Concrete rheology modifier as well as preparation method and application thereof

The concrete rheology modifier prepared by using polycondensation reaction of polyether large monomers and other components in high-salt and high-alkali environments has solved the problem of sensitivity of dosage and poor salt and alkali resistance, and achieved the stability and ease of concrete Improved, significantly improving the resistance to segregation and liquidity.

CN119019629APending Publication Date: 2024-11-26JIANGSU BOXIRI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411129070.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing concrete rheology modifiers have problems such as sensitivity in dosage and poor salt and alkali resistance, and it is difficult to maintain the flowability and segregation resistance of concrete in a high-salt and high-alkali environment.

Method used

High molecular weight concrete rheology modifiers prepared by polycondensation reaction of polyether large monomers, polyether phosphate monomers, alkylbenzene monomers and phenylamide monomers are used to combine aldehyde monomers under inert gas conditions The reaction was carried out to form a phenolic polycondensation main chain with high stability, enhancing the dispersion and adsorption ability of cement particles.

Benefits of technology

It significantly improves the ease of concrete, segregation resistance and temperature resistance, reduces the sensitivity to inorganic salts, and is insensitive to the amount of dosage, and can maintain good thickening and water retention and construction performance in high-temperature and high-salt environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004997306980000021
    Figure BDA0004997306980000021
  • Figure BDA0004997306980000031
    Figure BDA0004997306980000031
  • Figure BDA0004997306980000032
    Figure BDA0004997306980000032
Patent Text Reader

Abstract

The invention discloses a concrete rheology modifier, a preparation method thereof and application of the concrete rheology modifier as a concrete additive, and the concrete rheology modifier is mainly prepared by polycondensation of a polyether macromonomer A, a polyether phosphate monomer B, an alkylbenzene monomer C and a phenylamide monomer D in the presence of an aldehyde monomer E. Compared with the current common rheology modifier in the field of concrete, the rheology modifier disclosed by the invention is simple and convenient in synthesis method, has good compatibility with a polycarboxylate superplasticizer, and has excellent salt and alkali resistance; the peaceability of fresh concrete can be effectively improved, separation, bleeding and sedimentation are avoided, and the slurry wrapping effect is good; the influence on the fluidity retention value of the concrete is small, the contradiction between the fluidity and segregation resistance of the fresh concrete can be effectively solved, and the additive is not sensitive to the mixing amount.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and particularly relates to a concrete rheology modifier and a preparation method and application thereof. Background Art

[0002] With the continuous development of concrete technology, high-performance concrete has been widely used in engineering. The fluidity of concrete has developed from the previous 80-100mm to the current slump of 180-240mm, while the fluidity and cohesion of concrete are often a pair of contradictions that cannot be unified, that is, it is difficult for concrete to maintain high cohesion performance under large flow state. While pursuing high-fluidity concrete, water segregation is prone to occur. In addition, with the gradual depletion of river sand resources and mineral resources in my country, the gradation and fineness of river sand have fluctuated greatly. As a commercial concrete production enterprise, in order to reduce costs, reduce resource damage and achieve green production, the use of artificial fine aggregates such as machine-made sand has also become a general trend. Artificial machine-made sand generally has unreasonable particle gradation due to resource and process limitations. In addition, all commercial concrete companies currently generally use high-water-reducing but sensitive polycarboxylic acid-type water-reducing agents, and the quality control of ready-mixed concrete faces increasingly severe challenges. To this end, various admixtures such as rheology modifiers that improve and adjust the workability of concrete have emerged and are widely used.

[0003] Concrete rheology modifiers can increase the viscosity of concrete mixtures, reduce the tendency of separation between components, improve homogeneity, and alleviate segregation and bleeding. Common concrete rheology modifiers on the market include cellulose, xanthan gum, vinblastine gum, dimethoate gum, polyacrylamide, etc., but due to their large molecular weight, slow dissolution, and low solubility, these products are prone to agglomeration and stratification during the compounding of water reducers, which limits their scope of application. In addition, flocculation and poor salt and alkali resistance are prone to occur in cement paste, which can easily have a negative impact on the initial and time-dependent fluidity, setting time and strength of concrete.

