aid.

[0060] 4. Examples 1 to 38 and Comparative Examples 1 to 20

[0061] The formulas of the ceramic materials in Examples 1 to 9 and Comparative Examples 9 to 12 are shown in Table 4.

[0062] Table 4 Formulations of ceramic materials in Examples 1 to 9 and Comparative Examples 9 to 12

[0063]

[0064]

[0065] Examples 10 to 38, Comparative Examples 1 to 8 and Comparative Examples 13 to 20

[0066] The ceramic materials in Examples 8 to 22, Comparative Examples 1 to 8 and Comparative Examples 13 to 38 are basically the same as those in Example 1 (i.e., calculated by weight percentage, they all include 70% of a Class I ceramic solid solution, 20% of a Class II ceramic solid solution, 1.5% of MnO2, 1.2% of V2O5 and 7.3% of a sintering aid). The difference between them is that the Class I ceramic solid solution, the Class II ceramic solid solution and the sintering aid are different, as shown in Table 5.

[0067] Table 5 Formulations of ceramic materials in Examples 1 to 9, Comparative Examples 1 to 8 and Comparative Examples 9 to 12

[0068]

[0069]

[0070]

[0071] The preparation method of the ceramic material comprises the following steps: uniformly mixing a first type ceramic solid solution, a second type ceramic solid solution, MnO2, V2O5 and a sintering aid to obtain the ceramic material.

[0072] 5. Performance Testing

[0073] (1) Ceramic slurry

[0074] The ceramic materials in Examples 1 to 38 and Comparative Examples 1 to 20 are respectively used as ceramic powder, and are evenly mixed with an organic solvent (toluene, whose weight percentage relative to the ceramic powder is 85%) and a binder (polyvinyl butyral, whose weight percentage relative to the binder is 8%) to obtain ceramic slurry.

[0075] The specific preparation method is: add ceramic powder, binder, organic solvent and ball milling medium (2 mm diameter zirconia balls are used as ball milling media, and the added amount is 10 times the mass of ceramic powder) into a ball mill and perform wet mixing and dispersion. The ball milling time is about 40 hours and the ball milling speed is 150 rpm to make a uniform ceramic slurry.

[0076] (2) Multilayer ceramic capacitors

[0077] A method for preparing a multilayer ceramic capacitor comprises the following steps:

[0078] S1, casting the above ceramic slurry into a film with a thickness of 4 μm;

[0079] S2, using a conductive paste for internal electrodes mainly composed of base metal materials such as Ni to form a conductive film pattern on the surface of the film in S1 by screen printing, and then laminating the film with printed electrodes, isostatically pressing it, and cutting it to form a green billet;

[0080] S3, heat-treating the green body in S2 in air (temperature of 200-280°C, time of 10-12h) to remove organic matter inside the green body; then heat-treating the green body in a strong reducing atmosphere (composed of H2-N2-H2O gas, oxygen partial pressure of 10 -11 Pa) and sintered at 1150-1200°C for about 2-4h (heating rate 5-10°C / min) to obtain a ceramic body.

[0081] S4. Cover both ends of the ceramic body in S3 with copper external electrodes to obtain a multi-layer ceramic capacitor.

[0082] (3) Dielectric constant, dielectric loss, reliability and temperature characteristics (TCC) tests

[0083] The above multilayer ceramic capacitor was tested as follows, and the test results are shown in Table 7.

[0084] Table 6 Summary of test contents and their standards

[0085]

[0086]

[0087] Table 7 Performance test data

[0088]

[0089]

[0090]

[0091] According to the data in Table 7, it can be seen that the dielectric constant of the ceramic capacitors made using the ceramic material of the present invention reaches 2633~4082, which is greater than or equal to 2500; at the same time, the dielectric loss reaches 1.52%~2.54%, which is less than or equal to 5%; the reliability is greater than or equal to 1000h, and the temperature change rate of the capacitance in the range of -55℃~125℃ is within ±15%, that is, the ceramic capacitors have excellent performance.

