Polymer as well as preparation method and application thereof
Through the design and preparation method of new polymers, combined with polymer monomers and crosslinked monomers, the problems of existing materials taking into account both light transmittance and mechanical strength are solved, and polymers with high transmittance and mechanical properties are achieved. Medical devices for eye.
Patent Information
- Application Number
- CN202411223951.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-26
AI Technical Summary
Existing eye device materials are difficult to balance between maintaining high light transmission and mechanical strength, and cannot meet the increasing functional needs of eye devices.
A novel polymer is prepared by a specific polymer structure and a segmented heating treatment method, combining crosslinked monomers and ultraviolet absorbers to improve the refractive index, mechanical properties and light transmittance of the material.
It achieves high transmittance and good mechanical properties of polymers in the wavelength range of 400-780nm. It is suitable for eye medical devices such as foldable intraocular lenses, and has excellent molding and processing performance and stability.
Smart Images

Figure CN119019599A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of optical materials, and in particular relates to a polymer and a preparation method and use thereof. Background Art
[0002] Nowadays, a large number of ocular devices use a combination of acrylic monomers as a copolymer raw material to prepare raw materials. This method can produce a variety of polymer devices with excellent performance. Due to the needs of vision, such materials need to maintain high light transmittance, and at the same time, the materials need to meet sufficient mechanical strength. Therefore, it is of great significance to design and manufacture new polymer materials with excellent performance to meet the increasing functional requirements of ocular devices. Summary of the invention
[0003] The purpose of the present application is to provide a polymer and a preparation method and use thereof, aiming to provide a new polymer material suitable for ocular devices.
[0004] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:
[0005] In a first aspect, the present application provides a polymer, wherein the polymer is obtained by polymerizing at least one polymerizable monomer, wherein the polymerizable monomer includes a first monomer, and the structural formula of the first monomer is shown in the following formula I or formula II:
[0006]
[0007] Wherein, A is selected from hydrogen or C1-C6 alkyl;
[0008] R1 is selected from the group consisting of hydrogen, a halogen atom, a cyano group, a phenyl group, a C1-C6 alkyl group, a C1-C6 alkoxy group, a C1-C6 alkyl-substituted phenyl group, and a C1-C6 alkoxy-substituted phenyl group;
[0009] R2 is selected from one of the alkyl groups; R3 is selected from one of the alkylene groups;
[0010] n is a positive integer; m is a positive integer.
[0011] In a second aspect, the present application provides a method for preparing a polymer, comprising the following steps: providing the polymerizable monomers as described in the first aspect; mixing the polymerizable monomers, and performing a segmented heating treatment to obtain the polymer.
[0012] In a third aspect, the present application provides a use of the polymer described in the first aspect in preparing an ocular medical device.
[0013] The first aspect of the present application provides a novel polymer that can be used for ophthalmic materials. The polymerized monomers for synthesizing the polymer include a first monomer, which is a monomer containing multiple structures, whose main chain is an acrylate, and whose side group is a group containing a benzene ring. Since the first monomer has a suitable amount of different structures in its monomer structure, such as phenyl, alkyl, acrylic acid group, polyether segment, etc., different types of functional groups are directly integrated into its structure, which has better and more diverse performance, and the first monomer has better homogeneous characteristics, so that the polymer material obtained by polymerization has excellent performance and good uniformity.
[0014] The second aspect of the present application provides a method for preparing a polymer, wherein the polymer is obtained by segmented heating treatment. The preparation method is simple and easy to operate, and is suitable for the preparation of the polymer of the present application and for industrial production.
[0015] The third aspect of the present application provides a use of a polymer in the preparation of ophthalmic medical devices. The polymer of the present application has good optical properties and good molding and processing properties, and the polymer material has a relatively high refractive index in the range of 1.50-1.55 and good folding flexibility, and is suitable for the preparation of foldable intraocular lenses, such as artificial lenses, phakic intraocular lenses, etc. The polymer of the present application can also be used in other ocular medical devices, such as corneal rings, corneal inlays, corneal contact lenses, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0017] Figure 1 This is the appearance diagram of the artificial lens provided in Example 39 of the present application. DETAILED DESCRIPTION
[0018] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0019] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0020] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0021] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0022] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0023] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0024] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, features defined as "first" and "second" may explicitly or implicitly include one or more of the features.
[0025] In a first aspect, an embodiment of the present application provides a polymer, which is obtained by polymerizing at least one polymerizable monomer, wherein the polymerizable monomer includes a first monomer, and the structural formula of the first monomer is shown in the following formula I or formula II:
[0026]
[0027] In the above formula, A, R1, R2 and R3 each independently represent a substituent, wherein A is selected from hydrogen or C1-C6 alkyl;
[0028] R1 is selected from the group consisting of hydrogen, a halogen atom, a cyano group, a phenyl group, a C1-C6 alkyl group, a C1-C6 alkoxy group, a C1-C6 alkyl-substituted phenyl group, and a C1-C6 alkoxy-substituted phenyl group;
[0029] R2 is selected from one of the alkyl groups; R3 is selected from one of the alkylene groups;
[0030] n is the number of repeating units of R1, and n is a positive integer;
[0031] m is the number of repeating units of the -O-R3- segment, and m is a positive integer.
[0032] The term "C1-C6 alkyl" refers to a straight or branched saturated hydrocarbon group containing 1 to 6 carbon atoms. For example, C1-C6 alkyl includes, but is not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, 2-pentyl, 3-pentyl, 2-methyl-2-butyl, 3-methyl-2-butyl, 3-methyl-1-butyl, 2-methyl-1-butyl, n-hexyl, 2-hexyl, 3-hexyl, etc.
[0033] The term "C1-C6 alkoxy" refers to a group formed by connecting an alkyl group containing 1 to 6 carbon atoms to an oxygen atom. For example, C1-C6 alkoxy includes, but is not limited to, methoxy, ethoxy, 1-propoxy, 2-propoxy, 1-butoxy, 1-pentyloxy, 1-hexyloxy, and the like.
[0034] The term "C1-C6 alkyl substituted phenyl" refers to a group formed by replacing a hydrogen atom on a benzene ring with an alkyl group containing 1 to 6 carbon atoms. For example, C1-C6 alkyl substituted phenyl includes but is not limited to benzyl, phenethyl, phenylpropyl, and the like.
[0035] The term "C1-C6 alkoxy substituted phenyl" refers to a group formed by replacing a hydrogen atom on a benzene ring with an alkoxy group containing 1 to 6 carbon atoms. For example, C1-C6 alkoxy substituted phenyl includes but is not limited to methoxyphenyl, ethoxyphenyl, and the like.
[0036] The first monomer of the present application may contain chiral carbon atoms in structural formulas Ⅰ and Ⅱ, and may contain stereoisomers.
[0037] The first monomer of the embodiment of the present application is a monomer containing multiple structures, the main chain of which is acrylate, and the side group is a group containing a benzene ring. It should be noted that the "side group" here refers to the group on both sides of the main chain. Since the molecular chain of the first monomer contains a benzene ring group, it can increase the refractive index and mechanical properties of the polymer, and at the same time make the structural stability of the first monomer better. At the same time, the structural formula of the first monomer also includes -(O-R3) m -segment, -(O-R3) m - is a polyether structural segment, and the introduction of the polyether segment can increase the toughness of the material, thereby making the performance of the first monomer more diverse. Since the first monomer has a suitable amount of different structures in its monomer structure, such as phenyl, alkyl, acrylic acid group, polyether segment, etc., compared with a mixture of polymers with different functional groups, the advantage of the first monomer is that it directly integrates different functional groups, has better homogeneous characteristics, and the polymer material obtained by polymerization has excellent performance and good uniformity. The polymer of the embodiment of the present application can be obtained by polymerization of the first monomer. In some embodiments, the polymer is obtained by polymerization of the same first monomer; in other embodiments, the polymer is obtained by polymerization of two first monomers; in some other embodiments, the polymer is obtained by polymerization of more than two first monomers. It should be noted that, as can be seen from the structural formula of the first monomer, the first monomer is an acrylic compound containing a benzene ring, and the "polymerization" here refers to the polymerization reaction of acrylic acid. The polymerization reaction of acrylic acid can refer to the polymerization reaction method of acrylic acid commonly used in the art, and is not specifically limited here. For example, the polymerization reaction of acrylic acid can be a free radical polymerization reaction, that is, the acrylic compound is connected to the monomer molecules by the formation of chemical bonds under the action of an initiator to form a high molecular polymer.