[0004] In order to improve these deficiencies, there are currently some concrete rheology modifiers with good compatibility with water reducers. Patent CN114014995A uses allyl polyoxyethylene ether, polyvinyl alcohol, unsaturated amide monomer, unsaturated carboxylic acid monomer, unsaturated cationic monomer and crosslinking agent to prepare a cross-linked polyether concrete water retaining agent. CN105585673A discloses a concrete viscosity increasing water retaining agent, which is prepared by polymerization of methyl butyl polyoxypropylene, unsaturated monobasic acid or / and its derivatives, unsaturated olefin sulfonic acid or / and its sodium salt and unsaturated olefin organosilicon crosslinking agent as raw materials. The concrete rheology modifiers prepared by the above patents are all designed based on the structure of polycarboxylic acid water reducer. Although they have good compatibility with polycarboxylic acid water reducer, there is a problem of dosage sensitivity. When the dosage is low, the improvement of concrete water seepage segregation is insufficient. When the dosage is high, it has a significant effect on the fluidity over time. In addition, this type of concrete rheology modifier has poor salt and alkali resistance and is insufficient to continuously play a thickening and water retention role.

[0005] Therefore, developing a concrete stabilizer with good stability, good water retention, low dosage, good concrete workability, and no effect on the later performance of concrete has become a major technical difficulty. Summary of the invention

[0006] Purpose of the invention: In view of the problems of existing rheology modifiers such as poor dosage and salt-alkali resistance, based on the special environment of high salt, high alkali and strong shearing of concrete slurry, the present invention provides a polymer rheology modifier with good compatibility with high-efficiency water reducer, insensitive to dosage, and able to effectively solve the contradiction between fluidity and anti-segregation of fresh concrete, thereby improving the workability of fresh concrete. A preparation method of the rheology modifier and its application as a concrete additive are also provided.

[0007] Technical solution: In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:

[0008] A concrete rheology modifier, wherein the concrete rheology modifier is mainly formed by connecting the following structural units A1, B1, C1, and D1 through a structural unit E1:

[0009]

[0010] Among them, r is an integer of 10 to 25, s is an integer of 4 to 8; R1 is -CH2- or -COO-; R2 is a straight-chain alkyl group of C8 to C18; R3 is -CH2- or -CH2CH2-; R4 is H or a C1-C3 alkyl group.

[0011] As a specific implementation scheme, the molecular weight of the concrete rheology modifier is 300,000 to 1,200,000.

[0012] As a specific implementation, the concrete rheology modifier is mainly obtained by polycondensing polyether macromonomer A, polyether phosphate monomer B, alkylbenzene monomer C and phenylamide monomer D in the presence of aldehyde monomer E.

[0013] The polyether macromonomer A is a phenol polyether monomer, which is obtained by the addition of phenol or phenoxyethanol and ethylene oxide, and can be prepared according to the method described in the public literature or patents; its structural formula is shown in (II):

[0014]

[0015] Wherein, the definition of r is the same as above.

[0016] The polyether phosphate monomer B is prepared by modifying phenol polyether through phosphorylation reaction, and can be prepared according to the method described in the public literature or patents; its structural formula is shown in (III):

[0017]

[0018] Wherein, the definition of s is the same as above.

[0019] The alkylbenzene monomer C is a commercially available alkylbenzene or is obtained by esterification of benzoic acid and alkyl alcohol, and can be prepared according to the method described in the public literature or patents; its structural formula is shown in (IV):

[0020]

[0021] Wherein, R1 and R2 have the same meanings as above.

[0022] The phenylamide monomer D is a commercially available phenylamide, for example, any one of phenylacetamide and 3-phenylpropionamide; its structural formula is shown in (V):

[0023]

[0024] In the formula, R3 has the same definition as above.

