Ethylene-butadiene copolymer and single-kettle polymerization method thereof

Through a single-kettle solution batch polymerization system, the problem of industrial production of ethylene-butadiene copolymers is solved, and efficient and uniformly distributed copolymer production is achieved, which is suitable for continuous processes under industrial conditions.

CN119019586APending Publication Date: 2024-11-26GUANGRAO ZHENGHE PETROCHEMICAL CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411123823.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to realize the industrial production process of ethylene-butadiene copolymers, resulting in unsuitable polymerization temperature and conditions, resulting in problems such as product viscosity and easy degradation.

Method used

Using a single-kettle solution batch polymerization system, the polymerization reaction is carried out under anhydrous and oxygen-free conditions by purifying ethylene and butadiene, adding catalysts and solvents, and using constant temperature and constant pressure methods to control the reaction conditions and catalyst ratio to achieve ethylene - Uniform distribution and high conversion of -butadiene copolymer.

Benefits of technology

The conversion rate of butadiene monomer is improved, the viscosity of the gel is reduced, and the uniform distribution and efficient production of ethylene-butadiene copolymer are achieved, which is suitable for continuous production of industrial equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019586A_ABST
    Figure CN119019586A_ABST
Patent Text Reader

Abstract

The invention discloses an ethylene-butadiene copolymer and a single-kettle polymerization method thereof, relates to the technical field of polymer synthesis, and solves the key problem of industrial production of the ethylene-butadiene copolymer. The method is realized by applying an ethylene-butadiene copolymer single-kettle polymerization system. The system comprises a feeding unit, a single polymerization kettle, a liquid storage tank, a condensation kettle and a product drying unit, the feeding unit comprises an ethylene storage tank, an ethylene purification column, butadiene, a butadiene purification column, a catalyst storage tank and a solvent storage tank; the method comprises the following steps: removing impurities from ethylene and butadiene, and feeding ethylene, butadiene, a solvent and a catalyst into a single reaction kettle under anhydrous and anaerobic conditions to carry out polymerization reaction; during discharging, an inactivating agent and an anti-aging agent are added into the pipeline, and the mixture enters a liquid storage tank; and after entering the condensation kettle, separating the product from the unreacted monomer and solvent, feeding the colloidal particles obtained by condensation into a drying unit, purifying the unreacted monomer and solvent, and returning to the feeding unit. The method can be applied to industrial production of the ethylene-butadiene copolymer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer synthesis, and in particular to an ethylene-butadiene copolymer and a single-pot polymerization method thereof. Background Art

[0002] The random copolymerization of ethylene and butadiene sequences to prepare a high-performance ethylene-butadiene copolymer material is a goal that the academic and industrial circles have longed for. This ethylene-butadiene copolymer material is easy to mix and vulcanize and has excellent aging resistance, cold resistance, high tensile strength, excellent wear resistance, puncture resistance, and low rolling resistance. So far, there have been many patents reporting the preparation method and catalytic system of ethylene-butadiene copolymers. For example, Chinese patent documents CN106459311A, CN108690167A, CN110218274A, CN110520449A, CN113174001A. However, the literature and data reports on the amplification production process of the copolymerization of ethylene and butadiene are extremely rare. Therefore, to realize the industrial amplification production of ethylene-butadiene copolymers, it is necessary to develop a new process suitable for the continuous production of ethylene-butadiene copolymers, and solve the problem of industrial amplification production process of ethylene-butadiene copolymers, which has become one of the problems that those skilled in the art need to solve.

[0003] At present, the industrial production of polyolefins mainly adopts bulk polymerization, gas phase polymerization or slurry polymerization processes, such as Unipol process, Spheripol process and Novolene process. However, for ethylene-butadiene copolymers, the polymerization reaction temperature is between 30℃ and 80℃, and the produced polymer is viscous. It is not possible to use the preparation process and equipment of polyolefin elastomer POE (POE is generally prepared at 60℃ to 190℃, under which butadiene monomer is very easy to self-polymerize, and the produced ethylene-butadiene copolymer is also easy to degrade), nor can it use the production process and equipment of neodymium-based butadiene rubber or isoprene rubber (butadiene rubber and isoprene rubber only involve one conjugated diene monomer, and no ethylene is involved in the polymerization). Therefore, it is necessary to redevelop a set of processes and equipment systems suitable for the industrial production of ethylene-butadiene copolymers. Summary of the invention

[0004] The problem to be solved by the present invention is to provide an industrial production process of ethylene-butadiene copolymer, in particular, a single-pot solution batch polymerization system and process for producing ethylene-butadiene copolymer, so as to realize the preparation of ethylene-butadiene copolymer under industrial production conditions and solve the key problem of ethylene-butadiene copolymer from laboratory small-scale test to industrial production. In view of this, the present invention proposes an ethylene-butadiene copolymer and a single-pot polymerization method thereof.

