Phosphogypsum-based thermal insulation and sound insulation building block and preparation method thereof
By using phosphogypsum, light aggregate and fiber reinforced materials in the block, combined with dehydration and microwave puffing, the problem of insufficient insulation and sound insulation performance of traditional blocks is solved, and efficient energy-saving and sound insulation effect is achieved, and the environment is reduced. Pollution meets the requirements of modern green buildings.
Patent Information
- Application Number
- CN202410932416.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-26
AI Technical Summary
Traditional block materials have high thermal conductivity and poor thermal insulation performance, and have not fully considered sound insulation requirements, resulting in poor noise isolation performance, and consume a lot of resources during the production process, resulting in pollution, which is not in line with the environmental protection concept of modern green buildings.
Phosphogypsum is used as the main raw material, combined with light aggregate, fiber reinforced material and phase change material, improve the insulation and sound insulation performance of the block through dehydration and microwave puffing treatment, and ensure the compactness of the finished product through multi-cavity molds and vibration tables. Wet maintenance process improves quality and uniformity.
Significantly improve the thermal insulation and sound insulation performance of the block, reduce noise interference, reduce moisture content, enhance material stability and strength, reduce building load, use environmentally friendly materials, reduce environmental pollution, and improve easy operation of construction consistency between sex and finished product.
Smart Images

Figure CN119019184A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building blocks, in particular to a phosphogypsum-based heat-insulating and sound-insulating building block and a preparation method thereof. Background Art
[0002] Masonry blocks are man-made blocks made of concrete, industrial waste (slag, fly ash, etc.) or local materials. They are larger in size than bricks and have the advantages of simple equipment and fast masonry speed, which meets the requirements of wall reform in the development of building industrialization.
[0003] However, traditional block materials such as clay bricks and concrete blocks have high thermal conductivity and poor thermal insulation performance, which makes it difficult to meet the requirements of modern buildings for energy conservation and thermal insulation. The density and structural design of many traditional blocks do not fully consider the need for sound insulation, resulting in poor performance in noise isolation and failure to provide a quiet and comfortable living or working environment. Some traditional blocks consume a lot of resources and generate pollutants during the production process, which does not conform to the environmental protection concept of modern green buildings. In addition, the disposal of discarded blocks will also have an impact on the environment. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a thermal insulation and sound insulation building block based on phosphogypsum and a preparation method thereof, which solves the problem that the density and structural design of many traditional building blocks do not fully consider the sound insulation requirements, resulting in poor performance in noise isolation and inability to provide a quiet and comfortable living or working environment; some traditional building blocks consume a large amount of resources and generate pollutants during the production process, which does not conform to the environmental protection concept of modern green buildings.
[0005] To achieve the above objectives, the present invention is implemented by the following technical scheme: a method for preparing a thermal insulation and sound insulation building block based on phosphogypsum, comprising the following steps:
[0006] S1. Raw material preparation
[0007] Select 60%-80% phosphogypsum, 10%-20% cement, 5%-10% sand, 5%-10% fine aggregate, 5%-10% lightweight aggregate, 1%-5% fiber reinforcement, 0.5%-2.0% admixture and 50%-80% clean water;
[0008] S2. Raw material processing
[0009] The phosphogypsum is dehydrated by a dehydrating device to reduce the moisture content to less than 10% to improve its stability, and then the lightweight aggregate is expanded by a microwave puffing machine to improve its thermal insulation performance, and finally the limiting reinforcement material is cut into the same length by a cutting device;
[0010] S3. Dry Mixing
[0011] Put all the phosphogypsum, cement, sand, fine aggregate, lightweight aggregate and fiber reinforcement into a mixer and dry mix at a speed of 800-1200r / min for 10-15min;
[0012] S4. Wet mixing
[0013] Gradually add clean water into the mixer and continue stirring at a speed of 500-1500r / min. Adjust the amount of clean water as needed to achieve the desired consistency of the mixture. When the consistency of the mixture reaches the standard, add all the admixtures into the mixer and continue stirring for 5-10 minutes to ensure that the admixtures are mixed into the mixture.