[0025] The aldehyde monomer E has a structural formula as shown in (VI), and can be selected from any one of formaldehyde, paraformaldehyde and acetaldehyde:

[0026]

[0027] In the formula, R4 is defined as above, and n=8-15.

[0028] The present invention also provides a method for preparing the concrete rheology modifier, comprising the following steps:

[0029] The polyether macromonomer A, polyether phosphate monomer B, alkylbenzene monomer C, and phenylamide monomer D are melted under inert gas conditions, then heated to the reaction temperature, an acid catalyst and an aldehyde monomer E are added, and refluxed under normal pressure to react. After the reaction is completed, the temperature is lowered, and water is added for dilution to obtain a concrete rheology modifier.

[0030] As a specific implementation, the selection of the polyether macromonomer A, polyether phosphate monomer B, alkylbenzene monomer C, phenylamide monomer D and aldehyde monomer E is the same as described above.

[0031] As a specific implementation scheme, the melting is carried out at 90-100°C, the reaction temperature is 120-140°C, and the reaction is carried out under reflux at normal pressure for 4-8 hours.

[0032] As a specific embodiment, the molar ratio of the polyether macromonomer A, polyether phosphate monomer B, alkylbenzene monomer C, phenylamide monomer D and aldehyde monomer E is a:b:c:d:e, wherein a:b:c:d=1:10-15:1-3:10-20, (a+b+c+d):e=1.05-1.5:1;

[0033] The acid catalyst is selected from any one of concentrated sulfuric acid, benzenesulfonic acid, methanesulfonic acid, p-toluenesulfonic acid, and ethylsulfonic acid, or any combination of two of them in any proportion, and its usage is 0.5-2% of the total mass of monomer A, monomer B, monomer C, monomer D, and monomer E.

[0034] Finally, the invention provides application of the concrete rheology modifier as a concrete additive.

[0035] As a specific implementation scheme, when preparing concrete, the concrete rheology modifier can be added alone, or can also be compounded with aminosulfonic acid-based water reducer and polycarboxylic acid water reducer; preferably, air entraining agent, retarder and defoamer can also be added for compounding.

[0036] The concrete rheology modifier of the present invention is obtained by polycondensation reaction to obtain a phenolic polycondensation main chain, and the rupture of the phenolic polycondensation main chain requires very high energy, and it is not easy to break even if the ambient temperature is very high. Therefore, the concrete rheology modifier of the present invention is more stable than other types of rheology modifiers and has stronger temperature resistance. The long polyoxyethylene ether side chain of the polyether macromonomer A can extend into the cement paste solution, and like the long polyether side chain of the polycarboxylic acid water reducer, it produces a steric hindrance effect to achieve the dispersion of cement particles, and at the same time, it can effectively improve the workability of concrete. The polyether phosphate monomer B is a monomer containing a phosphate group, which can be effectively adsorbed on the surface of cement particles, has a stronger adsorption capacity than the carboxylic acid group, and can play a role in long-term stability; in addition, in a high temperature and high salt environment, it shows good concrete retention performance, and at the same time plays a certain retarding effect, which can make the concrete have a more durable construction performance. The polyether phosphate monomer B and the phenylamide monomer D provide a phosphate group and an amide group, respectively, and both have good water solubility. Alkylbenzene monomer C contains C8~C18 alkyl groups, which are introduced into the concrete rheology modifier as an air-entraining component, so that the concrete rheology modifier has mild air-entraining properties, which can introduce stable, tiny and uniform bubbles into the fresh concrete, and effectively improve its fluidity while improving the concrete's resistance to segregation and water bleeding, making the concrete have higher workability.

[0037] In general, the concrete rheology modifier described in the present invention is a condensation-polymerized high molecular weight polymer, which can greatly reduce the sensitivity to inorganic salts and show a higher saturation dosage and more excellent thickening, water retention and temperature and salt resistance in the cement / concrete system.