[0038] In some embodiments, the above A is preferably hydrogen or methyl.
[0039] In some embodiments, the above R1 is preferably hydrogen, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, 2-pentyl, 3-pentyl, 2-methyl-2-butyl, 3-methyl-2-butyl, 3-methyl-1-butyl, 2-methyl-1-butyl, n-hexyl, 2-hexyl, 3-hexyl, etc. n is preferably 1, 2, 3, 4 or 5.
[0040] In some embodiments, the above R2 is preferably hydrogen, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, 2-pentyl, 3-pentyl, 2-methyl-2-butyl, 3-methyl-2-butyl, 3-methyl-1-butyl, 2-methyl-1-butyl, n-hexyl, 2-hexyl, 3-hexyl, etc.
[0041] In some embodiments, the above R3 is preferably -CH2-, -(CH2)2-, -(CH2)3-, -(CH2)4-, -(CH2)5-, -(CH2)6-, etc.; m is preferably 1, 2, 3, 4, 5 or 6.
[0042] As an example, the first monomer includes at least one of the following compounds:
[0043]
[0044]
[0045] The polymer prepared by using the first monomer not only has more suitable mechanical properties, but also has higher light transmittance, and is more suitable for the field of optical materials.
[0046] In some embodiments, the polymerized monomer further includes a second monomer, and the second monomer includes at least one of a monofunctional acrylic monomer and a vinyl monomer.
[0047] In the present application, the polymer can also be obtained by polymerizing the first monomer and the second monomer. The obtained polymer also has suitable mechanical properties and good light transmittance, and is suitable for the field of optical materials. The second monomer is selected from at least one of monofunctional acrylic monomers. For example, the second monomer can be selected from methyl methacrylate, phenylethyl methacrylate, ethoxyethoxymethyl methacrylate, etc. Due to space limitations and for the sake of simplicity, the specific compounds that can be selected are no longer exhaustively listed here.
[0048] In some embodiments, the monofunctional acrylic monomer includes at least one of 2-(2-methoxyethoxy)ethyl methacrylate (denoted as B1), 2-phenoxyethyl acrylate (denoted as B2), butyl methacrylate (denoted as B3), ethoxyethoxyethyl acrylate (denoted as B4), polyethylene glycol methyl ether methacrylate (number average molecular weight of 475 g / mol) (denoted as B5), ethylene glycol phenyl ether acrylate (denoted as B6), 2-phenylethyl acrylate (denoted as B7), hydroxyethyl acrylate (denoted as B8), phenylethyl methacrylate (denoted as B9), 2-ethoxyethyl methacrylate (denoted as B10), methyl methacrylate (denoted as B11), ethyl methacrylate (denoted as B12), and hydroxyethyl methacrylate (denoted as B13).
[0049] The polymer prepared by polymerizing the second monomer and the first monomer not only has more suitable mechanical properties, but also has higher light transmittance, and is more suitable for the field of optical materials.
[0050] In some embodiments, based on the total mass of the polymerized monomers used to synthesize the polymer, the amount of the second monomer is 20 to 40 wt%. Here, it means that when the polymerized monomer is polymerized using a mixture of the first monomer and the second monomer, the amount of the second monomer accounts for 20 wt% to 40 wt% of the total weight of the polymerized monomers used. As an example, the amount of the second monomer includes but is not limited to any point value of 20 wt%, 22 wt%, 24 wt%, 26 wt%, 28 wt%, 30 wt%, 32 wt%, 34 wt%, 36 wt%, 38 wt%, 40 wt%, or any range point value between the two. If the amount of the second monomer is too much or too little, it may affect the mechanical properties and refractive index of the polymer. When the amount of the second monomer is controlled within the above range, the obtained polymer has a maximum transmittance of >90% in the wavelength range of 400 nm-780 nm, an average transmittance of >88%, a refractive index of 1.51 to 1.55, an Abbe number of 40 to 48, and a Tg of <15 ° C, which is suitable for foldable intraocular lens materials.
[0051] In some embodiments, the polymerizable monomer further comprises a crosslinking monomer, and the crosslinking monomer comprises at least one of a difunctional acrylic monomer and a trifunctional acrylic monomer. By adding a crosslinking monomer to the polymerizable monomer, the mechanical strength of the polymer can be better adjusted, making it more suitable for the field of optical materials.
[0052] In some embodiments, the crosslinking monomer includes ethylene glycol diacrylate, diethylene glycol diacrylate, allyl acrylate, 1,3-propylene glycol diacrylate, 2,3-propylene glycol diacrylate, 1,6-hexanediol diacrylate, 1,4-butylene glycol diacrylate, triethylene glycol diacrylate, cyclohexane-1,1-diyl dimethanol diacrylate, 1,4-cyclohexanediol diacrylate, 1,3-adamantanediol diacrylate, 1,3-adamantanedimethyl diacrylate, 2,2-diethyl-1,3-propylene glycol diacrylate, 2,2-diisobutyl-1,3-propylene glycol diacrylate, 1,3-cyclohexanedimethyl diacrylate, 1,4-cyclohexanedimethyl diacrylate, neopentyl glycol diacrylate, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, methyl dimethacrylate, 1,3-propylene glycol dimethacrylate, 2,3-propylene glycol dimethacrylate, 1,6-hexanediol dimethacrylate, 1,4-butylene glycol dimethacrylate, triethylene glycol dimethacrylate, cyclohexane-1,1-diyl dimethanol dimethacrylate, 1,4-cyclohexanediol dimethacrylate, 1,3-adamantanediol dimethacrylate, 1,3-adamantanediol dimethacrylate, 2,2-diethyl-1,3-propylene glycol dimethacrylate, 2,2-diisobutyl-1,3-propylene glycol dimethacrylate, 1,3-cyclohexanedimethyl dimethacrylate, 1,4-cyclohexanedimethyl dimethacrylate, neopentyl glycol dimethacrylate, poly(ethylene glycol) dimethacrylate, and poly(ethylene glycol) dimethacrylate. At least one of poly(ethylene glycol) dimethacrylate, poly(ethylene glycol) diacrylate, poly(propylene glycol) dimethacrylate, and poly(propylene glycol) diacrylate.
[0053] In some embodiments, the cross-linking monomer includes at least one of ethylene glycol dimethacrylate (denoted as C1), trimethylolpropane trimethacrylate (denoted as C2), butanediol dimethacrylate (denoted as C3), polyethylene glycol dimethacrylate (number average molecular weight Mn is 200g / mol) (denoted as C4), polyethylene glycol dimethacrylate (number average molecular weight Mn is 550g / mol) (denoted as C5), neopentyl glycol dimethacrylate (denoted as C6), polyethylene glycol dimethacrylate (number average molecular weight Mn is 1100g / mol) (denoted as C7), dipropylene glycol diacrylate (denoted as C8), and butanediol diacrylate (denoted as C9). The above cross-linking monomer is more compatible with the first monomer and the second monomer of the present application, and the obtained polymer is more suitable for the field of ocular medical devices.