[0014] S5. New functional material mixing
[0015] Add phase change material, nano silicon dioxide and polyurethane foam particles to a mixer and mix them at a speed of 300-600 r / min, mix them into the mixture, then add a foaming agent to the mixer and stir at a speed of 100-200 r / min, while heating the temperature to 20-30°C, and continue stirring and heating for 10-30 minutes;
[0016] S6. Molding
[0017] Use a multi-cavity mold or a special shape mold, and apply a release agent on the inner surface of the mold. Then pour the mixture into the mold evenly, use a vibration table or manual vibration to expel bubbles to ensure that the finished product is dense, and finally let it stand at room temperature for 24 hours to allow the mixture to initially solidify and form;
[0018] S7. Maintenance
[0019] Move the preliminarily formed blocks to a wet curing environment without demoulding, maintain humidity above 70%, and maintain for no less than 7 days. During this period, spray water regularly to ensure that the surface and interior of the blocks remain moist;
[0020] S8. Demolding
[0021] After curing, the mold is removed, the blocks are taken out, and the finished products are then quality checked to ensure that the size, strength and appearance meet the requirements.
[0022] Preferably, the cement in S1 is any one of silicate cement and expanded silicate cement, the particle size of the sand in S1 is 2-5 mm, the fine aggregate in S1 is any one of polystyrene particles, fly ash and slag powder, the lightweight aggregate in S1 is any one of perlite, vermiculite, rice husk, straw and sawdust, the fiber reinforcement material in S1 is any one of plant fiber, nylon fiber, glass fiber and polypropylene fiber, and the admixture in S1 is any two of acrylic emulsion, epoxy resin, diatom mud and polyurethane.
[0023] Preferably, the phase change material in S5 is any one of sodium stearate, calcium stearate and polyethylene glycol, and the foaming agent in S5 is any one of azodicarbonamide and diphenylsulfone hydrazine.
[0024] Preferably, a thermal insulation and sound insulation block based on phosphogypsum comprises a block body, the surface of the block body is provided with cavities of uniform or different sizes, and the cavities may be irregular, a sound insulation layer is arranged on the inner side of the block body, and the interior of the sound insulation layer is filled with rock wool, and a thermal insulation layer is arranged on the outer side of the block body, and the interior of the thermal insulation layer is filled with polystyrene foam board.
[0025] The present invention provides a thermal insulation and sound insulation building block based on phosphogypsum and a preparation method thereof. It has the following beneficial effects:
[0026] 1. The present invention realizes resource utilization by using phosphogypsum as the main raw material, reduces environmental pollution and waste disposal pressure, and by adding lightweight aggregates and phase change materials into the mixture, the building blocks can significantly improve thermal insulation performance, and are suitable for building energy-saving projects. By adding fiber-reinforced materials and using lightweight aggregates, the building blocks have good sound insulation effects, effectively reduce noise interference, and improve living comfort. The dehydrated phosphogypsum reduces the moisture content and improves the stability of the material. In addition, the addition of cement and admixtures further enhances the strength and durability of the building blocks. The use of lightweight aggregates and other lightweight materials makes the overall weight of the building blocks lighter, which is convenient for construction and transportation, and reduces the load on the building.
[0027] 2. The present invention ensures the density of the finished product by adopting a multi-cavity mold and a vibration table during the preparation process, and improves the quality and uniformity of the blocks through a wet curing process, thereby ensuring the ease of operation during the construction process and the consistency of the finished product. Most of the materials used are harmless and environmentally friendly materials, which reduce the impact on the environment and protect the health of users. Overall, the thermal insulation and sound insulation blocks based on phosphogypsum not only effectively utilize industrial by-products, but also significantly improve the thermal insulation and sound insulation properties of building materials, while maintaining high strength and stability, and have good economic and environmental benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of the process of the preparation method of the present invention;
[0029] Figure 2 It is a structural schematic diagram of the building block in the present invention;
[0030] Figure 3 It is a schematic structural diagram of the building block filling layer in the present invention.
