Ethylene-butadiene copolymer and continuous production method thereof
By designing a continuous production process and device system, using the method of increasing temperature step and decreasing ethylene pressure step, the problem of industrial production of ethylene-butadiene copolymers is solved, and efficient production of ethylene-butadiene copolymers is achieved, solving the problem of industrial production of ethylene-butadiene copolymers. The product is viscous and easy to degrade.
Patent Information
- Application Number
- CN202411123824.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art is difficult to achieve industrial production of ethylene-butadiene copolymers, and the polymerization reaction temperature and conditions are not suitable, resulting in problems such as product viscosity and easy degradation.
A continuous production process and device system is designed, including feed unit, polymerization unit, condenser and product drying unit. The polymerization reaction of temperature step increment and ethylene pressure step decreases through a tandem reactor is carried out, combining appropriate catalysts and solvents Use to realize the industrial production of ethylene-butadiene copolymers.
It improves the conversion rate of butadiene monomer, reduces the viscosity of the gel, and achieves uniform distribution of ethylene and butadiene structural units in the molecular chain, which is suitable for industrial production.
Smart Images

Figure CN119019587A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer synthesis, and in particular to an olefin-conjugated diene copolymer and a continuous production method thereof. Background Art
[0002] The random copolymerization of ethylene and butadiene sequences to prepare a high-performance ethylene-butadiene copolymer material is a goal that the academic and industrial circles have longed for. This ethylene-butadiene copolymer material is easy to mix and vulcanize and has excellent aging resistance, cold resistance, high tensile strength, excellent wear resistance, puncture resistance, and low rolling resistance. So far, there have been many patents reporting the preparation method and catalytic system of ethylene-butadiene copolymers. For example, Chinese patent documents CN106459311A, CN108690167A, CN110218274A, CN110520449A, CN113174001A. However, the literature and data reports on the amplification production process of the copolymerization of ethylene and butadiene are extremely rare. Therefore, to realize the industrial amplification production of ethylene-butadiene copolymers, it is necessary to develop a new process suitable for the continuous production of ethylene-butadiene copolymers, and solve the problem of industrial amplification production process of ethylene-butadiene copolymers, which has become one of the problems that those skilled in the art need to solve.
[0003] At present, the industrial production of polyolefins mainly adopts bulk polymerization, gas phase polymerization or slurry polymerization processes, such as Unipol process, Spheripol process and Novolene process. However, for ethylene-butadiene copolymers, the polymerization reaction temperature is between 30℃ and 80℃, and the produced polymer is viscous. It is not possible to use the preparation process and equipment of polyolefin elastomer POE (POE is generally prepared at 60℃ to 190℃, under which butadiene monomer is very easy to self-polymerize, and the produced ethylene-butadiene copolymer is also easy to degrade), nor can it use the production process and equipment of neodymium-based butadiene rubber or isoprene rubber (butadiene rubber and isoprene rubber only involve one conjugated diene monomer, and no ethylene is involved in the polymerization). Therefore, it is necessary to redevelop a set of processes and equipment systems suitable for the industrial production of ethylene-butadiene copolymers. Summary of the invention
[0004] The problem to be solved by the present invention is to provide an industrial production process of ethylene-butadiene copolymer, in particular, a process production system for continuously producing ethylene-butadiene copolymer, so as to realize the preparation of ethylene-butadiene copolymer under industrial production conditions and solve the key problem of ethylene-butadiene copolymer from laboratory small-scale test to industrial production. In view of this, the present invention proposes an ethylene-butadiene copolymer and a continuous production method thereof.