[0038] Beneficial effects: Compared with the commonly used rheology modifiers in the concrete field, the present invention has the following characteristics: (1) The rheology modifier of the present invention has a simple synthesis method, has good compatibility with polycarboxylic acid water-reducing agent, and has excellent salt and alkali resistance; (2) The rheology modifier of the present invention can effectively improve the workability of fresh concrete, without segregation, water seepage, sedimentation, and good slurry coating effect; (3) The rheology modifier of the present invention has a small effect on the retention value of concrete fluidity, that is, it can effectively solve the contradiction between the fluidity and anti-segregation of fresh concrete; (4) The rheology modifier of the present invention is not sensitive to the dosage, and the optimal dosage is 0.005% to 0.02% of the amount of concrete adhesive. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] The present invention provides a method for preparing the concrete rheology modifier, comprising the following steps:

[0041] Place polyether macromonomer A, polyether phosphate monomer B, alkylbenzene monomer C and phenylamide monomer D in a reaction vessel under nitrogen protection, heat to 90-100°C, stir evenly after melting, then heat to 120-140°C, add acid catalyst F and aldehyde monomer E, reflux at normal pressure for 4-8h, and after the reaction is completed, slowly cool to 55°C, then dilute with water to obtain a concrete rheology modifier.

[0042] The raw materials used in the examples are listed in Table 1, as follows:

[0043] Table 1 Compound codes in the synthetic examples

[0044]

[0045]

[0046] The rheology modifier information in the examples is listed in Table 2, as follows:

[0047] Table 2 Synthesis information of concrete rheology modifier

[0048]

[0049]

[0050] Example 1

[0051] 1 mol of polyether macromonomer A-1, 10 mol of polyether phosphate monomer B-2, 1 mol of alkylbenzene monomer C-1, and 10 mol of phenylamide monomer D-1 are placed in a reaction container under nitrogen protection, heated to 90°C, stirred evenly after melting, then heated to 120°C, acid catalyst F-1 (0.5% of the total mass of monomers A, B, C, D, and E) and 20.95 mol of aldehyde monomer E-2 are added, and refluxed at normal pressure for 8 hours. After the reaction is completed, the temperature is slowly lowered to 55°C, and then diluted with water to obtain concrete rheology modifier P-1 (the molecular weight of P-1 is 830000).

[0052] Example 2

[0053] 1 mol of polyether macromonomer A-2, 15 mol of polyether phosphate monomer B-3, 3 mol of alkylbenzene monomer C-2 and 20 mol of phenylamide monomer D-1 are placed in a reaction vessel under nitrogen protection, heated to 95°C, stirred evenly after melting, then heated to 130°C, acid catalyst F-2 (1% of the total mass of monomers A, B, C, D and E) and 26 mol of aldehyde monomer E-1 are added, and refluxed at normal pressure for 6 hours. After the reaction is completed, the temperature is slowly lowered to 55°C, and then diluted with water to obtain concrete rheology modifier P-2 (the molecular weight of P-2 is 1150000).

[0054] Example 3

[0055] 1 mol of polyether macromonomer A-3, 10 mol of polyether phosphate monomer B-1, 3 mol of alkylbenzene monomer C-3, and 20 mol of phenylamide monomer D-1 are placed in a reaction vessel under nitrogen protection, heated to 100°C, stirred evenly after melting, then heated to 140°C, and acid catalyst F-3 (2% of the total mass of monomers A, B, C, D, and E) and 30.91 mol of aldehyde monomer E-3 are added. The reaction is refluxed at normal pressure for 4 hours. After the reaction is completed, the temperature is slowly lowered to 55°C, and then diluted with water to obtain concrete rheology modifier P-3 (the molecular weight of P-3 is 350,000).