[0005] The present invention first provides a single-pot polymerization method for ethylene-butadiene copolymer, and the method is implemented by using a single-pot polymerization system for ethylene-butadiene copolymer;

[0006] The ethylene-butadiene copolymer single-pot polymerization system comprises a feed unit, a single polymerization kettle, a liquid storage tank, a condensation kettle and a product drying unit; the feed unit comprises an ethylene storage tank, an ethylene purification column, butadiene, a butadiene purification column, a catalyst storage tank and a solvent storage tank;

[0007] The single-pot polymerization method specifically comprises the following steps:

[0008] S1. Ethylene and butadiene are respectively passed through purification columns to remove impurities. Under anhydrous and oxygen-free conditions, ethylene, butadiene, solvent and catalyst are introduced into a single reactor from a bottom feed port, and a polymerization reaction occurs in the reactor;

[0009] S2. When the reacted solution is discharged from the polymerization unit, a deactivator and an antioxidant are added in situ in the pipeline and enter the liquid storage tank;

[0010] S3, after the glue liquid enters the coagulation kettle from the liquid storage tank, the product is separated from the unreacted monomers and the solvent by water vapor, the ethylene-butadiene copolymer glue particles obtained after coagulation are sent to the drying unit, and the unreacted monomers and the solvent are returned to the feeding unit for recycling after purification.

[0011] Preferably, the reaction conditions of the polymerization reaction in step S1 are as follows:

[0012] The saturated vapor pressure is 0.1MPa to 5MPa, more preferably 0.3MPa to 3Mpa, and most preferably 0.5MPa to 1.5MPa; the reaction temperature is 20°C to 140°C, more preferably 40°C to 100°C, and most preferably 50°C to 90°C; the polymerization reaction time is 1h to 6h, more preferably 2h to 5h, and most preferably 3h to 4h.

[0013] Preferably, the solvent is selected from one or a combination of at least two of toluene, xylene, n-pentane, n-hexane, cyclohexane, n-heptane, n-octane, n-nonane, n-decane, methylcyclopentane, methylcyclohexane, isopentane, isohexane, isoheptane, isooctane, isononane and isodecane.

[0014] Preferably, the catalyst comprises a co-catalyst and a main catalyst;

[0015] The main catalyst is selected from one or a combination of at least two of a restricted geometry rare earth catalyst, a monocyclopentadienyl rare earth catalyst, and a non-cyclopentadienyl rare earth catalyst;

[0016] The co-catalyst includes a main group alkyl reagent and an organic boron reagent.

[0017] Preferably, the main catalyst is selected from rare earth catalysts 1 to 6 having the following structures:

[0018]

[0019] Preferably, the main group alkyl reagent is selected from one or a combination of at least two of trimethylaluminum, triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, methylaluminoxane, modified methylaluminoxane, dried methylaluminoxane, silica-supported MAO, diethylaluminum hydride, diisobutylaluminum hydride, dibutylmagnesium, and diethylzinc;

[0020] The organic boron reagent is selected from one of trispentafluorophenyl boron, triphenyl carbon tetrakis (pentafluorophenyl boron), N,N dimethylaniline tetrakis (pentafluorophenyl boron), N,N di(hexadecyl)aniline tetrakis (pentafluorophenyl boron), and N,N di(octadecyl)aniline tetrakis (pentafluorophenyl boron), or a combination of at least two thereof.

[0021] Preferably, the molar ratio of the main catalyst to butadiene is in the range of 1:5000 to 1:200000; the molar ratio of the main catalyst to the organic boron reagent is 1:0 to 1:2; the molar ratio of the main catalyst to the main group alkyl reagent is 1:20 to 1:2000.

[0022] Preferably, the ethylene pressure is 0.1 MPa to 5 MPa; the concentration of the butadiene monomer entering the first reactor is 8 g / 100 mL to 20 g / 100 mL; and the initial temperature of the mixed solution of butadiene, ethylene and inert solvent before entering the reactor is 20° C. to 40° C.

[0023] Preferably, the operating pressure of the coagulation reactor is 0.1 MPa(G) to 1 MPa(G).