[0005] The present invention first provides a method for continuous production of ethylene-butadiene copolymer, wherein the method is implemented by using an industrial production device for ethylene-butadiene copolymer;
[0006] The industrial production device of ethylene-butadiene copolymer comprises a feeding unit, a polymerization unit, a liquid storage tank, a coagulation kettle and a product drying unit;
[0007] The feeding unit includes an ethylene storage tank, an ethylene purification column, butadiene, a butadiene purification column, a catalyst storage tank and a solvent storage tank; the polymerization unit includes three or four reaction kettles connected in series; the condensation kettle is composed of one or more stirring kettles connected in series; the product drying unit includes a vibrating screen, an extrusion dehydrator and a drying box; the condensation kettle is connected to the vibrating screen, the extrusion dehydrator and the drying box in sequence.
[0008] The continuous production method specifically comprises the following steps:
[0009] S1. Ethylene and butadiene are respectively passed through purification columns to remove impurities. Under anhydrous and oxygen-free conditions, ethylene, butadiene, solvent and catalyst are introduced into a polymerization unit from a bottom feed port, and polymerization reactions are sequentially carried out in three or four reactors connected in series;
[0010] S2. When the reacted solution is discharged from the polymerization unit, a deactivator and an antioxidant are added in situ in the pipeline and enter the liquid storage tank;
[0011] S3, after the glue liquid enters the coagulation kettle from the liquid storage tank, the product is separated from the unreacted monomers and the solvent by water vapor, the ethylene-butadiene copolymer glue particles obtained after coagulation are sent to the drying unit, and the unreacted monomers and the solvent are returned to the feeding unit for recycling after purification.
[0012] Preferably, the reaction conditions of the polymerization reaction in step S1 are as follows:
[0013] S11, after entering the first reactor, the saturated vapor pressure is controlled to be 0.5MPa-5MPa, and the reaction temperature is 30°C-50°C;
[0014] S12, after entering the second reactor, the saturated vapor pressure is controlled to be 0.4MPa-3MPa, and the reaction temperature is 50℃-60℃;
[0015] S13, after entering the third reactor, the saturated vapor pressure is controlled to be 0.3MPa-2MPa, and the reaction temperature is 60°C-70°C;
[0016] S14. If the polymerization unit includes four reactors, after entering the fourth reactor, the saturated vapor pressure is controlled to be 0.2MPa-1.5MPa and the reaction temperature is controlled to be 70°C-80°C.
[0017] The above reaction conditions are more preferably that the ethylene pressure of the first kettle is 0.5MPa-3MPa, the ethylene pressure of the second kettle is 0.4MPa-2MPa, the ethylene pressure of the third kettle is 0.3MPa-1.5MPa, and the ethylene pressure of the fourth kettle is 0.2MPa-1MPa;
[0018] Most preferably, the ethylene pressure of the first kettle is 0.5 MPa to 2 MPa, the ethylene pressure of the second kettle is 0.4 MPa to 2 MPa, the ethylene pressure of the third kettle is 0.3 MPa to 1 MPa, and the ethylene pressure of the fourth kettle is 0.3 MPa to 0.8 MPa.
[0019] Preferably, the polymerization reaction time of each reactor is 40 min to 70 min, more preferably 45 min to 65 min, and most preferably 50 min to 60 min. The polymerization reaction time is the time from when the material enters the reactor inlet to when it leaves the reactor.
[0020] Preferably, the solvent is selected from one or a combination of at least two of toluene, xylene, n-pentane, n-hexane, cyclohexane, n-heptane, n-octane, n-nonane, n-decane, methylcyclopentane, methylcyclohexane, isopentane, isohexane, isoheptane, isooctane, isononane and isodecane.
[0021] Preferably, the catalyst comprises a co-catalyst and a main catalyst;
[0022] The main catalyst is selected from one or a combination of at least two of a restricted geometry rare earth catalyst, a monocyclopentadienyl rare earth catalyst, and a non-cyclopentadienyl rare earth catalyst;
[0023] The co-catalyst includes a main group alkyl reagent and / or an organic boron reagent.