[0056] Example 4

[0057] 1 mol of polyether macromonomer A-1, 15 mol of polyether phosphate monomer B-3, 1 mol of alkylbenzene monomer C-4, and 10 mol of phenylamide monomer D-2 are placed in a reaction container under nitrogen protection, heated to 90°C, stirred evenly after melting, then heated to 125°C, acid catalyst F-4 (2% of the total mass of monomers A, B, C, D, and E) and 22.5 mol of aldehyde monomer E are added, and refluxed at normal pressure for 8 hours. After the reaction is completed, the temperature is slowly lowered to 55°C, and then diluted with water to obtain concrete rheology modifier P-4 (P-4 molecular weight is 670000).

[0058] Example 5

[0059] 1 mol of polyether macromonomer A-2, 12 mol of polyether phosphate monomer B-2, 2 mol of alkylbenzene monomer C-1, and 15 mol of phenylamide monomer D-2 are placed in a reaction container under nitrogen protection, heated to 100°C, stirred evenly after melting, then heated to 135°C, acid catalyst F-5 (1.5% of the total mass of monomers A, B, C, D, and E) and 23.08 mol of aldehyde monomer E-1 are added, and refluxed at normal pressure for 8 hours. After the reaction is completed, the temperature is slowly lowered to 55°C, and then diluted with water to obtain concrete rheology modifier P-5 (P-5 molecular weight is 780000).

[0060] Example 6

[0061] 1 mol of polyether macromonomer A-3, 13 mol of polyether phosphate monomer B-2, 3 mol of alkylbenzene monomer C-2 and 18 mol of phenylamide monomer D-2 are placed in a reaction vessel under nitrogen protection, heated to 95°C, stirred evenly after melting, then heated to 140°C, acid catalyst F-1 (1% of the total mass of monomers A, B, C, D and E) and 25 mol of aldehyde monomer E-2 are added, and refluxed at normal pressure for 6 hours. After the reaction is completed, the temperature is slowly lowered to 55°C, and then diluted with water to obtain concrete rheology modifier P-6 (the molecular weight of P-6 is 420,000).

[0062] Example 7

[0063] 1 mol of polyether macromonomer A-1, 11 mol of polyether phosphate monomer B-1, 1 mol of alkylbenzene monomer C-3, and 12 mol of phenylamide monomer D-2 are placed in a reaction container under nitrogen protection, heated to 90°C, stirred evenly after melting, then heated to 125°C, acid catalyst F-2 (2% of the total mass of monomers A, B, C, D, and E) and 21.74 mol of aldehyde monomer E-2 are added, and refluxed at normal pressure for 8 hours. After the reaction is completed, the temperature is slowly lowered to 55°C, and then diluted with water to obtain concrete rheology modifier P-7 (the molecular weight of P-7 is 1,170,000).

[0064] Example 8

[0065] 1 mol of polyether macromonomer A-2, 14 mol of polyether phosphate monomer B-2, 2.5 mol of alkylbenzene monomer C-4, and 20 mol of phenylamide monomer D-2 are placed in a reaction container under nitrogen protection, heated to 100°C, stirred evenly after melting, then heated to 140°C, acid catalyst F-3 (2% of the total mass of monomers A, B, C, D, and E) and 35.71 mol of aldehyde monomer E-3 are added, and refluxed at normal pressure for 4 to 8 hours. After the reaction is completed, the temperature is slowly lowered to 55°C, and then diluted with water to obtain concrete rheology modifier P-8 (P-8 molecular weight is 980000).

[0066] Example 9

[0067] 1 mol of polyether macromonomer A-3, 10 mol of polyether phosphate monomer B-3, 2 mol of alkylbenzene monomer C-1, and 15 mol of phenylamide monomer D-1 are placed in a reaction container under nitrogen protection, heated to 100°C, stirred evenly after melting, then heated to 120°C, acid catalyst F-4 (2% of the total mass of monomers A, B, C, D, and E) and 20.74 mol of aldehyde monomer E-3 are added, and refluxed at normal pressure for 8 hours. After the reaction is completed, the temperature is slowly lowered to 55°C, and then diluted with water to obtain concrete rheology modifier P-9 (P-9 molecular weight is 510000).

