Glycidyl azide polymer and preparation method thereof
Through the azide process of cationic ring-opening polymerization method and phosphine ionic liquid media, the problems of high GAP reaction temperature and long time in the indirect method are solved, and the molecular weight and functionality of efficient synthesis of GAP are maintained, and the process flow is simplified .
Patent Information
- Application Number
- CN202411431657.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When polyazide glycidyl ether (GAP) is prepared by indirect method, the reaction temperature is high and the time is long, resulting in a decrease in molecular weight and functionality.
The cationic ring-opening polymerization method is used, and the epoxychlorohydrin monomer is ring-opening polymerized with diol as the initiator and Lewis acid as the catalyst to obtain polyepoxychlorohydrin (PECH) with clear end groups, and then phosphine salt ionic liquid react with sodium azide under the medium to avoid the high temperature and long-term azide process.
It realizes efficient synthesis of GAP under mild conditions, maintains a high level of molecular weight and functionality, avoids the occurrence of side reactions, and simplifies the process flow.
Smart Images

Figure CN119039580A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a polyazide glycidyl ether-based adhesive, and in particular to a polyazide glycidyl ether and a preparation method thereof. Background Art
[0002] Glycidyl azide poly (GAP) is an important energetic polymer. It is considered to be one of the most promising binders in the next generation of solid propellants due to its excellent properties such as high energy, high density, high burning rate, low smoke and low sensitivity.
[0003] The synthesis methods of GAP reported so far mainly include direct method and indirect method. The direct method is to directly form GAP by one-step ring-opening polymerization of azidomethyl propylene oxide (GA) under the action of a catalyst. However, this route involves small molecule organic azide monomers, which are generally sensitive high-energy explosives, so this route is more dangerous in operation. The indirect method, also known as the macromolecular group substitution method, requires the synthesis of polyepichlorohydrin or its derivatives first, and then reacts with sodium azide (NaN3) in an organic solvent such as N, N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), polyethylene glycol or ionic liquid / water mixed solvent to prepare GAP. This can avoid the operational hazards caused by the presence of GA, and the synthesis process of the intermediate PECH is mature, and the molecular weight is easy to control. Therefore, the indirect method has become the key route for GAP synthesis research.
[0004] When GAP is prepared by the indirect method, the azidation process usually requires high temperature (~100°C) and long time (>24 h) reaction, which can easily cause GAP chain breakage and side reactions such as cyclization, thereby reducing its molecular weight and functionality. Summary of the invention
[0005] In view of the problem that the indirect method for preparing GAP currently has high reaction temperature and long time, resulting in reduced molecular weight and functionality, the present invention provides a polyazide glycidyl ether and a preparation method thereof, which has mild preparation conditions, simple operation and efficient reaction.
[0006] In order to achieve the above object, the present invention provides a method for preparing polyazide glycidyl ether, which comprises the following steps: S1. After the diol initiator and the Lewis acid catalyst are uniformly mixed, epichlorohydrin monomer is added dropwise at 1-2.6 mL / h. After the addition is completed, the reaction is carried out for 1-3 hours to obtain polyepichlorohydrin. The molar ratio of the diol initiator, the Lewis acid catalyst and the epichlorohydrin monomer is (2-15):1:(50-100); S2, polyepichlorohydrin and phosphonium salt ionic liquid [P 444E3 + ][Cl- ] and the azide reagent NaN3 are mixed evenly, and reacted at 70~90℃ for 5~12 h to obtain polyazido glycidyl ether.
[0007] In the above technical scheme of the present invention, cationic ring-opening polymerization is firstly adopted, with diol as initiator and Lewis acid as catalyst, to carry out ring-opening polymerization on epichlorohydrin monomer, so as to obtain polyepichlorohydrin (PECH) with a clear terminal group of hydroxyl group and a functionality close to 2.00; the synthesis method is simple and fast, the synthesis process is insensitive to water and oxygen, the reaction can be carried out at room temperature in an open system, the monomer can be added dropwise quickly, the reaction time is short, and the synthesized PECH has a narrow distribution, a clear terminal group and a functionality close to 2.00.
[0008] Secondly, in the azidation process, the phosphine ionic liquid [P 444E3 + ][Cl - ] as the reaction medium, which can dissolve PECH and sodium azide well, making the reaction conditions of the azidation process mild and efficient. 444E3 + ][Cl - ] as the reaction medium, sodium azide is used as the azide reagent, and PECH is subjected to nucleophilic substitution. The azidation process can be efficiently completed under relatively mild reaction conditions, avoiding high temperature and long-term reaction. The molecular weight and functionality of GAP obtained by this method will not be reduced compared with its raw material PECH.