[0024] Preferably, the main catalyst is selected from rare earth catalysts 1 to 6 having the following structures:
[0025]
[0026] Preferably, the main group alkyl reagent is selected from one or a combination of at least two of trimethylaluminum, triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, methylaluminoxane (MAO), modified methylaluminoxane (MMAO), dried methylaluminoxane (DMAO), supported MAO (silicon dioxide as a carrier), diethylaluminum hydride, diisobutylaluminum hydride, dibutylmagnesium, and diethylzinc;
[0027] The organic boron reagent is selected from one of trispentafluorophenyl boron, triphenyl carbon tetrakis (pentafluorophenyl boron), N,N dimethylaniline tetrakis (pentafluorophenyl boron), N,N di(hexadecyl)aniline tetrakis (pentafluorophenyl boron), and N,N di(octadecyl)aniline tetrakis (pentafluorophenyl boron), or a combination of at least two thereof.
[0028] Preferably, the molar ratio of the main catalyst to butadiene is in the range of 1:5000 to 1:200000; the molar ratio of the main catalyst to the organic boron reagent is 1:0 to 1:2; the molar ratio of the main catalyst to the main group alkyl reagent is 1:20 to 1:5000.
[0029] Preferably, the ethylene pressure is 0.2MPa-5MPa; the concentration of butadiene monomer entering the first reactor is 8g / 100mL-20g / 100mL; the initial temperature of the mixed solution of butadiene, ethylene and inert solvent before entering the reactor is 20°C-40°C.
[0030] Preferably, the operating pressure of the coagulation reactor is 0.1 MPa(G) to 1 MPa(G).
[0031] The present invention also provides an ethylene-butadiene copolymer prepared by the above production method.
[0032] Compared with the prior art, the specific beneficial effects of the present invention are:
[0033] The invention relates to an industrial production system and method for continuously producing ethylene-butadiene copolymers. Three or four reactors are used in series, and a method of gradually increasing the temperature and gradually decreasing the ethylene pressure is adopted. The system can effectively control the uniform distribution of the two structural units of ethylene and butadiene in the molecular chain of the ethylene-butadiene copolymer while improving the conversion rate of the butadiene monomer and reducing the viscosity of the rubber solution, thereby providing a set of solutions for the continuous production of ethylene and butadiene on an industrial device.
[0034] The industrial verification results show that the production method provided by the present invention can be used to continuously produce ethylene-butadiene copolymer with a polymerization activity of 4.1×10 6 g / (mol·h)~5.7×10 6 g / (mol·h), the single-pass butadiene conversion rate is 67% to 78%, and the number average molecular weight of the ethylene-butadiene copolymer is 14.7×10 4 g / mol~20.5×10 4 g / mol, the molecular weight distribution is 1.73-2.43, and the molar insertion rate of butadiene is 44%-47%. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The present invention is a schematic flow chart of a continuous production system and method for ethylene-butadiene copolymer;
[0036] Figure 2 This is a schematic diagram of the appearance of the ethylene-butadiene copolymer n-hexane glue solution in Example 2;
[0037] Figure 3 This is a schematic diagram of the appearance of the ethylene-butadiene copolymer dry rubber in Example 2;
[0038] Figure 4 This is the GPC spectrum of the ethylene-butadiene copolymer in Example 2. DETAILED DESCRIPTION
[0039] In order to make the technical solution of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the specification of the present invention. It should be noted that the following embodiments are only used to better understand the technical solution of the present invention and should not be understood as a limitation to the present invention.
[0040] Example 1.
[0041] In the first step, cyclohexane is used as the polymerization solvent, and all raw materials are purified through a refining system to reduce the water and oxygen content in cyclohexane, ethylene and butadiene to below 1 ppm.
[0042] In the second step, the polymerization reactor was purged with nitrogen and flushed with purified cyclohexane for 8 h.