[0054] In some embodiments, based on the total mass of the polymerized monomers used to synthesize the polymer, the amount of the cross-linking monomer is 0.25wt% to 30wt%. As an example, the amount of the cross-linking monomer includes but is not limited to any one of 0.25wt%, 0.5wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt% or any range of values between two of them. The amount of the cross-linking monomer plays an important role in strengthening and improving the mechanical properties of the polymer. When the mass proportion of the cross-linking monomer is controlled within the above range, the cross-linking reaction speed is fast and the obtained polymer has good mechanical strength.
[0055] In some embodiments, the polymerizable monomer further includes an ultraviolet light absorber. Since ultraviolet light is a harmful light, if it is not properly protected, ultraviolet light will enter the eye from the outside, causing varying degrees of damage to the cornea, pupil, lens, vitreous body, retina, etc. The ultraviolet light absorber can absorb the ultraviolet light in sunlight and fluorescent light sources to protect the eyes from ultraviolet light damage.
[0056] In some embodiments, the ultraviolet absorber includes but is not limited to 2-(4-benzoyl-3-hydroxyphenoxy)ethyl acrylate (denoted as E1), 2-[3-(2H-benzotriazol-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate (denoted as E2), etc. The above ultraviolet absorber has strong ultraviolet absorption, light color, good compatibility with the first monomer, the second monomer, the cross-linking monomer, etc., and is suitable for the polymer of the present application.
[0057] In some embodiments, the amount of the ultraviolet absorber is 0.2 wt% to 2 wt% based on the total weight of the polymerized monomers used to synthesize the polymer. As an example, the amount of the ultraviolet absorber includes but is not limited to any one of 0.2 wt%, 0.4 wt%, 0.6 wt%, 0.8 wt%, 1.0 wt%, 1.2 wt%, 1.4 wt%, 1.6 wt%, 1.8 wt%, 2.0 wt% or any range of values between two of them.
[0058] In some embodiments, the polymerizable monomer further includes an initiator. Acrylic acid polymerization can be carried out by free radical polymerization, and the activity of the initiator promotes cross-linking between polymer molecules, thereby increasing the strength of the polymer.
[0059] In some embodiments, the initiator includes at least one of 2,5-dimethyl-2,5-bis(2-ethylhexanoic acid peroxide)hexane (denoted as D1), bis(4-tert-butylcyclohexyl)peroxydicarbonate (denoted as D2), and azobisisobutyronitrile (denoted as D3). The initiator can accelerate the polymerization reaction, and the selection of the initiator should be based on the properties of the polymerization monomer. The above initiators have high chemical activity and are suitable for the polymer preparation reaction of the present application.
[0060] In some embodiments, the amount of the initiator is 0.1 wt% to 5 wt% based on the total weight of the polymerized monomers used to synthesize the polymer. As an example, the amount of the initiator includes, but is not limited to, any one of 0.1 wt%, 0.5 wt%, 1.0 wt%, 1.5 wt%, 2.0 wt%, 2.5 wt%, 3.0 wt%, 3.5 wt%, 4.0 wt%, 4.5 wt%, 5.0 wt% or any range of values between two of them.
[0061] In some embodiments, the polymer has a refractive index of 1.51 to 1.55, an Abbe number of 37 to 54, and an average transmittance in the visible light band greater than 88%.
[0062] In some embodiments, the polymer material obtained by homopolymerizing or copolymerizing the first monomer shown in structural formula I has a relatively high refractive index of more than 1.50, an Abbe number greater than 37, and an average transmittance in the visible light band of more than 88%.
[0063] In some embodiments, the first monomer of structural formula II is copolymerized with a cross-linking monomer to obtain a polymer material having a relatively high refractive index of more than 1.50, an Abbe number greater than 40, and an average transmittance in the visible light band of more than 88%.
[0064] In some embodiments, the first monomer of structural formula I is copolymerized with the second monomer to obtain a polymer having a maximum transmittance of >90% in the wavelength range of 400nm to 780nm, an average transmittance of >88%, a refractive index of 1.51 to 1.55, an Abbe number of 40 to 48, and a Tg of <15°C, which is suitable for foldable intraocular lens materials.
[0065] In some embodiments, the first monomer of structural formula I is copolymerized with the first monomer and the second monomer of formula II to obtain a polymer having a maximum transmittance of >90% in the wavelength range of 400nm to 780nm, an average transmittance of >88%, a refractive index of 1.51 to 1.55, an Abbe number of 40 to 48, and a Tg of <15°C, which is suitable for foldable intraocular lens materials.
[0066] In a second aspect, an embodiment of the present application provides a method for preparing a polymer, comprising the following steps: providing polymerizable monomers; mixing the polymerizable monomers, and performing a segmented heating treatment to obtain a polymer. The preparation method is simple and easy to operate, suitable for the preparation of the polymer of the present application, and suitable for industrial production.
[0067] In some embodiments, the preparation method of the polymer is as follows: accurately weigh the required polymer monomer materials, mix the polymer monomer materials, and then ultrasonically dissolve the polymer monomers into a transparent state. After the dissolved mixture is filtered through a polytetrafluoroethylene filter membrane, it is transferred to a curing mold. Then, it is placed in an oven and heated and cured in sections.
[0068] In some embodiments, the segmented heating treatment includes the following three stages of heating: the first stage heating condition is heating at 45-55°C for 1-3 hours, thereby allowing each polymerization monomer to undergo preliminary curing under relatively mild conditions, and the monomer molecules continuously react to form long-chain polymers; the second stage heating condition is heating at 65-75°C for 2-4 hours, thereby allowing the polymer to further cross-link and completely cure as the polymerization reaction proceeds; the third stage heating condition is heating at 80-120°C for 12-20 hours, thereby reducing the small molecule residues in the polymer material.
[0069] The third aspect of the embodiment of the present application provides a use of a polymer in preparing an optical material. The polymer of the present application has good optical properties and good molding and processing properties, and the polymer material has a high refractive index of more than 1.50, and is suitable for the preparation of foldable intraocular lenses, such as intraocular lenses, phakic intraocular lenses, etc. The polymer of the present application can also be used in other ocular medical devices, such as corneal rings, corneal inlays, corneal contact lenses, etc.
[0070] The following describes the invention in conjunction with specific embodiments.
[0071] Example 1
[0072] An embodiment of the present application provides a polymer. Based on the total mass of the polymerized monomers used to synthesize the polymer, the polymerized monomers of the polymer include: a first monomer A2: 95.88 wt%, a cross-linking monomer C1: 2.40 wt%, 2,5-dimethyl-2,5-bis(2-ethylhexanoic acid peroxide)hexane (initiator): 0.77 wt%, and 2-(4-benzoyl-3-hydroxyphenoxy)ethyl acrylate (ultraviolet absorber): 0.95 wt%.
[0073] The preparation method of the polymer comprises the following steps: mixing the polymerization monomers and dissolving them by ultrasonication, then putting them into an oven and heating them to 50°C for curing for 2 hours, then heating them to 70°C for curing for 3 hours, and then heating them to 85°C for curing for 16 hours to obtain the polymer.