[0031] Among them, 1. block body; 2. cavity; 3. sound insulation layer; 4. thermal insulation layer. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Embodiment 1:
[0034] like Figure 1 As shown, an embodiment of the present invention provides a method for preparing a thermal insulation and sound insulation building block based on phosphogypsum, comprising the following steps:
[0035] S1. Raw material preparation
[0036] Select 60% phosphogypsum, 10% cement, 5% sand, 5% fine aggregate, 5% lightweight aggregate, 1% fiber reinforcement material, 0.5% admixture and 50% clean water;
[0037] S2. Raw material processing
[0038] The phosphogypsum is dehydrated by a dehydrating device to reduce the moisture content to less than 10% to improve its stability, and then the lightweight aggregate is expanded by a microwave puffing machine to improve its thermal insulation performance, and finally the limiting reinforcement material is cut into the same length by a cutting device;
[0039] S3. Dry Mixing
[0040] Put all the phosphogypsum, cement, sand, fine aggregate, lightweight aggregate and fiber reinforcement into a mixer and dry mix at a speed of 800r / min for 10min;
[0041] S4. Wet mixing
[0042] Gradually add clean water into the mixer and continue stirring at a speed of 500r / min. Adjust the amount of clean water as needed to achieve the desired consistency of the mixture. When the consistency of the mixture reaches the standard, add all the admixtures into the mixer and continue stirring for 5 minutes to ensure that the admixtures are mixed into the mixture.
[0043] S5. New functional material mixing
[0044] Add phase change material, nano-silicon dioxide and polyurethane foam particles to a mixer and mix them at a speed of 300 r / min. Mix them into the mixture, then add a foaming agent to the mixer and stir at a speed of 100 r / min. Heat the temperature to 20°C and continue stirring and heating for 10 minutes.
[0045] S6. Molding
[0046] Use a multi-cavity mold or a special shape mold, and apply a release agent on the inner surface of the mold. Then pour the mixture into the mold evenly, use a vibration table or manual vibration to expel bubbles to ensure that the finished product is dense, and finally let it stand at room temperature for 24 hours to allow the mixture to initially solidify and form;
[0047] S7. Maintenance
[0048] Move the preliminarily formed blocks to a wet curing environment without demoulding, maintain humidity above 70%, and maintain for no less than 7 days. During this period, spray water regularly to ensure that the surface and interior of the blocks remain moist;
[0049] S8. Demolding
[0050] After curing, the mold is removed, the blocks are taken out, and the finished products are then inspected to ensure that the size, strength and appearance meet the requirements;
[0051] The cement in S1 is any one of silicate cement and expansive silicate cement, the particle size of the sand in S1 is 2 mm, the fine aggregate in S1 is any one of polystyrene particles, fly ash and slag powder, the lightweight aggregate in S1 is any one of perlite, vermiculite, rice husk, straw and sawdust, the fiber reinforcement material in S1 is any one of plant fiber, nylon fiber, glass fiber and polypropylene fiber, the admixture in S1 is any two of acrylic emulsion, epoxy resin, diatom mud and polyurethane; the phase change material in S5 is any one of sodium stearate, calcium stearate and polyethylene glycol, and the foaming agent in S5 is any one of azodicarbonamide and diphenylsulfone hydrazine.
[0052] As an industrial by-product, phosphogypsum has been used as a main raw material to achieve resource utilization, reducing environmental pollution and waste disposal pressure. By adding lightweight aggregates and phase change materials to the mixture, the building blocks can significantly improve the thermal insulation performance and are suitable for building energy-saving projects. The addition of fiber-reinforced materials and the use of lightweight aggregates make the building blocks have better sound insulation effects, effectively reducing noise interference and improving living comfort. The dehydrated phosphogypsum has reduced moisture content and improved material stability. In addition, the addition of cement and admixtures further enhances the strength and durability of the building blocks. Lightweight aggregates and other lightweight materials The use of phosphogypsum makes the overall weight of the blocks lighter, which is convenient for construction and transportation and reduces the load on the building; multi-cavity molds and vibration tables are used in the preparation process to ensure the density of the finished product, and the quality and uniformity of the blocks are improved through wet curing technology to ensure the ease of operation during construction and the consistency of the finished product. Most of the materials used are harmless and environmentally friendly materials, which reduces the impact on the environment and protects the health of users; on the whole, the thermal insulation and sound insulation blocks based on phosphogypsum not only effectively utilize industrial by-products, but also significantly improve the thermal insulation and sound insulation properties of building materials, while maintaining high strength and stability, and have good economic and environmental benefits.