[0068] Example 10

[0069] 1 mol of polyether macromonomer A-1, 15 mol of polyether phosphate monomer B-2, 3 mol of alkylbenzene monomer C-2, and 15 mol of phenylamide monomer D-1 are placed in a reaction container under nitrogen protection, heated to 95°C, stirred evenly after melting, then heated to 125°C, acid catalyst F-5 (1% of the total mass of monomers A, B, C, D, and E) and 23.45 mol of aldehyde monomer E-2 are added, and refluxed at normal pressure for 8 hours. After the reaction is completed, the temperature is slowly lowered to 55°C, and then diluted with water to obtain concrete rheology modifier P-10 (P-10 molecular weight is 380000).

[0070] Comparative Example 1

[0071] During the synthesis of the concrete rheology modifier P-1 in Example 1, the alkylbenzene monomer C-1 was removed and the other reaction conditions remained unchanged to obtain a concrete rheology modifier, which was recorded as K-1 (the molecular weight of K-1 was 730,000).

[0072] Comparative Example 2

[0073] Commercially available hydroxypropyl methylcellulose (HPMC) is referred to as K-2.

[0074] Comparative Example 3

[0075] The concrete rheology modifier prepared according to Example 1 in patent CN105542090B is denoted as K-3.

[0076] Application Example 1

[0077] The rheology modifiers of Examples 1 to 10 and Comparative Examples 1 to 3 were tested for cement paste bleeding. The test method is: 1500g of cement, 900g of water, and 5g of a rheology modifier with a solid content of 2% were fully stirred and mixed, 100mL of the mixed cement paste was placed in a measuring cylinder, and the bleeding height was tested for 20, 40, and 60 minutes respectively. The test results are shown in Table 3.

[0078] Table 3 Test on water seepage performance of cement paste with different concrete rheology modifiers

[0079]

[0080]

[0081] From the test results of water seepage performance in Table 3, after adding the concrete rheology modifier prepared by the present invention to the cement paste, the water seepage at 20min, 40minn and 60min was greatly improved, and was better than the comparative samples K-2 and K-3 as a whole, indicating that the concrete rheology modifier prepared by the present invention has good anti-segregation and anti-water seepage performance. Compared with samples P-1 and K-1, the water seepage performance of the two samples is not much different, indicating that the difference in the air entraining components between the two samples has little effect on the water seepage performance.

[0082] Application Example 2

[0083] The rheology modifiers of Examples 1 to 10 and Comparative Examples 1 to 3 were subjected to concrete performance tests. According to the relevant provisions of the national standard GB / T14902-2018, the slump / expansion, air content and outflow time of the concrete were determined. The water reducer used in the present invention is the high-performance water reducer BST-900 (polycarboxylic acid water reducer, weight-average molecular weight of 36800) produced by Boshitong, with a solid content of 0.25%; the cement is Onoda 52.5RP.II cement; the sand is medium sand with a fineness modulus of Mx=2.6; the gravel is a crushed stone with a particle size of 5-25mm and continuous grading. The concrete mix ratio used is: 5.4kg cement, 1.8kg fly ash, 1.8kg mineral powder, 16.0kg sand, 13.0kg large stone, 5.6kg small stone, and 3.3kg water. All rheology modifiers were added in the same dosage, which was 0.25 per ten thousand of the mass of the cementitious material. The test results are shown in Table 4.

[0084] Table 4 Concrete performance test of different concrete rheology modifiers

[0085]

[0086]

[0087] Note: “+” indicates the degree of segregation and water seepage. The more “+” there are, the more serious the segregation and water seepage is.

[0088] It can be seen from Table 4 that the concrete rheology modifier prepared by the present invention can make the fresh concrete have better anti-segregation and water bleeding performance. At the same time, compared with K-1 (without air entraining component), K-2 (commercially available HPMC) and K-3, the concrete rheology modifier prepared by the present invention has obvious air entraining performance, greater slump and expansion, and shorter outflow time, which shows that they have better fluidity.