[0009] Preferably, in step S1, the diol initiator is one or more of 3-chloro-1,2-propylene glycol, 1,4-butanediol, and 3-chloro-1,2-propylene glycol.
[0010] After the initiator such as 3-chloro-1,2-propylene glycol is activated by the catalyst, the active substance formed has good solubility in the reaction system. The monomer can be quickly reacted after being added. The instantaneous monomer concentration in the system is relatively low, avoiding the occurrence of side reactions. Compared with other initiators, at the same dosage, the GAP prepared by using the above initiators has a higher molecular weight, a narrower distribution, and a functionality closer to 2.00.
[0011] Preferably, in step S1, the Lewis acid catalyst is one or more of boron trifluoride ether complex, boron trifluoride tetrahydrofuran complex, and tin tetrachloride.
[0012] In the CROP of ECH, BF3•Et2O can make ECH have higher functionality and lower dispersity on the chain end hydroxyl groups compared with SnCl4, even at slightly different ECH / initiator ratios.
[0013] Preferably, in step S1, after the reaction is terminated, the polyepichlorohydrin is obtained by washing, purification and drying.
[0014] Preferably, in step S2, after the reaction is completed, the polyazide glycidyl ether is obtained by filtering, extracting, separating and drying.
[0015] The second aspect of the present invention provides a polyazide glycidyl ether prepared by the above preparation method, which has the following structure: , Wherein, n is an integer between 20 and 49.
[0016] Through the above technical solution, the present invention achieves the following beneficial effects: The present invention firstly adopts cationic ring-opening polymerization, uses diol as initiator and Lewis acid as catalyst, and performs ring-opening polymerization on epichlorohydrin monomer to obtain polyepichlorohydrin (PECH) with a clear terminal group of hydroxyl and a functionality of 2; the synthesis method is simple and fast, the synthesis process is insensitive to water and oxygen, can react at room temperature and in an open system, can quickly add monomers, and has a short reaction time. The synthesized PECH has a narrow distribution, a clear terminal group, and a functionality close to 2.00. Secondly, in the azidation process, a phosphonium salt ionic liquid [P 444E3 + ][Cl - ] as the reaction medium, which can dissolve PECH and sodium azide well, making the reaction conditions of the azidation process mild and efficient. 444E3 + ][Cl - ] as the reaction medium, sodium azide is used as the azide reagent, and PECH is subjected to nucleophilic substitution. The azidation process can be efficiently completed under relatively mild reaction conditions, avoiding high temperature and long-term reaction. The molecular weight and functionality of GAP obtained by this method will not be reduced compared with its raw material PECH. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The gel permeation chromatography spectra of PECH and GAP prepared in Example 1 of the present invention; Figure 2 This is the nuclear magnetic resonance spectrum of GAP prepared in Example 1 of the present invention; Figure 3 The gel permeation chromatography spectra of PECH and GAP prepared in Example 2 of the present invention; Figure 4 This is the nuclear magnetic resonance spectrum of GAP prepared in Example 2 of the present invention; Figure 5 The gel permeation chromatography spectra of PECH and the prepared GAP in Example 3 of the present invention; Figure 6This is the nuclear magnetic resonance spectrum of GAP prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0018] The specific implementation of the present invention is described in detail below in conjunction with the examples. It should be understood that the specific implementation described herein is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0019] Example 1 (1) Add 0.5 g of 3-chloro-1,2-propylene glycol to the reactor, add 1 / 2 equivalent of boron trifluoride etherate, and mix well. Prepare a toluene solution of ECH (epichlorohydrin monomer) (ECH is 100 times the equivalent of 3-chloro-1,2-propylene glycol, ECH: toluene = 2:1, v:v), and quickly add the monomer solution to the three-necked flask. After the monomer solution is added, the reaction is continued for 3 h. Terminate the reaction, wash, purify, and dry to obtain PECH with a yield of 72.07%. After analysis, the number average molecular weight of the product is M n = 4000; functionality is 1.94.