[0074] Example 2
[0075] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A1: 93.75wt%, crosslinking monomer C1: 1.56wt%, crosslinking monomer C2: 1.25wt%, 2,5-dimethyl-2,5-bis(2-ethylhexanoic acid peroxide) hexane (initiator): 1.88wt%, 2-(4-benzoyl-3-hydroxyphenoxy)ethyl acrylate (ultraviolet absorber): 1.56wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0076] Example 3
[0077] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A3: 93.75wt%, crosslinking monomer C1: 1.56wt%, crosslinking monomer C2: 1.25wt%, 2,5-dimethyl-2,5-bis(2-ethylhexanoic acid peroxide) hexane (initiator): 1.88wt%, 2-(4-benzoyl-3-hydroxyphenoxy)ethyl acrylate (ultraviolet absorber): 1.56wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0078] Example 4
[0079] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A1: 26.88wt%, first monomer A4: 67.20wt%, crosslinking monomer C3: 2.15wt%, crosslinking monomer C4: 1.34wt%, bis(4-tert-butylcyclohexyl) peroxydicarbonate (initiator): 1.21wt%, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate (ultraviolet absorber): 1.22wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0080] Example 5
[0081] The embodiment of the present application provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A1: 13.89wt%, first monomer A4: 27.78wt%, first monomer A5: 38.89wt%, first monomer A6: 13.89wt%, crosslinking monomer C1: 1.39wt%, crosslinking monomer C2: 1.11wt%, 2,5-dimethyl-2,5-bis(2-ethylhexanoic acid peroxide) hexane (initiator): 1.67wt%, 2-(4-benzoyl-3-hydroxyphenoxy)ethyl acrylate (ultraviolet absorber): 1.38wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0082] Example 6
[0083] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A1: 74.99wt%, first monomer A5: 15.30wt%, crosslinking monomer C1: 1.07wt%, crosslinking monomer C5: 6.12wt%, bis (4-tert-butylcyclohexyl) peroxydicarbonate (initiator): 1.22wt%, 2- (4-benzoyl-3-hydroxyphenoxy) ethyl acrylate (ultraviolet absorber): 1.30wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0084] Example 7
[0085] The embodiment of the present application provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A1: 55.11wt%, second monomer B1: 27.56wt%, crosslinking monomer C6: 2.07wt%, crosslinking monomer C5: 13.78wt%, bis(4-tert-butylcyclohexyl) peroxydicarbonate (initiator): 0.66wt%, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate (ultraviolet absorber): 0.82wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0086] Example 8
[0087] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A1: 55.11wt%, second monomer B2: 27.56wt%, crosslinking monomer C6: 2.07wt%, crosslinking monomer C5: 13.78wt%, bis(4-tert-butylcyclohexyl) peroxydicarbonate (initiator): 0.66wt%, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate (ultraviolet absorber): 0.82wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0088] Example 9
[0089] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A1: 55.11wt%, second monomer B3: 27.56wt%, crosslinking monomer C6: 2.07wt%, crosslinking monomer C5: 13.78wt%, bis(4-tert-butylcyclohexyl) peroxydicarbonate (initiator): 0.66wt%, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate (ultraviolet absorber): 0.82wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0090] Example 10
[0091] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A1: 47.57wt%, second monomer B4: 35.68wt%, crosslinking monomer C6: 3.57wt%, crosslinking monomer C7: 11.89wt%, azobisisobutyronitrile (initiator): 0.57wt%, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate (ultraviolet absorber): 0.72wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0092] Embodiment 11
[0093] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A1: 47.57wt%, second monomer B5: 35.68wt%, crosslinking monomer C6: 3.57wt%, crosslinking monomer C7: 11.89wt%, azobisisobutyronitrile (initiator): 0.57wt%, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate (ultraviolet absorber): 0.72wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0094] Example 12
[0095] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A2: 63.8wt%, second monomer B4: 31.90wt%, crosslinking monomer C3: 2.39wt%, bis(4-tert-butylcyclohexyl) peroxydicarbonate (initiator): 0.96wt%, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate (ultraviolet absorber): 0.95wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0096] Embodiment 13
[0097] The embodiment of the present application provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A2: 55.02wt%, second monomer B6: 27.51wt%, second monomer B8: 13.76wt%, crosslinking monomer C3: 2.06wt%, bis (4-tert-butyl cyclohexyl) peroxydicarbonate (initiator): 0.83wt%, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl] ethyl 2-methylacrylate (ultraviolet absorber): 0.82wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0098] Embodiment 14
[0099] The embodiment of the present application provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A2: 55.02wt%, second monomer B7: 27.51wt%, second monomer B8: 13.76wt%, crosslinking monomer C3: 2.06wt%, bis (4-tert-butyl cyclohexyl) peroxydicarbonate (initiator): 0.83wt%, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl] ethyl 2-methylacrylate (ultraviolet absorber): 0.82wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0100] Embodiment 15
[0101] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A4: 59.24wt%, first monomer A6: 11.85wt%, second monomer B9: 23.70wt%, crosslinking monomer C3: 1.90wt%, crosslinking monomer C4: 1.18wt%, bis(4-tert-butylcyclohexyl) peroxydicarbonate (initiator): 1.07wt%, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate (ultraviolet absorber): 1.06wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0102] Example 16
[0103] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A1: 42.41wt%, second monomer B1: 42.41wt%, crosslinking monomer C6: 3.18wt%, crosslinking monomer C7: 10.60wt%, azobisisobutyronitrile (initiator): 0.76wt%, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate (ultraviolet absorber): 0.64wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0104] Embodiment 17
[0105] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A1: 53.82wt%, second monomer B4: 26.91wt%, crosslinking monomer C6: 4.04wt%, crosslinking monomer C7: 13.46wt%, azobisisobutyronitrile (initiator): 0.97wt%, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate (ultraviolet absorber): 0.80wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0106] Embodiment 18
[0107] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A1: 48.44wt%, second monomer B1: 36.33wt%, crosslinking monomer C6: 1.82wt%, crosslinking monomer C7: 12.11wt%, azobisisobutyronitrile (initiator): 0.58wt%, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate (ultraviolet absorber): 0.72wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0108] Embodiment 19
[0109] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A4: 54.05wt%, first monomer A3: 13.51wt%, second monomer B10: 27.03wt%, crosslinking monomer C1: 1.35wt%, crosslinking monomer C2: 1.08wt%, bis (4-tert-butylcyclohexyl) peroxydicarbonate (initiator): 1.62wt%, 2- (4-benzoyl-3-hydroxyphenoxy) ethyl acrylate (ultraviolet absorber): 1.36wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0110] Embodiment 20
[0111] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A4: 52.63wt%, first monomer A6: 15.79wt%, second monomer B7: 26.32wt%, crosslinking monomer C1: 1.32wt%, crosslinking monomer C2: 1.05wt%, bis (4-tert-butylcyclohexyl) peroxydicarbonate (initiator): 1.58wt%, 2- (4-benzoyl-3-hydroxyphenoxy) ethyl acrylate (ultraviolet absorber): 1.31wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0112] Embodiment 21
[0113] The present embodiment provides a polymer, based on the total mass of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A16: 95.88wt%, crosslinking monomer C1: 2.40wt%, 2,5-dimethyl-2,5-bis(2-ethylhexanoic acid peroxide)hexane (initiator): 0.77wt%, 2-(4-benzoyl-3-hydroxyphenoxy)ethyl acrylate (ultraviolet absorber): 0.95wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0114] Embodiment 22
[0115] The present embodiment provides a polymer, based on the total mass of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A10: 95.88wt%, crosslinking monomer C1: 2.40wt%, 2,5-dimethyl-2,5-bis(2-ethylhexanoic acid peroxide) hexane (initiator): 0.77wt%, 2-(4-benzoyl-3-hydroxyphenoxy)ethyl acrylate (ultraviolet absorber): 0.95wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0116] Embodiment 23