[0024] The present invention also provides an ethylene-butadiene copolymer, which is prepared by the above-mentioned single-pot polymerization method, and the number average molecular weight of the ethylene-butadiene copolymer is 13.7×10 4 ~15.4×10 4 g / mol, the molecular weight distribution is 1.97-2.37, and the molar insertion rate of butadiene is 42%-46%.

[0025] Compared with the prior art, the specific beneficial effects of the present invention are:

[0026] The present invention relates to an intermittent preparation process system and method for producing ethylene-butadiene copolymers. By using a single polymerization reactor and a constant temperature and constant pressure method, the system can effectively control the uniform distribution of two structural units, ethylene and butadiene, in the ethylene-butadiene copolymer in the molecular chain while improving the conversion rate of butadiene monomers and reducing the viscosity of the rubber solution, thereby providing a set of solutions for the continuous production of ethylene and butadiene on industrial equipment.

[0027] The experimental verification results show that the process system and method provided by the present invention can be used to intermittently produce ethylene-butadiene copolymers with a polymerization activity of 2.1×10 6 ~6.4×10 6 g / (mol·h), the single-pass butadiene conversion rate can reach 75%, and the number average molecular weight of ethylene-butadiene copolymer is 13.7×10 4 ~15.4×10 4 g / mol, the molecular weight distribution is 1.97-2.37, and the molar insertion rate of butadiene is 42%-46%. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The single-pot polymerization system and method flow diagram of ethylene-butadiene copolymer;

[0029] Figure 2 This is a schematic diagram of the appearance of the ethylene-butadiene copolymer toluene glue solution in Example 3;

[0030] Figure 3 This is a schematic diagram of the appearance of the ethylene-butadiene copolymer dry rubber in Example 3;

[0031] Figure 4 This is the GPC spectrum of the ethylene-butadiene copolymer in Example 3. DETAILED DESCRIPTION

[0032] In order to make the technical solution of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the specification of the present invention. It should be noted that the following embodiments are only used to better understand the technical solution of the present invention and should not be understood as a limitation to the present invention.

[0033] Example 1.

[0034] In the first step, cyclohexane is used as the polymerization solvent, and all raw materials are purified through a refining system to reduce the water and oxygen content in cyclohexane, ethylene and butadiene to below 1 ppm.

[0035] In the second step, the polymerization reactor was purged with nitrogen and flushed with purified cyclohexane for 8 h.

[0036] In the third step, cyclohexane at 23 L / h, butadiene at 3 kg / h, ethylene at 1200 L / h and cocatalyst 1 (Al iBu3, 3.4wt% cyclohexane solution) is mixed in situ in the pipeline at a flow rate of 0.3L / h and then enters the polymerization reactor; the mixture solution of the main catalyst and the organic boron salt (1.0g / L toluene solution) is mixed online with the above mixed solution through the pipeline at a flow rate of 0.3L / h and then enters the polymerization reactor. All raw materials are bottom fed, and the reaction temperature of the polymerization reactor is controlled at 60±5℃, and the polymerization is carried out for 4h. When the reacted solution is discharged from the polymerization unit, a deactivator and an antioxidant are added in situ in the pipeline and enter the liquid storage tank to obtain ethylene-butadiene copolymer n-hexane glue.

[0037] In the fourth step, after the glue liquid enters the coagulation kettle from the liquid storage tank, the product is separated from the unreacted monomers and the solvent by water vapor, and the ethylene-butadiene copolymer glue particles obtained after coagulation are sent to the drying unit to obtain ethylene-butadiene copolymer dry glue, and the unreacted monomers and solvent are returned to the feeding unit for recycling after purification.

[0038] The obtained copolymer was tested, and the test results are as follows:

[0039] The polymerization activity was 2.1×10 6 g / (mol·h), the butadiene conversion rate was 75%; the number average molecular weight of the ethylene-butadiene copolymer was 145,000, the molecular weight distribution was 2.14, and the butadiene molar insertion rate was 45%.

[0040] Example 2.

[0041] In the first step, cyclohexane is used as the polymerization solvent, and all raw materials are purified through a refining system to reduce the water and oxygen content in n-hexane, ethylene and butadiene to below 1 ppm.

[0042] In the second step, the polymerization reactor was purged with nitrogen and flushed with purified n-hexane for 8 h.