[0043] In the third step, cyclohexane at 23 L / h, butadiene at 3 kg / h, ethylene at 1200 L / h and the main group alkyl reagent (Al i Bu3, 3.4wt% cyclohexane solution) is mixed in situ in the pipeline at a flow rate of 0.3L / h and then enters the polymerization reactor; the mixture solution of the main catalyst 4 and the organic boron salt (1.0g / L toluene solution) is mixed online with the above mixed solution through the pipeline at a flow rate of 0.3L / h and then enters the polymerization reactor. All raw materials are bottom-fed, the reaction temperature of the first reactor is controlled at 40±3℃, the reaction temperature of the second reactor is controlled at 53±5℃, the reaction temperature of the third reactor is controlled at 63±3℃, and the reaction temperature of the fourth reactor is controlled at 73±3℃, and the continuous operation is 72h. When the reacted solution is discharged from the polymerization unit, a deactivator and an antioxidant are added in situ in the pipeline and enter the liquid storage tank to obtain ethylene-butadiene copolymer n-hexane glue.
[0044] In the fourth step, after the glue liquid enters the coagulation kettle from the liquid storage tank, the product is separated from the unreacted monomers and the solvent by water vapor, and the ethylene-butadiene copolymer glue particles obtained after coagulation are sent to the drying unit to obtain ethylene-butadiene copolymer dry glue, and the unreacted monomers and solvent are returned to the feeding unit for recycling after purification.
[0045] The obtained copolymer was tested, and the test results are as follows:
[0046] The polymerization activity was 4.1×10 6g / (mol.h), the butadiene conversion rate was 67%; the number average molecular weight of the ethylene-butadiene copolymer was 151,000, the molecular weight distribution was 1.99, and the butadiene molar insertion rate was 46%.
[0047] Example 2.
[0048] In the first step, cyclohexane is used as the polymerization solvent, and all raw materials are purified through a refining system to reduce the water and oxygen content in n-hexane, ethylene and butadiene to below 1 ppm.
[0049] In the second step, the polymerization reactor was purged with nitrogen and flushed with purified n-hexane for 8 h.
[0050] In the third step, n-hexane at 23 L / h, butadiene at 3 kg / h, ethylene at 1200 L / h and the main group alkyl reagent (Al i Bu3, 3.4wt% cyclohexane solution) is mixed in situ in the pipeline at a flow rate of 0.3L / h and then enters the polymerization reactor; the mixture solution of the main catalyst 4 and the organic boron salt (1.0g / L toluene solution) is mixed with the above mixed solution online through the pipeline at a flow rate of 0.3L / h and then enters the polymerization reactor. All raw materials are bottom-fed, the reaction temperature of the first reactor is controlled at 40±3℃, the reaction temperature of the second reactor is controlled at 53±3℃, the reaction temperature of the third reactor is controlled at 63±3℃, and the reaction temperature of the fourth reactor is controlled at 73±3℃, and the continuous operation is 72h. When the reacted solution is discharged from the polymerization unit, a deactivator and an antioxidant are added in situ in the pipeline and enter the liquid storage tank to obtain ethylene-butadiene copolymer n-hexane glue.
[0051] In the fourth step, after the glue liquid enters the coagulation reactor from the liquid storage tank, the product is separated from the unreacted monomers and the solvent by water vapor, and the ethylene-butadiene copolymer glue particles obtained after coagulation are sent to the drying unit to obtain ethylene-butadiene copolymer dry glue, and the unreacted monomers and solvent are returned to the feeding unit for recycling after purification. The appearance schematic diagram of the ethylene-butadiene copolymer n-hexane glue liquid obtained in this embodiment is shown in Figure 2 , the appearance diagram of ethylene-butadiene copolymer dry glue is shown in Figure 3 .
[0052] The obtained copolymer was tested and the results were as follows:
[0053] The polymerization activity was 4.3×10 6 g / (mol.h), butadiene conversion rate was 70%; GPC spectrum of copolymer is shown in Figure 4 The number average molecular weight of the ethylene-butadiene copolymer is 147,000, the molecular weight distribution is 2.43, and the butadiene molar insertion rate is 44%.
[0054] Example 3.