[0117] The present embodiment provides a polymer, based on the total mass of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A11: 95.88wt%, crosslinking monomer C1: 2.40wt%, 2,5-dimethyl-2,5-bis(2-ethylhexanoic acid peroxide)hexane (initiator): 0.77wt%, 2-(4-benzoyl-3-hydroxyphenoxy)ethyl acrylate (ultraviolet absorber): 0.95wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0118] Embodiment 24
[0119] The present embodiment provides a polymer, based on the total mass of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A13: 95.88wt%, crosslinking monomer C1: 2.40wt%, 2,5-dimethyl-2,5-bis(2-ethylhexanoic acid peroxide) hexane (initiator): 0.77wt%, 2-(4-benzoyl-3-hydroxyphenoxy)ethyl acrylate (ultraviolet absorber): 0.95wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0120] Embodiment 25
[0121] The present embodiment provides a polymer, based on the total mass of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A12: 95.88wt%, crosslinking monomer C1: 2.40wt%, 2,5-dimethyl-2,5-bis(2-ethylhexanoic acid peroxide) hexane (initiator): 0.77wt%, 2-(4-benzoyl-3-hydroxyphenoxy)ethyl acrylate (ultraviolet absorber): 0.95wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0122] Embodiment 26
[0123] The present embodiment provides a polymer, based on the total mass of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A15: 95.88wt%, crosslinking monomer C1: 2.40wt%, 2,5-dimethyl-2,5-bis(2-ethylhexanoic acid peroxide) hexane (initiator): 0.77wt%, 2-(4-benzoyl-3-hydroxyphenoxy)ethyl acrylate (ultraviolet absorber): 0.95wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0124] Embodiment 27
[0125] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A16: 51.60wt%, first monomer A11: 17.20wt%, second monomer B11: 24.08, cross-linking monomer C1: 2.58wt%, cross-linking monomer C8: 1.38wt%, 2,5-dimethyl-2,5-bis(2-ethylhexanoic acid peroxide) hexane (initiator): 1.72wt%, 2-(4-benzoyl-3-hydroxyphenoxy)ethyl acrylate (ultraviolet absorber): 1.44wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0126] Embodiment 28
[0127] The embodiment of the present application provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A16: 35.65wt%, first monomer A11: 11.88wt%, second monomer B9: 47.54, cross-linking monomer C1: 1.78wt%, cross-linking monomer C8: 0.95wt%, 2,5-dimethyl-2,5-bis(2-ethylhexanoic acid peroxide) hexane (initiator): 1.19wt%, 2-(4-benzoyl-3-hydroxyphenoxy)ethyl acrylate (ultraviolet absorber): 1.01wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0128] Embodiment 29
[0129] The present application embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A12: 53.48wt%, second monomer B12: 40.11, crosslinking monomer C6: 2.67wt%, crosslinking monomer C8: 1.60wt%, 2,5-dimethyl-2,5-bis(2-ethylhexanoic acid peroxide) hexane (initiator): 1.07wt%, 2-[2-hydroxy-5-[2-(methacryloyloxy)ethyl]phenyl]-2H-benzotriazole (ultraviolet absorber): 1.07wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0130] Embodiment 30
[0131] The present application embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A15: 73.94wt%, first monomer A11: 18.48wt%, cross-linking monomer C9: 2.77wt%, cross-linking monomer C3: 1.85wt%, bis(4-tert-butylcyclohexyl) peroxydicarbonate (initiator): 1.66wt%, 2-[2-hydroxy-5-[2-(methacryloyloxy)ethyl]phenyl]-2H-benzotriazole (ultraviolet absorber): 1.30wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0132] Embodiment 31
[0133] The embodiment of the present application provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A15: 62.40wt%, first monomer A13: 31.20wt%, crosslinking monomer C9: 2.34wt%, crosslinking monomer C3: 1.56wt%, bis(4-tert-butylcyclohexyl) peroxydicarbonate (initiator): 1.40wt%, 2-[2-hydroxy-5-[2-(methacryloyloxy)ethyl]phenyl]-2H-benzotriazole (ultraviolet absorber): 1.10wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0134] Embodiment 32
[0135] The present application embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A15: 66.56wt%, second monomer B7: 26.62wt%, crosslinking monomer C9: 2.50wt%, crosslinking monomer C3: 1.66wt%, bis(4-tert-butylcyclohexyl) peroxydicarbonate (initiator): 1.50wt%, 2-[2-hydroxy-5-[2-(methacryloyloxy)ethyl]phenyl]-2H-benzotriazole (ultraviolet absorber): 1.16wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0136] Embodiment 33
[0137] The embodiment of the present application provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A15: 66.89wt%, first monomer A12: 6.69wt%, first monomer A13: 16.72wt%, cross-linking monomer C3: 2.51wt%, cross-linking monomer C2: 1.34wt%, cross-linking monomer C4: 3.34wt%, bis (4-tert-butylcyclohexyl) peroxydicarbonate (initiator): 1.34wt%, 2-acrylic acid 2- (4-benzoyl-3-hydroxyphenoxy) ethyl ester (ultraviolet absorber): 1.17wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0138] Embodiment 34
[0139] The embodiment of the present application provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A15: 62.11wt%, first monomer A14: 18.01wt%, second monomer B13: 10.87wt%, cross-linking monomer C3: 2.33wt%, cross-linking monomer C2: 1.24wt%, cross-linking monomer C4: 3.11wt%, bis (4-tert-butylcyclohexyl) peroxydicarbonate (initiator): 1.24wt%, 2-acrylic acid 2- (4-benzoyl-3-hydroxyphenoxy) ethyl ester (ultraviolet absorber): 1.09wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0140] Embodiment 35
[0141] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A15: 54.20wt%, first monomer A8: 10.84wt%, second monomer B11: 27.10wt%, cross-linking monomer C3: 2.03wt%, cross-linking monomer C2: 1.08wt%, cross-linking monomer C4: 2.71wt%, bis (4-tert-butylcyclohexyl) peroxydicarbonate (initiator): 1.08wt%, 2-acrylic acid 2- (4-benzoyl-3-hydroxyphenoxy) ethyl ester (ultraviolet absorber): 0.95wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0142] Embodiment 36
[0143] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A7: 63.92wt%, first monomer A16: 31.96wt%, crosslinking monomer C1: 2.40wt%, 2,5-dimethyl-2,5-bis(2-ethylhexanoic acid peroxide) hexane (initiator): 0.77wt%, 2-acrylic acid 2-(4-benzoyl-3-hydroxyphenoxy) ethyl ester (ultraviolet absorber): 0.95wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0144] Embodiment 37
[0145] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A7: 63.92wt%, first monomer A9: 31.96wt%, crosslinking monomer C1: 2.40wt%, 2,5-dimethyl-2,5-bis(2-ethylhexanoic acid peroxide) hexane (initiator): 0.77wt%, 2-acrylic acid 2-(4-benzoyl-3-hydroxyphenoxy) ethyl ester (ultraviolet absorber): 0.95wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0146] Embodiment 38
[0147] The present embodiment provides a polymer, based on the total weight of the polymer monomers used to synthesize the polymer, the polymer monomers of the polymer include: first monomer A7: 63.92wt%, first monomer A11: 31.96wt%, crosslinking monomer C1: 2.40wt%, 2,5-dimethyl-2,5-bis(2-ethylhexanoic acid peroxide) hexane (initiator): 0.77wt%, 2-acrylic acid 2-(4-benzoyl-3-hydroxyphenoxy) ethyl ester (ultraviolet absorber): 0.95wt%. The preparation method of the polymer is the same as the preparation method of Example 1.
[0148] Embodiment 39
[0149] Make an artificial lens. Prepare the raw materials according to the polymerization monomer ratio of Example 37, introduce the polymerization monomer stock solution into a special plastic mold. The upper and lower surfaces of the mold have specific optical surfaces, and the designed refractive power is 17D. Then put it into an oven horizontally for curing. The curing temperature is: 50°C for 1 hour, rise to 65°C for 2 hours, and then raise the temperature to 85°C for 16 hours. After the curing is completed, the mold is removed, and the cured sample is adhered to one of the mold surfaces of the two molds. Then the sample with the mold is milled under freezing conditions at a milling speed of 15,000 rpm to obtain the desired haptic structure. The milled sample is removed from the mold to obtain an artificial lens with a smooth and flat cross-section. The actual image is as shown in the figure. Figure 1 shown.
[0150] Performance Testing
[0151] 1. Determination of glass transition temperature: The glass transition temperature of the material was tested using a Shimadzu differential scanning calorimeter, model DSC-60Plus, at a temperature rate of 20°C / min.