[0092] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A ceramic material, It is characterized in that The ceramic material includes a first type of ceramic solid solution, a second type of ceramic solid solution, MnO 2 、V 2 O 5 and sintering aids; The general chemical formula of the ceramic solid solution is A 1 x A 2 y B 1 z B 2 w O 3 , Where 0.01≤x≤0.1, 0.005≤w≤0.02; A 1 is at least one of La, Gd, Pr, Sm, and Ce, A 2 for Ba, B 1 Ti, B 2 Mg; The chemical formula of the second type of ceramic solid solution is A 3 B 3 α B 4 β B 5 γ O 3 , Where 0.005≤α≤0.05, 0.001≤β≤0.005; A 3 for Ba, B 3 is at least one of Er, Tm, Yb, Lu, and Sc, B 4 Mg, B 5 is Ti; The sintering aid includes at least CaO, Li 2 O and SiO 2 .

2. The ceramic material according to claim 1, It is characterized in that The ceramic solid solution A 1 x A 2 y B 1 z B 2 w O 3 The z and w in satisfy: z+w=1.

3. The ceramic material according to claim 1, It is characterized in that The ceramic solid solution A 1 x A 2 y B 1 z B 2 w O 3 Where x and y satisfy: 0.96≤x+y≤1.

015.

4. The ceramic material according to claim 1, It is characterized in that The second type of ceramic solid solution A 3 B 3 α B 4 β B 5 γ O 3 Among α, β and γ satisfy: (1+α) / (β+γ)=1.006~1.

090.

5. The ceramic material according to claim 1, It is characterized in that The weight percentage of the first type of ceramic solid solution in the ceramic material is 50% to 85%, the weight percentage of the second type of ceramic solid solution is 12% to 35%, and the weight percentage of MnO 2 The weight percentage is 0.1% to 5%, V 2 O 5 The weight percentage of the sintering aid is 0.1% to 3%, and the weight percentage of the sintering aid is 2.4% to 15%.

6. The ceramic material according to any one of claims 1 to 5, It is characterized in that The CaO accounts for 10% to 30% of the total weight of the sintering aid, and the Li 2 O accounts for 10% to 30% of the total weight of the sintering aid.

7. The ceramic material according to claim 1, It is characterized in that The ceramic solid solution is prepared by the following preparation method: according to the chemical formula A 1 x A 2 y B 1 z B 2 w O 3 The stoichiometric ratio of each element in A 1 Oxide, B 2 Oxide and BaTiO 3 After ball milling for 15 to 20 hours, the product is calcined at 1000 to 1050° C. for 3 to 5 hours in an air atmosphere; And / or, the second type of ceramic solid solution is prepared by the following preparation method: according to the chemical formula A 3 B 3 α B 4 β B 5 γ O 3 The stoichiometric ratio of each element in B 3 Oxide, B 4 Oxide and BaTiO 3 After ball milling for 15 to 20 hours, the product is calcined at 1050 to 1100° C. for 3 to 5 hours in an air atmosphere.

8. A method for preparing the ceramic material according to any one of claims 1 to 7, It is characterized in that The method comprises the following steps: mixing a first type ceramic solid solution, a second type ceramic solid solution, MnO 2 、V 2 O 5 The mixture is mixed evenly with a sintering aid to obtain a ceramic material.

9. A ceramic slurry comprising ceramic powder, an organic solvent and a binder, It is characterized in that The ceramic powder is the ceramic material according to any one of claims 1 to 7.

10. A chip-type multilayer ceramic capacitor, It is characterized in that It comprises a ceramic medium made from the ceramic slurry according to claim 9.

Citation Information

Patent Citations

  • Dielectric ceramic composition and multilayer ceramic capacitor comprising the same

    CN111559910A

  • Dielectric material of multilayer chip ceramic capacitor, and preparation method thereof

    CN113880569A

  • Dielectric ceramic composition and ceramic capacitor

    CN1812022A

  • Dielectric ceramic and method for producing the same, and laminated ceramic capacitor

    JP2011011919A

  • Dielectric ceramic composition and multiplayer ceramicchip capacitor using the same composition

    KR1020050091138A