[0055] In the first step, toluene is used as the polymerization solvent, and all raw materials are purified through a refining system to reduce the water and oxygen content in toluene, ethylene and butadiene to below 1 ppm.
[0056] In the second step, the polymerization reactor was purged with nitrogen and flushed with purified toluene for 8 h.
[0057] In the third step, toluene was added at 23 L / h, butadiene at 3 kg / h, ethylene at 1200 L / h, and the main group alkyl reagent (Al i Bu3, 3.4wt% cyclohexane solution) is mixed in situ in the pipeline at a flow rate of 0.3L / h and then enters the polymerization reactor; the mixture solution of the main catalyst 4 and the organic boron salt (1.0g / L toluene solution) is mixed online with the above mixed solution through the pipeline at a flow rate of 0.3L / h and then enters the polymerization reactor. All raw materials are bottom-fed, the reaction temperature of the first reactor is controlled at 40±3℃, the reaction temperature of the second reactor is controlled at 53±3℃, the reaction temperature of the third reactor is controlled at 63±3℃, and the reaction temperature of the fourth reactor is controlled at 73±3℃, and the continuous operation is 72h. When the reacted solution is discharged from the polymerization unit, a deactivator and an antioxidant are added in situ in the pipeline and enter the liquid storage tank to obtain an ethylene-butadiene copolymer toluene glue solution.
[0058] In the fourth step, after the glue liquid enters the coagulation kettle from the liquid storage tank, the product is separated from the unreacted monomers and the solvent by water vapor, and the ethylene-butadiene copolymer glue particles obtained after coagulation are sent to the drying unit to obtain ethylene-butadiene copolymer dry glue, and the unreacted monomers and solvent are returned to the feeding unit for recycling after purification.
[0059] The obtained copolymer was tested and the results were as follows:
[0060] The polymerization activity was 5.7×10 6 g / (mol.h), the butadiene conversion rate was 78%; the number average molecular weight of the ethylene-butadiene copolymer was 205,000, the molecular weight distribution was 1.73, and the butadiene molar insertion rate was 47%.
[0061] The above is a detailed introduction to a process system and method for continuously producing ethylene-butadiene copolymers provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method and its core ideas of the present invention, including the best mode, and also enables any technician in the field to practice the present invention, including manufacturing and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, the present invention can also be improved and modified in several ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements that are not different from the textual expression of the claims, or if they include equivalent structural elements that are not substantially different from the textual expression of the claims, then these other embodiments should also be included in the scope of the claims.
Claims
1. A method for continuous production of ethylene-butadiene copolymer, characterized in that: The method is implemented by using an industrial production system of ethylene-butadiene copolymer; The industrial production system of ethylene-butadiene copolymer comprises a feeding unit, a polymerization unit, a liquid storage tank, a coagulation kettle and a product drying unit; The feeding unit includes an ethylene storage tank, an ethylene purification column, butadiene, a butadiene purification column, a catalyst storage tank and a solvent storage tank; the polymerization unit includes three or four reaction kettles connected in series; the coagulation kettle is composed of one or more stirring kettles connected in series; The continuous production method specifically comprises the following steps: S1. Ethylene and butadiene are respectively passed through purification columns to remove impurities. Under anhydrous and oxygen-free conditions, ethylene, butadiene, solvent and catalyst are introduced into a polymerization unit from a bottom feed port, and polymerization reactions are sequentially carried out in three or four reactors connected in series; S2. When the reacted solution is discharged from the polymerization unit, a deactivator and an antioxidant are added in situ in the pipeline and enter the liquid storage tank; S3, after the glue liquid enters the coagulation kettle from the liquid storage tank, the product is separated from the unreacted monomers and the solvent by water vapor, the ethylene-butadiene copolymer glue particles obtained after coagulation are sent to the drying unit, and the unreacted monomers and the solvent are returned to the feeding unit for recycling after purification.