[0152] 2. Determination of refractive index and Abbe number: Use ATO Abbe refractometer, model DR-M2, to measure the refractive index and Abbe number of the material. Abbe number Vd = (nD-1) / (nF-nC), where nD, nF, and nC are the refractive indices at 589nm, 486nm, and 656nm respectively. Test conditions: 35℃, measure the refractive index and Abbe number Vd of the material at 546nm.
[0153] 3. Determination of spectral transmittance: The spectral transmittance of the material in the wavelength range of 300 to 1100 nm was measured using a Shimadzu visible-ultraviolet spectrophotometer, model UV-1900i.
[0154] 4. Determination of mechanical parameters: The elastic modulus, tensile strength, elongation at break, etc. were determined by uniform rate stretching at room temperature using a universal material testing machine, model WBE-9010B.
[0155] 5. Evaluation of intraocular lens application
[0156] The artificial lens prepared in Example 39 was evaluated by application simulation. Evaluation of imaging quality: The artificial lens was soaked in physiological saline for one night, and the MTF value at a spatial frequency of 100mm-1 at 3mm aperture was measured using a LAMBDA-X optical analyzer, model NIMOTR0815, in the state of being immersed in physiological saline. Evaluation of folding and injection performance: The artificial lens was folded, and a certain amount of ophthalmic viscoelastic was added for lubrication. The artificial lens implantation push injection system, model Accuject2.0-1P, of Medicel Co., Ltd. was used for push injection evaluation. 35°C physiological saline was injected into it at room temperature, and the time taken for it to unfold to be flat, the stickiness of the loop were observed and recorded, and the damage to its surface and structure were observed under a microscope. Determination of the strength of the loop: A universal material testing machine was used to measure the breaking tensile force of the loop by equal-rate stretching at room temperature.
[0157] The test results are shown in Tables 1 to 8.
[0158] Table 1
[0159] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 First monomer A1 (wt%) 0 93.75 0 26.88 13.89 74.99 First monomer A2 (wt%) 95.88 0 0 0 0 0 First monomer A3 (wt%) 0 0 93.75 0 0 0 First monomer A4 (wt%) 0 0 0 67.20 27.78 0 First monomer A5 (wt%) 0 0 0 0 38.89 15.30 First monomer A6 (wi%) 0 0 0 0 13.89 0 Crosslinking monomer C1 (wt%) 2.40 1.56 1.56 0 1.39 1.07 Crosslinking monomer C2 (wt%) 0 1.25 1.25 0 1.11 0 Crosslinking monomer C3 (wt%) 0 0 0 2.15 0 0 Crosslinking monomer C4 (wt%) 0 0 0 1.34 0 0 Crosslinking monomer C5 (wt%) 0 0 0 0 0 6.12 Initiator D1 (wt%) 0.77 1.88 1.88 0 1.67 0 Initiator D2 (wt%) 0 0 0 1.21 0 1.22 UV absorber E1 (wt%) 0.95 1.56 1.56 0 1.38 1.29 UV absorber E2 (wt%) 0 0 0 1.22 0 0 Glass transition temperature / ℃ 50.21 50.05 15.58 23.64 9.64 6.33 Refractive index at 546nm, 35℃ / 1.5507 1.5354 1.5423 1.5336 1.5283 Abbe number, 35°C / 40.2 38.8 39.9 40.1 43.4 10% spectral transmittance cut-off wavelength 383nm 386nm 388nm 388nm 381nm 383nm Maximum transmittance in the spectral range of 400-780nm 91% 91% 90% 91% 90% 91% Average transmittance in the spectral range of 400-780nm 90% 90% 89% 89% 88% 89% Mechanical state of materials at room temperature Hard, brittle Hard, brittle / / / / Tensile strength / MPa / / 1.362 4.241 0.491 1.305 Elastic modulus / MPa / / 23.818 85.386 4.983 0.753 Elongation at break / % / / 32 25 32 136
[0160] Table 2
[0161] Example 7 Example 8 Example 9 Example 10 Embodiment 11 First monomer A1 (wt%) 55.11 55.11 55.11 47.57 47.57 Second monomer B1 (wt%) 27.56 0 0 0 0 Second monomer B2 (wt%) 0 27.56 0 0 0 Second monomer B3 (wt%) 0 0 27.56 0 0 First monomer B4 (wt%) 0 0 0 35.68 0 First monomer B5 (wt%) 0 0 0 0 35.68 Crosslinking monomer C5 (wt%) 13.78 13.78 13.78 0 0 Crosslinking monomer C6 (wt%) 2.07 2.07 2.07 3.57 3.57 Crosslinking monomer C7 (wt%) 0 0 0 11.89 11.89 Initiator D2 (wt%) 0.66 0.66 0.66 0 0 Initiator D3 (wt%) 0 0 0 0.57 0.57 UV absorber E2 (wt%) 0.82 0.82 0.82 0.72 0.72 Glass transition temperature / ℃ 26.69 28.63 39.38 -9.04 -18.43 Refractive index at 546nm, 35℃ 1.5185 1.5340 1.5180 1.5157 1.5122 Abbe number, 35°C 54.3 41.8 44.0 49.8 49.5 10% spectral transmittance cut-off wavelength 385nm 386nm 387nm 386nm 386nm Maximum transmittance in the spectral range of 400-780nm 91% 90% 90% 90% 90% Average transmittance in the spectral range of 400-780nm 89% 88% 88% 88% 88% Mechanical state of materials at room temperature Hard, brittle Hard, brittle Hard, brittle Soft Soft
[0162] Table 3
[0163] Example 12 Embodiment 13 Embodiment 14 First monomer A2 (wt%) 63.80 55.02 55.02 Second monomer B4 (wt%) 31.90 0 0 Second monomer B6 (wt%) 0 27.51 0 Second monomer B7 (wt%) 0 0 27.51 Second monomer B8 (wt%) 0 13.76 13.76 Crosslinking monomer C3 (wt%) 2.39 2.06 2.06 Initiator D2 (wt%) 0.96 0.83 0.83 UV absorber E2 (wt%) 0.95 0.82 0.82 Glass transition temperature / ℃ -13.55 16.22 16.26 Refractive index at 546nm, 35℃ 1.5113 1.5361 1.5363 Abbe number, 35°C 45.4 41.3 40.4 10% spectral transmittance cut-off wavelength 388nm 388nm 388nm Maximum transmittance in the spectral range of 400-780nm 91% 90% 90% Average transmittance in the spectral range of 400-780nm 89% 88% 88% Tensile strength / MPa 0.635 1.436 1.292 Elastic modulus / MPa 0.440 20.414 21.525 Elongation at break / % 136 87 69
[0164] Table 4
[0165] Embodiment 15 Example 16 Embodiment 17 First monomer A1 (wt%) 0 42.41 53.82 First monomer A4 (wt%) 59.24 0 0 First monomer A6 (wt%) 11.85 0 0 Second monomer B1 (wt%) 0 42.41 0 Second monomer B9 (wt%) 23.70 0 0 Second monomer B4 (wt%) 0 0 26.91 Crosslinking agent C3 (wt%) 1.90 0 0 Crosslinking agent C6 (wt%) 0 3.18 4.04 Crosslinking agent C4 (wt%) 1.18 0 0 Crosslinking agent C7 (wt%) 0 10.60 13.46 Initiator D3 (wt%) 0 0.76 0.97 Initiator D2 (wt%) 1.07 0 0 UV absorber E2 (wt%) 1.06 0.64 0.80 Glass transition temperature / ℃ 22.32 4.50 2.69 Refractive index at 546nm, 35℃ 1.5437 1.5122 1.5195 Abbe number, 35°C 37.5 47.6 47.0 10% spectral transmittance cut-off wavelength 387nm 389nm 389nm Maximum transmittance in the spectral range of 400-780nm 91% 91% 90% Average transmittance in the spectral range of 400-780nm 90% 89% 88% Tensile strength / MPa 2.820 2.47 1.79 Elastic modulus / MPa 39.805 2.29 1.63 Elongation at break / % 39 104 84
[0166] Table 5