[0089] The implementation modes of the present invention have been described in detail above in conjunction with specific embodiments, but the present invention is not limited to the above-mentioned implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A concrete rheology modifier, characterized in that: The concrete rheology modifier is mainly formed by connecting the following structural units A1, B1, C1, and D1 through a structural unit E1: Among them, r is an integer of 10 to 25, s is an integer of 4 to 8; R1 is -CH2- or -COO-; R2 is a straight-chain alkyl group of C8 to C18; R3 is -CH2- or -CH2CH2-; R4 is H or a C1-C3 alkyl group.

2. The concrete rheology modifier according to claim 1, characterized in that: The molecular weight of the concrete rheology modifier is 300,000-1,200,000.

3. The concrete rheology modifier according to claim 1, characterized in that: It is mainly obtained by polycondensing polyether macromonomer A, polyether phosphate monomer B, alkylbenzene monomer C and phenylamide monomer D in the presence of aldehyde monomer E.

4. The concrete rheology modifier according to claim 3, characterized in that: The structural formula of the polyether macromonomer A is shown in (II): Wherein, the definition of r is the same as that in claim 1; The structural formula of the polyether phosphate monomer B is shown in (III): Wherein, the definition of s is the same as that in claim 1; The structural formula of the alkylbenzene monomer C is shown in (IV): Wherein, R1 and R2 are defined as in claim 1; The structural formula of the phenylamide monomer D is shown in (V): Wherein, the definition of R3 is the same as that in claim 1; The structural formula of the aldehyde monomer E is shown in (VI): In the formula, R4 has the same definition as in claim 1, and n=8-15.

5. The method for preparing a concrete rheology modifier according to claim 3, characterized in that: The polyether macromonomer A is a phenol polyether monomer, which is mainly obtained by the addition of phenol or phenoxyethanol and ethylene oxide; the polyether phosphate monomer B is mainly obtained by modifying phenol polyether through a phosphorylation reaction; the alkylbenzene monomer C is selected from commercially available alkylbenzenes, or is mainly obtained by esterification of benzoic acid and alkyl alcohol; the phenylamide monomer D is selected from any one of phenylacetamide and 3-phenylpropionamide; the aldehyde monomer E is selected from any one of formaldehyde, paraformaldehyde and acetaldehyde.

6. The method for preparing the concrete rheology modifier according to any one of claims 1 to 5, characterized in that: The following steps are involved: The polyether macromonomer A, polyether phosphate monomer B, alkylbenzene monomer C, and phenylamide monomer D are melted under inert gas conditions, then heated to the reaction temperature, an acid catalyst and an aldehyde monomer E are added, and refluxed under normal pressure to react. After the reaction is completed, the temperature is lowered, and water is added for dilution to obtain a concrete rheology modifier.

7. The method for preparing a concrete rheology modifier according to claim 6, characterized in that: The melting is carried out at 90-100°C, the reaction temperature is 120-140°C, and the reaction is carried out under reflux at normal pressure for 4-8 hours.

8. The method for preparing a concrete rheology modifier according to claim 6, characterized in that: The molar ratio of the polyether macromonomer A, polyether phosphate monomer B, alkylbenzene monomer C, phenylamide monomer D and aldehyde monomer E is a:b:c:d:e, wherein a:b:c:d=1:10-15:1-3:10-20, (a+b+c+d):e=1.05-1.5:1; The acid catalyst is selected from any one of concentrated sulfuric acid, benzenesulfonic acid, methanesulfonic acid, p-toluenesulfonic acid, and ethylsulfonic acid, or any combination of two of them in any proportion, and its usage is 0.5-2% of the total mass of monomer A, monomer B, monomer C, monomer D, and monomer E.

9. Use of the concrete rheology modifier according to any one of claims 1 to 5 as a concrete additive.

10. The use according to claim 9, characterized in that: When preparing concrete, the concrete rheology modifier can be added alone, or mixed with aminosulfonic acid water reducer and polycarboxylic acid water reducer; preferably, air entraining agent, retarder and defoamer are also added for use.