[0053] Embodiment 2:
[0054] like Figure 1 As shown, an embodiment of the present invention provides a method for preparing a thermal insulation and sound insulation building block based on phosphogypsum, comprising the following steps:
[0055] S1. Raw material preparation
[0056] Select 80% phosphogypsum, 20% cement, 10% sand, 10% fine aggregate, 10% lightweight aggregate, 5% fiber reinforcement material, 2.0% admixture and 80% clean water;
[0057] S2. Raw material processing
[0058] The phosphogypsum is dehydrated by a dehydrating device to reduce the moisture content to less than 10% to improve its stability, and then the lightweight aggregate is expanded by a microwave puffing machine to improve its thermal insulation performance, and finally the limiting reinforcement material is cut into the same length by a cutting device;
[0059] S3. Dry Mixing
[0060] Put all the phosphogypsum, cement, sand, fine aggregate, lightweight aggregate and fiber reinforcement into a mixer and dry mix at a speed of 1200r / min for 15min;
[0061] S4. Wet mixing
[0062] Gradually add clean water into the mixer and continue stirring at a speed of 1500r / min. Adjust the amount of clean water as needed to achieve the desired consistency of the mixture. When the consistency of the mixture reaches the standard, add all the admixtures into the mixer and continue stirring for 10 minutes to ensure that the admixtures are mixed into the mixture.
[0063] S5. New functional material mixing
[0064] Add phase change material, nano-silicon dioxide and polyurethane foam particles to a mixer and mix them at a speed of 600 r / min, mix them into the mixture, then add a foaming agent to the mixer and stir at a speed of 200 r / min, while heating the temperature to 30°C, and continue stirring and heating for 30 minutes;
[0065] S6. Molding
[0066] Use a multi-cavity mold or a special shape mold, and apply a release agent on the inner surface of the mold. Then pour the mixture into the mold evenly, use a vibration table or manual vibration to expel bubbles to ensure that the finished product is dense, and finally let it stand at room temperature for 24 hours to allow the mixture to initially solidify and form;
[0067] S7. Maintenance
[0068] Move the preliminarily formed blocks to a wet curing environment without demoulding, maintain humidity above 70%, and maintain for no less than 7 days. During this period, spray water regularly to ensure that the surface and interior of the blocks remain moist;
[0069] S8. Demolding
[0070] After curing, the mold is removed, the blocks are taken out, and the finished products are then inspected to ensure that the size, strength and appearance meet the requirements;
[0071] The cement in S1 is any one of silicate cement and expanded silicate cement, the particle size of the sand in S1 is 5 mm, the fine aggregate in S1 is any one of polystyrene particles, fly ash and slag powder, the lightweight aggregate in S1 is any one of perlite, vermiculite, rice husk, straw and sawdust, the fiber reinforcement material in S1 is any one of plant fiber, nylon fiber, glass fiber and polypropylene fiber, the admixture in S1 is any two of acrylic emulsion, epoxy resin, diatom mud and polyurethane; the phase change material in S5 is any one of sodium stearate, calcium stearate and polyethylene glycol, and the foaming agent in S5 is any one of azodicarbonamide and diphenylsulfone hydrazine.
[0072] As an industrial by-product, phosphogypsum has been used as a main raw material to achieve resource utilization, reducing environmental pollution and waste disposal pressure. By adding lightweight aggregates and phase change materials to the mixture, the building blocks can significantly improve the thermal insulation performance and are suitable for building energy-saving projects. The addition of fiber-reinforced materials and the use of lightweight aggregates make the building blocks have better sound insulation effects, effectively reducing noise interference and improving living comfort. The dehydrated phosphogypsum has reduced moisture content and improved material stability. In addition, the addition of cement and admixtures further enhances the strength and durability of the building blocks. Lightweight aggregates and other lightweight materials The use of phosphogypsum makes the overall weight of the blocks lighter, which is convenient for construction and transportation and reduces the load on the building; multi-cavity molds and vibration tables are used in the preparation process to ensure the density of the finished product, and the quality and uniformity of the blocks are improved through wet curing technology to ensure the ease of operation during construction and the consistency of the finished product. Most of the materials used are harmless and environmentally friendly materials, which reduces the impact on the environment and protects the health of users; on the whole, the thermal insulation and sound insulation blocks based on phosphogypsum not only effectively utilize industrial by-products, but also significantly improve the thermal insulation and sound insulation properties of building materials, while maintaining high strength and stability, and have good economic and environmental benefits.
[0073] Embodiment three:
[0074] like Figure 2 and Figure 3 As shown, an embodiment of the present invention provides a thermal insulation and sound insulation block based on phosphogypsum, including a block body 1, a surface of the block body 1 is provided with cavities 2 of uniform or different sizes, and the cavity 2 may be irregular, a sound insulation layer 3 is arranged on the inner side of the block body 1, and the interior of the sound insulation layer 3 is filled with rock wool, and a thermal insulation layer 4 is arranged on the outer side of the block body 1, and the interior of the thermal insulation layer 4 is filled with polystyrene foam board.