[0167] Embodiment 18 Embodiment 19 Embodiment 20 First monomer A1 (wt%) 48.44 0 0 First monomer A4 (wt%) 0 54.05 52.63 First monomer A3 (wt%) 0 13.51 0 First monomer A6 (wt%) 0 0 15.79 Second monomer B1 (wt%) 36.33 0 0 Second monomer B10 (wt%) 0 27.03 0 Second monomer B7 (wt%) 0 0 26.32 Crosslinking agent C1 (wt%) 0 1.35 1.32 Crosslinking agent C6 (wt%) 1.82 0 0 Crosslinking agent C2 (wt%) 0 1.08 1.05 Crosslinking agent C7 (wt%) 12.11 0 0 Initiator D3 (wt%) 0.58 0 0 Initiator D2 (wt%) 0 1.62 1.58 UV absorber E1 (wt%) 0 1.36 1.31 UV absorber E2 (wt%) 0.72 0 0 Glass transition temperature / ℃ 20.60 11.03 11.24 Refractive index at 546nm, 35℃ 1.5184 1.5236 1.5432 Abbe number, 35°C 46.4 42.3 40.0 10% spectral transmittance cut-off wavelength 386nm 384nm 389nm Maximum transmittance in the spectral range of 400-780nm 91% 90% 90% Average transmittance in the spectral range of 400-780nm 89% 88% 88% Tensile strength / MPa 1.82 1.553 1.365 Elastic modulus / MPa 24.60 1.733 1.442 Elongation at break / % 25 74 82
[0168] Table 6
[0169] Embodiment 21 Embodiment 22 Embodiment 23 First monomer A16 (wt%) 95.88 0 0 First monomer A10 (wt%) 0 95.88 0 First monomer A11 (wt%) 0 0 95.88 Homogenizer C1 (wt%) 2.40 2.40 2.40 Initiator D1 (wt%) 0.77 0.77 0.77 UV absorber E1 (wt%) 0.960.95 0.960.95 0.960.95 Glass transition temperature / ℃ -4 -11 -12 Mechanical state of materials at room temperature Soft and weak Soft and weak Soft and weak
[0170] Table 7
[0171] Embodiment 24 Embodiment 25 Embodiment 26 First monomer A13 (wt%) 95.88 0 0 First monomer A12 (wt%) 0 95.88 0 First monomer A15 (wt%) 0 0 95.88 Crosslinking agent C1 (wt%) 2.40 2.40 2.40 Initiator D1 (wt%) 0.77 0.77 0.77 UV absorber E1 (wt%) 0.95 0.95 0.95 Glass transition temperature / ℃ -0.25 -16.81 5.64 Refractive index at 546nm, 35℃ 1.5243 1.5176 1.5268 Abbe number, 35°C 42.1 43.9 45.1 10% spectral transmittance cut-off wavelength / nm 386 387 385 546nm spectral transmittance 91% 90% 91% Average transmittance in the spectral range of 400-780nm 90% 90% 92% Mechanical state of material at room temperature / Soft and weak / Tensile strength / MPa 0.547 / 1.686 Elastic modulus / MPa 0.512 / 9.565 Elongation at break / % 80 / 32
[0172] Table 8
[0173] Embodiment 27 Embodiment 28 Embodiment 29 First monomer A16 (wt.%) 51.60 35.65 0 First monomer A11 (wt.%) 17.20 11.88 0 First monomer A12 (wt.%) 0 0 53.48 Second monomer B11 24.08 0 0 Second monomer B9 0 47.54 0 Second monomer B12 0 0 40.11 Crosslinker C1 2.58 1.78 0 Crosslinker C6 0 0 2.67 Crosslinker C8 1.38 0.95 1.60 Initiator D1 1.72 1.19 1.07 UV absorber E1 1.44 1.01 0 UV absorber E2 0 0 1.07 Glass transition temperature / ℃ 14.17 14.90 9.13 Refractive index at 546nm, 35℃ 1.5196 1.5436 1.5041 Abbe number, 35°C 44.2 41.2 47.8 10% spectral transmittance cut-off wavelength / nm 385 383 386 546nm spectral transmittance 91% 91% 90% Average transmittance in the spectral range of 400-780nm 90% 89% 90% Tensile strength / MPa 5.164 1.403 1.464 Elastic modulus / MPa 49.882 1.984 1.061 Elongation at break / % 66 93 107
[0174] Table 9
[0175] Embodiment 30 Embodiment 31 Embodiment 32 First monomer A15 (wt.%) 73.94 62.40 66.56 First monomer A11 (wt.%) 18.48 0 0 First monomer A13 (wt.%) 0 31.20 0 Second monomer B7 (wt.%) 0 0 26.62 Crosslinking agent C9 (wt.%) 2.77 2.34 2.50 Crosslinking agent C3 (wt.%) 1.85 1.56 1.66 Initiator D2 (wt.%) 1.66 1.40 1.50 UV absorber E2 (wt.%) 1.30 1.10 1.16 Glass transition temperature / ℃ 3.69 5.34 7.23 Refractive index at 546nm, 35℃ 1.5237 1.5257 1.5329 Abbe number, 35°C 42.4 43.2 39.5 10% spectral transmittance cut-off wavelength / nm 387 386 388 546nm spectral transmittance 88% 90% 89% Average transmittance in the spectral range of 400-780nm 88% 90% 88% Tensile strength / MPa 0.718 1.165 0.726 Elastic modulus / MPa 1.150 2.765 0.730 Elongation at break / % 56 65 73
[0176] Table 10
[0177] Embodiment 33 Embodiment 34 Embodiment 35 First monomer A15 (wt.%) 66.89 62.11 54.20 First monomer A12 (wt.%) 6.69 0 0 First monomer A14 (wt.%) 0 18.01 0 First monomer A8 (wt.%) 0 0 10.84 First monomer A13 (wt.%) 16.72 0 0 Second monomer B13 (wt.%) 0 10.87 0 Second monomer B11 (wt.%) 0 0 27.10 Crosslinking agent C3 (wt.%) 2.51 2.33 2.03 Crosslinking agent C2 (wt.%) 1.34 1.24 1.08 Crosslinking agent C4 (wt.%) 3.34 3.11 2.71 Initiator D2 (wt.%) 1.34 1.24 1.08 UV absorber E1 (wt.%) 1.17 1.09 0.95 Glass transition temperature / ℃ 11.64 17.96 41.58 Refractive index at 546nm, 35℃ 1.5248 1.5241 1.5194 Abbe number, 35°C 43.5 45.7 46.1 10% spectral transmittance cut-off wavelength / nm 382nm 382nm 381nm 546nm spectral transmittance 88% 89% 89% Average transmittance in the spectral range of 400-780nm 88% 88% 88% Tensile strength / MPa 1.064 2.203 2.939 Elastic modulus / Pa 4.012 18.320 50.148 Elongation at break / % 35 24 3
[0178] Table 11
[0179] Embodiment 36 Embodiment 37 Embodiment 38 First monomer A7 (wt.%) 63.92 63.92 63.92 First monomer A16 (wt.%) 31.96 0 0 First monomer A9 (wt.%) 0 31.96 0 First monomer A11 (wt.%) 0 0 31.96 Crosslinking agent C1 (wt.%) 2.40 2.40 2.40 Initiator D1 (wt.%) 0.77 0.77 0.77 UV absorber E1 (wt.%) 0.95 0.95 0.95 Glass transition temperature / ℃ 13.92 10.00 9.90 Refractive index at 546nm, 35℃ 1.5306 1.5229 1.5158 Abbe number, 35°C 43.2 40.9 42.7 10% spectral transmittance cut-off wavelength / nm 382nm 382nm 381nm 546nm spectral transmittance 88% 89% 90% Average transmittance in the spectral range of 400-780nm 88% 89% 89% Tensile strength / MPa 1.560 1.112 0.986 Elastic modulus / MPa 4.091 2.981 1.886 Elongation at break / % 91 108 110
[0180] The polymers of Examples 1 to 6 are polymerized using the first monomer of structural formula I, wherein the amount of the first monomer accounts for more than 90wt% of the total mass of the polymerized monomers. The ophthalmic polymer material obtained by homopolymerization or copolymerization of the first monomer of structural formula I has a relatively high refractive index of more than 1.50, an Abbe number greater than 37, and an average transmittance in the visible light band of more than 88%. Among them, the polymer of Example 6 has a refractive index of 1.5283, an Abbe number of 43.4, a glass transition temperature of 6.33°C, a visible light transmittance of more than 89%, an elastic modulus of 0.7535MPa, a tensile strength of 1.305MPa, and an elongation at break of 136%, and is suitable for the preparation of foldable intraocular lenses.