[0043] In the third step, n-hexane at 23 L / h, butadiene at 3 kg / h, ethylene at 1200 L / h and co-catalyst 1 (Al i Bu3, 3.4wt% cyclohexane solution) is mixed in situ in the pipeline at a flow rate of 0.3L / h and then enters the polymerization reactor; the mixture solution of the main catalyst and the organic boron salt (1.0g / L toluene solution) is mixed online with the above mixed solution through the pipeline at a flow rate of 0.3L / h and then enters the polymerization reactor. All raw materials are bottom fed, the reaction temperature of the polymerization reactor is controlled at 60±5℃, and the polymerization runs for 4h. When the reacted solution is discharged from the polymerization unit, the deactivator and antioxidant are added in situ in the pipeline and enter the liquid storage tank to obtain ethylene-butadiene copolymer n-hexane glue.

[0044] In the fourth step, after the glue liquid enters the coagulation kettle from the liquid storage tank, the product is separated from the unreacted monomers and the solvent by water vapor, and the ethylene-butadiene copolymer glue particles obtained after coagulation are sent to the drying unit to obtain ethylene-butadiene copolymer dry glue, and the unreacted monomers and solvent are returned to the feeding unit for recycling after purification.

[0045] The obtained copolymer was tested, and the test results are as follows:

[0046] The polymerization activity was 3.1×10 6 g / (mol·h), the butadiene conversion rate was 74%; the number average molecular weight of the ethylene-butadiene copolymer was 154,000, the molecular weight distribution was 2.37, and the butadiene molar insertion rate was 42%.

[0047] Example 3.

[0048] In the first step, toluene is used as the polymerization solvent, and all raw materials are purified through a refining system to reduce the water and oxygen content in toluene, ethylene and butadiene to below 1 ppm.

[0049] In the second step, the polymerization reactor was purged with nitrogen and flushed with purified toluene for 8 h.

[0050] In the third step, toluene was added at 23 L / h, butadiene at 3 kg / h, ethylene at 1200 L / h, and a cocatalyst 1 (Al i Bu3, 3.4wt% cyclohexane solution) is mixed in situ in the pipeline at a flow rate of 0.3L / h and then enters the polymerization reactor; the mixture solution of the main catalyst and the organic boron salt (1.0g / L toluene solution) is mixed online with the above mixed solution through the pipeline at a flow rate of 0.3L / h and then enters the polymerization reactor. All raw materials are bottom fed, the reaction temperature of the polymerization reactor is controlled at 70±5℃, and the polymerization runs for 4h. When the reacted solution is discharged from the polymerization unit, the deactivator and antioxidant are added in situ in the pipeline and enter the liquid storage tank to obtain ethylene-butadiene copolymer n-hexane glue.

[0051] In the fourth step, after the glue liquid enters the coagulation reactor from the liquid storage tank, the product is separated from the unreacted monomers and the solvent by water vapor, and the ethylene-butadiene copolymer glue particles obtained after coagulation are sent to the drying unit to obtain ethylene-butadiene copolymer dry glue, and the unreacted monomers and solvent are returned to the feeding unit for recycling after purification. The appearance schematic diagram of the ethylene-butadiene copolymer toluene glue liquid obtained in this embodiment is shown in Figure 2 , the appearance diagram of ethylene-butadiene copolymer dry glue is shown in Figure 3 .

[0052] The obtained copolymer was tested, and the test results are as follows:

[0053] The polymerization activity was 6.4×10 6g / (mol·h), butadiene conversion rate was 75%; GPC spectrum of copolymer is shown in Figure 4 The number average molecular weight of the ethylene-butadiene copolymer is 137,000, the molecular weight distribution is 1.97, and the butadiene molar insertion rate is 46%.

[0054] The above is a detailed introduction to a process system and method for producing ethylene-butadiene copolymers by an intermittent process provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method and its core ideas of the present invention, including the best mode, and also enables any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, the present invention can also be improved and modified in a number of ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements that are not different from the textual expression of the claims, or if they include equivalent structural elements that are not substantially different from the textual expression of the claims, then these other embodiments should also be included in the scope of the claims.

Claims

1. A single-pot polymerization method for ethylene-butadiene copolymer, characterized in that: The method is implemented by using an ethylene-butadiene copolymer single-pot polymerization system; The ethylene-butadiene copolymer single-pot polymerization system comprises a feed unit, a single polymerization kettle, a liquid storage tank, a condensation kettle and a product drying unit; the feed unit comprises an ethylene storage tank, an ethylene purification column, butadiene, a butadiene purification column, a catalyst storage tank and a solvent storage tank; The single-pot polymerization method specifically comprises the following steps: S1. Ethylene and butadiene are respectively passed through purification columns to remove impurities. Under anhydrous and oxygen-free conditions, ethylene, butadiene, solvent and catalyst are introduced into a single reactor from a bottom feed port, and a polymerization reaction occurs in the reactor; S2. When the reacted solution is discharged from the polymerization unit, a deactivator and an antioxidant are added in situ in the pipeline and enter the liquid storage tank; S3, after the glue liquid enters the coagulation kettle from the liquid storage tank, the product is separated from the unreacted monomers and the solvent by water vapor, the ethylene-butadiene copolymer glue particles obtained after coagulation are sent to the drying unit, and the unreacted monomers and the solvent are returned to the feeding unit for recycling after purification.