[0020] (2) Add the above PECH into the reactor and add 3 times [P 444E3 + ][Cl - ], 4 times NaN3, react at 70℃ for 12h, filter, wash and dry to obtain GAP. The gel permeation chromatography and nuclear magnetic resonance spectra of the product are shown in Figure 1 and Figure 2 After analysis, the product number average molecular weight M n = 4900; functionality is 2.00.
[0021] Example 2 (1) Add 1g of 1,3-propylene glycol and 0.067 equivalent of boron trifluoride tetrahydrofuran complex to the reactor and mix well. Add 50 times the equivalent of ECH to the reactor and react for 1 hour after the monomer addition is completed. After the reaction is completed, wash, purify and dry to obtain PECH with a yield of 69.7%. GPC analysis shows that the product has a number average molecular weight of M n = 2200, functionality is 2.03.
[0022] (2) Add the above 0.2762 g PECH into the reactor and add 2 times [P 444E3 + ][Cl - ], 1.8 times NaN3, react at 90℃ for 5 h, filter, wash and dry to obtain GAP. The gel permeation chromatography and nuclear magnetic resonance spectra of the product are shown in Figure 3 and Figure 4 After analysis, the product number average molecular weight M n = 3000, functionality is 1.98.
[0023] Example 3 (1) Add 1g of 1,4-butanediol and 7 equivalents of tin tetrachloride to the reactor and mix well. Add 80 equivalents of ECH to the reactor and react for 2 hours after the monomer addition is completed. After the reaction is completed, wash, purify and dry to obtain PECH with a yield of 70.71%. GPC analysis shows that the product has a number average molecular weight of M n = 3100, functionality is 1.95.
[0024] (2) Add the above 0.2762 g PECH into the reactor and add 5 times [P 444E3 + ][Cl - ], 1.2 times NaN3, react at 80℃ for 8 h, filter, wash and dry to obtain GAP. After analysis, the product number average molecular weight M n = 3600, functionality is 1.99.
[0025] Comparative Example 1 (1) The PECH purchased from Liming Chemical Research and Design Institute Co., Ltd. was analyzed and the product number average molecular weight was M n =3300, functionality is 2.59.
[0026] (2) Add the above 0.7974 g PECH into the reactor and add 2 times [P 444E3 + ][Cl - ], 1.8 times NaN3, reacted at 80℃ for 8 h, after the reaction, filtered, washed and dried to obtain 0.667 g GAP with a yield of 66.7%. The gel permeation chromatography and nuclear magnetic resonance spectra of the product are shown in Figure 5 and Figure 6 After analysis, the product number average molecular weight M n = 4200, functionality is 2.61.
[0027] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0028] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0029] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing polyazide glycidyl ether, characterized in that: The steps include: S1. After uniformly mixing the diol initiator and the Lewis acid catalyst, epichlorohydrin monomer or its monomer solution is added dropwise, and the mixture is reacted for 1 to 3 hours after the addition is completed to obtain polyepichlorohydrin, wherein the molar ratio of the diol initiator, the Lewis acid catalyst and the epichlorohydrin monomer is (2 to 15):1:(50 to 100); S2, polyepichlorohydrin and phosphonium salt ionic liquid [P 444E3 + ][Cl - ] and the azide reagent NaN3 are mixed evenly, and reacted at 70~90℃ for 5~12 h to obtain polyazido glycidyl ether.
2. The preparation method according to claim 1, characterized in that: In step S1, the diol initiator is one or more of 1,3-propylene glycol, 1,4-butanediol, and 3-chloro-1,2-propylene glycol.
3. The preparation method according to claim 1, characterized in that: In step S1, the Lewis acid catalyst is one or more of boron trifluoride ether complex, boron trifluoride tetrahydrofuran complex, and tin tetrachloride.
4. The preparation method according to claim 1, characterized in that: In step S1, the dropping speed is 1-2.6 mL / h.
5. The preparation method according to claim 1, characterized in that: In step S1, after the reaction is terminated, the polyepichlorohydrin is obtained by washing, purification and drying.
6. The preparation method according to claim 1, characterized in that: In step S2, after the reaction is completed, the polyazide glycidyl ether is obtained by filtering, extracting, separating and drying.
7. The polyazide glycidyl ether prepared by the preparation method according to any one of claims 1 to 6, characterized in that: It has the following structure: , Wherein, n is an integer between 20 and 49.
Citation Information
Cited By
Glycidyl azide polymer and preparation method thereof
CN121108473A
A method to produce polyepichlorohydrin terminated with primary hydroxyl groups
KR102883307B1