[0181] The polymers of Examples 7 to 20 are polymerized using the first monomer and the second monomer of structural formula I. The amount of the first monomer is 40wt% to 70wt% of the total mass of the polymerized monomers. The polymer obtained by copolymerizing the first monomer and the second monomer of structural formula I has a maximum transmittance of not less than 90% in the wavelength range of 400-780nm, an average transmittance of not less than 88%, a refractive index of 1.51-1.55, an Abbe number of 40-48, and a Tg<15°C, which is suitable for foldable intraocular lens materials. Among them, the polymers of Examples 16, 17, 19, and 20 have a Tg of 2-11°C, a refractive index of 1.51-1.54, and an elongation at break of 70-105%, which are suitable for foldable intraocular lens materials.
[0182] The polymers of Examples 21 to 26 are polymerized using the first monomer of structural formula II, wherein the amount of the first monomer accounts for more than 95wt% of the total mass of the polymerized monomers. The polymer of Example 24 has: a glass transition temperature of -0.25°C, a refractive index of 1.5243 at 546nm at 35°C, an Abbe number of 42.1, a 10% spectral transmittance cutoff wavelength of 386nm, an average transmittance of 90% in the 400-780nm spectral range, a tensile strength of 0.547MPa, an elastic modulus of 0.512MPa, and an elongation at break of 80%, and is suitable for preparing foldable intraocular lens materials.
[0183] The polymers of Examples 27 to 35 are polymerized by using the first monomer and the second monomer of structural formula II. The amount of the first monomer is 50 wt% to 92 wt% of the total weight of the polymerized monomers. The polymer of Example 29 has the following characteristics: glass transition temperature of 9.13°C, refractive index of 1.5041 at 546 nm at 35°C, Abbe number of 47.8, 10% spectral transmittance cutoff wavelength of 386 nm, average transmittance of 90% in the spectral range of 400-780 nm, tensile strength of 1.464 MPa, elastic modulus of 1.061 MPa, elongation at break of 107%, and is suitable for preparing foldable intraocular lens materials.
[0184] The polymers of Examples 36 to 38 are copolymerized using the first monomer of structural formula I and the first monomer of structural formula II. Among them, the polymer of Example 37 has: a glass transition temperature of 10.00°C, a refractive index of 1.5229 at 546nm at 35°C, an Abbe number of 40.9, a 10% spectral transmittance cutoff wavelength of 382nm, a tensile strength of 1.112MPa, an elastic modulus of 2.981MPa, and an elongation at break of 108%, and is suitable for preparing foldable intraocular lens materials.
[0185] The intraocular lens of Example 39 is transparent without glare and has smooth edges. The MTF value under the simulated human eye environment is 0.556, and the imaging quality is excellent. It can be folded and smoothly pushed out through a 2.0mm diameter pusher. No adhesion occurs after being pushed out. The unfolding time is about 1 second. There is no damage to the surface and the body. The breaking tensile force of its loop is 0.33N. The above test performance supports its use in the production of foldable intraocular lenses, and its properties are excellent. Its appearance is shown in the attached picture. Figure 1 shown.
[0186] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A polymer, characterized in that The polymer is obtained by polymerizing at least one polymerizable monomer, wherein the polymerizable monomer includes a first monomer, and the structural formula of the first monomer is shown in the following formula I or formula II: Wherein, A is selected from hydrogen or C1-C6 alkyl; R1 is selected from one of hydrogen, halogen atom, cyano, phenyl, C1-C6 alkyl, C1-C6 alkoxy, C1-C6 alkyl substituted phenyl, and C1-C6 alkoxy substituted phenyl; R2 is selected from one of the alkyl groups; R3 is selected from one of the alkylene groups; n is a positive integer, and m is a positive integer.
2. The polymer according to claim 1, characterized in that A is selected from hydrogen or methyl; R1 is selected from hydrogen, C1-C6 alkyl; R2 is selected from C1-C6 alkyl; R3 is selected from C1-C6 alkylene; n is selected from 1, 2, 3, 4 or 5; m is selected from 1, 2, 3, 4, 5 or 6.
3. The polymer according to claim 1, characterized in that The first monomer includes at least one of the following compounds:
4. The polymer according to claim 1, characterized in that The polymerizable monomer further includes a second monomer, and the second monomer includes at least one of monofunctional acrylic monomers.
5. The polymer according to claim 4, characterized in that The monofunctional acrylic monomer includes at least one of 2-(2-methoxyethoxy)ethyl methacrylate, 2-phenoxyethyl acrylate, butyl methacrylate, ethoxyethoxyethyl acrylate, polyethylene glycol methyl ether methacrylate, ethylene glycol phenyl ether acrylate, 2-phenylethyl acrylate, hydroxyethyl acrylate, phenylethyl methacrylate, 2-ethoxyethyl methacrylate, methyl methacrylate, ethyl methacrylate, and hydroxyethyl methacrylate.
6. The polymer according to claim 4, characterized in that Based on the total weight of the polymerized monomers used to synthesize the polymer, the amount of the second monomer used is 20 wt % to 40 wt %.
7. The polymer according to claim 1, characterized in that The polymerizable monomer further includes a cross-linking monomer, and the cross-linking monomer includes at least one of a difunctional acrylic monomer and a trifunctional acrylic monomer.
8. The polymer according to claim 7, characterized in that The difunctional acrylic monomer includes at least one of ethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, butanediol dimethacrylate, polyethylene glycol dimethacrylate, neopentyl glycol dimethacrylate, dipropylene glycol diacrylate and butanediol diacrylate; and / or, The trifunctional acrylic monomer includes trimethylolpropane trimethacrylate.
9. The polymer according to claim 7, characterized in that Based on the total weight of the polymerized monomers used to synthesize the polymer, the amount of the cross-linking monomer is 0.25 wt % to 30 wt %.
10. The polymer according to claim 1, characterized in that The polymerizable monomers also include an ultraviolet absorber and an initiator.
11. The polymer according to claim 10, characterized in that Based on the total weight of the polymerized monomers used to synthesize the polymer, the amount of the ultraviolet absorber is 0.2 wt% to 2 wt%; and / or, Based on the total weight of the polymerization monomers used to synthesize the polymer, the amount of the initiator used is 0.1 wt% to 5 wt%.
12. The polymer according to any one of claims 1 to 11, characterized in that The polymer has a refractive index of 1.50-1.55, an Abbe number of 37-54, and an average light transmittance in the visible light band greater than 88%.
13. A method for preparing a polymer, characterized in that: The following steps are involved: Providing a polymerizable monomer as claimed in any one of claims 1 to 11; After the polymerization monomers are mixed, they are subjected to stage-by-stage heating treatment to obtain the polymer.
14. The method for preparing a polymer according to claim 13, characterized in that: The segmented heating process includes the following three stages of heating: The first stage heating condition is heating at 45-55°C for 1h-3h; The second stage heating condition is heating at 65-75°C for 2h-4h; The third stage heating condition is heating at 80-120°C for 12h-20h.