[0075] The outer insulation layer is filled with polystyrene foam board, which has excellent thermal insulation properties and can effectively reduce heat conduction, maintain stable indoor temperature, reduce energy consumption and achieve energy-saving effects. The sound insulation layer set inside the block is filled with rock wool, which is a high-efficiency acoustic material that can effectively absorb and block the propagation of sound waves, thereby significantly improving the sound insulation effect of the building and enhancing the comfort of the living or working environment.
[0076] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a thermal insulation and sound insulation building block based on phosphogypsum, characterized in that: The following steps are involved: S1. Raw material preparation Select 60%-80% phosphogypsum, 10%-20% cement, 5%-10% sand, 5%-10% fine aggregate, 5%-10% lightweight aggregate, 1%-5% fiber reinforcement, 0.5%-2.0% admixture and 50%-80% clean water; S2. Raw material processing The phosphogypsum is dehydrated by a dehydrating device to reduce the moisture content to less than 10% to improve its stability, and then the lightweight aggregate is expanded by a microwave puffing machine to improve its thermal insulation performance, and finally the limiting reinforcement material is cut into the same length by a cutting device; S3. Dry Mixing Put all the phosphogypsum, cement, sand, fine aggregate, lightweight aggregate and fiber reinforcement into a mixer and dry mix at a speed of 800-1200r / min for 10-15min; S4. Wet mixing Gradually add clean water into the mixer and continue stirring at a speed of 500-1500r / min. Adjust the amount of clean water as needed to achieve the desired consistency of the mixture. When the consistency of the mixture reaches the standard, add all the admixtures into the mixer and continue stirring for 5-10 minutes to ensure that the admixtures are mixed into the mixture. S5. New functional material mixing Add phase change material, nano silicon dioxide and polyurethane foam particles to a mixer and mix them at a speed of 300-600 r / min, mix them into the mixture, then add a foaming agent to the mixer and stir at a speed of 100-200 r / min, while heating the temperature to 20-30°C, and continue stirring and heating for 10-30 minutes; S6. Molding Use a multi-cavity mold or a special shape mold, and apply a release agent on the inner surface of the mold. Then pour the mixture into the mold evenly, use a vibration table or manual vibration to expel bubbles to ensure that the finished product is dense, and finally let it stand at room temperature for 24 hours to allow the mixture to initially solidify and form; S7. Maintenance Move the preliminarily formed blocks to a wet curing environment without demoulding, maintain humidity above 70%, and maintain for no less than 7 days. During this period, spray water regularly to ensure that the surface and interior of the blocks remain moist; S8. Demoulding After curing, the mold is removed, the blocks are taken out, and the finished products are then quality checked to ensure that the size, strength and appearance meet the requirements.
2. The method for preparing a thermal insulation and sound insulation building block based on phosphogypsum according to claim 1, characterized in that: The cement in S1 is any one of silicate cement and expanded silicate cement, the particle size of the sand in S1 is 2-5 mm, the fine aggregate in S1 is any one of polystyrene particles, fly ash and slag powder, the lightweight aggregate in S1 is any one of perlite, vermiculite, rice husk, straw and sawdust, the fiber reinforcement material in S1 is any one of plant fiber, nylon fiber, glass fiber and polypropylene fiber, and the admixture in S1 is any two of acrylic emulsion, epoxy resin, diatom mud and polyurethane.
3. The method for preparing a thermal insulation and sound insulation building block based on phosphogypsum according to claim 1, characterized in that: The phase change material in S5 is any one of sodium stearate, calcium stearate and polyethylene glycol, and the foaming agent in S5 is any one of azodicarbonamide and diphenylsulfone hydrazine.
4. A thermal insulation and sound insulation building block based on phosphogypsum, characterized in that: The invention comprises a block body (1), wherein the surface of the block body (1) is provided with cavities (2) of uniform or different sizes, and the cavities (2) may be irregular, a sound insulation layer (3) is arranged on the inner side of the block body (1), and the interior of the sound insulation layer (3) is filled with rock wool, and a heat insulation layer (4) is arranged on the outer side of the block body (1), and the interior of the heat insulation layer (4) is filled with a polystyrene foam board.