2. The method for continuous production of ethylene-butadiene copolymer according to claim 1, characterized in that: The reaction conditions of the polymerization reaction in step S1 are specifically as follows: S11, after entering the first reactor, the saturated vapor pressure is controlled to be 0.5MPa-5MPa, and the reaction temperature is 30°C-50°C; S12, after entering the second reactor, the saturated vapor pressure is controlled to be 0.4MPa-3MPa, and the reaction temperature is 50℃-60℃; S13, after entering the third reactor, the saturated vapor pressure is controlled to be 0.3MPa-2MPa, and the reaction temperature is 60°C-70°C; S14. If the polymerization unit includes four reactors, after entering the fourth reactor, the saturated vapor pressure is controlled to be 0.2MPa-1.5MPa and the reaction temperature is controlled to be 70°C-80°C.
3. The method for continuous production of ethylene-butadiene copolymer according to claim 2, characterized in that: The polymerization reaction time of each kettle is 40min to 70min.
4. The method for continuous production of ethylene-butadiene copolymer according to claim 1, characterized in that: The solvent is selected from one or a combination of at least two of toluene, xylene, n-pentane, n-hexane, cyclohexane, n-heptane, n-octane, n-nonane, n-decane, methylcyclopentane, methylcyclohexane, isopentane, isohexane, isoheptane, isooctane, isononane and isodecane.
5. The method for continuous production of ethylene-butadiene copolymer according to claim 1, characterized in that: The catalyst includes a co-catalyst and a main catalyst; The main catalyst is selected from one or a combination of at least two of a restricted geometry rare earth catalyst, a monocyclopentadienyl rare earth catalyst, and a non-cyclopentadienyl rare earth catalyst; The co-catalyst includes a main group alkyl reagent and / or an organic boron reagent.
6. The method for continuous production of ethylene-butadiene copolymer according to claim 1, characterized in that: The main catalyst is selected from rare earth catalysts 1 to 6 with the following structures:
7. The method for continuous production of ethylene-butadiene copolymer according to claim 5, characterized in that: The main group alkyl reagent is selected from one or a combination of at least two of trimethylaluminum, triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, methylaluminoxane, modified methylaluminoxane, dried methylaluminoxane, silica-supported MAO, diethylaluminum hydride, diisobutylaluminum hydride, dibutylmagnesium, and diethylzinc; The organic boron reagent is selected from one of trispentafluorophenyl boron, triphenyl carbon tetrakis (pentafluorophenyl boron), N,N dimethylaniline tetrakis (pentafluorophenyl boron), N,N di(hexadecyl)aniline tetrakis (pentafluorophenyl boron), and N,N di(octadecyl)aniline tetrakis (pentafluorophenyl boron), or a combination of at least two thereof.
8. The method for continuous production of ethylene-butadiene copolymer according to claim 7, characterized in that: The molar ratio of the main catalyst to butadiene is in the range of 1:5000 to 1:200000; the molar ratio of the main catalyst to the organic boron reagent is in the range of 1:0 to 1:2; and the molar ratio of the main catalyst to the main group alkyl reagent is in the range of 1:20 to 1:5000.
9. The method for continuous production of ethylene-butadiene copolymer according to claim 1, characterized in that: The ethylene pressure is 0.2MPa~5MPa; the concentration of butadiene monomer entering the first reactor is 8g / 100mL~20g / 100mL; the initial temperature of the mixed liquid of butadiene, ethylene and inert solvent before entering the reactor is 20℃~40℃; the operating pressure of the condensation reactor is 0.1MPa(G)~1MPa(G).
10. An ethylene-butadiene copolymer, characterized in that: The ethylene-butadiene copolymer is prepared by the production method according to any one of claims 1 to 9, wherein the number average molecular weight of the ethylene-butadiene copolymer is 14.7×10 4 g / mol~20.5×10 4 g / mol, the molecular weight distribution is 1.73-2.43, and the molar insertion rate of butadiene is 44%-47%.