2. The single-pot polymerization method of ethylene-butadiene copolymer according to claim 1, characterized in that: The reaction conditions of the polymerization reaction in step S1 are specifically as follows: The saturated vapor pressure is 0.1MPa to 5MPa, the reaction temperature is 20°C to 140°C, and the polymerization reaction time is 1h to 6h.

3. The single-pot polymerization method of ethylene-butadiene copolymer according to claim 1, characterized in that: The solvent is selected from one or a combination of at least two of toluene, xylene, n-pentane, n-hexane, cyclohexane, n-heptane, n-octane, n-nonane, n-decane, methylcyclopentane, methylcyclohexane, isopentane, isohexane, isoheptane, isooctane, isononane and isodecane.

4. The single-pot polymerization method of ethylene-butadiene copolymer according to claim 1, characterized in that: The catalyst includes a co-catalyst and a main catalyst; The main catalyst is selected from one or a combination of at least two of a restricted geometry rare earth catalyst, a monocyclopentadienyl rare earth catalyst, and a non-cyclopentadienyl rare earth catalyst; The co-catalyst includes a main group alkyl reagent and an organic boron reagent.

5. The single-pot polymerization method of ethylene-butadiene copolymer according to claim 1, characterized in that: The main catalyst is selected from rare earth catalysts 1 to 6 with the following structures:

6. The single-pot polymerization method of ethylene-butadiene copolymer according to claim 4, characterized in that: The main group alkyl reagent is selected from one or a combination of at least two of trimethylaluminum, triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, methylaluminoxane, modified methylaluminoxane, dried methylaluminoxane, silica-supported MAO, diethylaluminum hydride, diisobutylaluminum hydride, dibutylmagnesium, and diethylzinc; The organic boron reagent is selected from one of trispentafluorophenyl boron, triphenyl carbon tetrakis (pentafluorophenyl boron), N,N dimethylaniline tetrakis (pentafluorophenyl boron), N,N di(hexadecyl)aniline tetrakis (pentafluorophenyl boron), and N,N di(octadecyl)aniline tetrakis (pentafluorophenyl boron), or a combination of at least two thereof.

7. The single-pot polymerization method of ethylene-butadiene copolymer according to claim 6, characterized in that: The molar ratio of the main catalyst to butadiene is in the range of 1:5000 to 1:200000; the molar ratio of the main catalyst to the organic boron reagent is in the range of 1:0 to 1:2; and the molar ratio of the main catalyst to the main group alkyl reagent is in the range of 1:20 to 1:2000.

8. The single-pot polymerization method of ethylene-butadiene copolymer according to claim 1, characterized in that: The ethylene pressure is 0.1MPa-5MPa; the concentration of the butadiene monomer entering the first reactor is 8g / 100mL-20g / 100mL; the initial temperature of the mixed liquid of butadiene, ethylene and inert solvent before entering the reactor is 20°C-40°C.

9. The single-pot polymerization method of ethylene-butadiene copolymer according to claim 1, characterized in that: The operating pressure of the coagulation kettle is 0.1MPa(G) to 1MPa(G).

10. An ethylene-butadiene copolymer, characterized in that: The ethylene-butadiene copolymer is prepared by the single-pot polymerization method according to any one of claims 1 to 9, wherein the number average molecular weight of the ethylene-butadiene copolymer is 13.7×10 4 ~15.4×10 4 g / mol, the molecular weight distribution is 1.97-2.37, and the molar insertion rate of butadiene is 42%-46%.

Citation Information

Patent Citations

  • Method for producing multi-component copolymer

    CN106459311A

  • Ethylene and conjugated diene copolymer and preparation method thereof

    CN108690167A

  • Preparation method of ethylene-conjugated diene random copolymer

    CN110218274A

  • Method for producing multi-copolymer, multi-copolymer, rubber composition, and tire

    CN110520449A

  • Ethylene-butadiene random copolymer as well as preparation method and application thereof

    CN113174001A