Preparation method of thickening pigment paste carrier resin
Through the multi-step preparation method, the problem of high viscosity and difficult to thicken the pigment paste support resin is solved, and a low molecular weight and thickened resin is prepared, which improves the performance and production efficiency of the pigment paste and reduces the cost.
Patent Information
- Application Number
- CN202411012820.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-26
AI Technical Summary
The pigment paste carrier resin produced in the prior art has a large viscosity and is difficult to thicken, resulting in poor fluidity of the pigment paste, difficult to apply or mix, and requires a large amount of diluent to adjust the viscosity, which increases costs and affects performance.
The multi-step preparation method is adopted, and the reaction temperature and time are controlled through hydrolysis reaction, hydrogen ion shift addition reaction and polycondensation reaction, diol, catalyst and polymerization inhibitor are added, and the reaction is gradually heated up and the reaction is carried out in vacuum dehydration to prepare low molecular weight Thickable pigment paste carrier resin.
The prepared carrier resin has a uniform molecular weight, low viscosity and stable acid value. It can thicken through simple methods, improve the performance of the pigment paste, reduce production costs, and stable product quality, making it suitable for industrial production.
Smart Images

Figure CN119019663A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer compounds, and in particular relates to a method for preparing a carrier resin capable of thickening a pigment paste. Background Art
[0002] The pigment paste carrier resin of SMC / BMC is usually a low molecular weight saturated polyester or unsaturated polyester resin, without cross-linking monomers or active solvent dilution. Unsaturated polyester resin is generally a low viscosity polymer with ester bonds and unsaturated double bonds formed by the condensation of unsaturated dibasic acid and diol or saturated dibasic acid and unsaturated diol, and saturated polyester resin is generally a low viscosity polymer with ester bonds formed by the condensation of saturated dibasic acid and diol.
[0003] In the preparation process of pigment paste, carrier resin is often used as a base material to provide the function of bonding and stabilizing the pigment. However, in the existing technology, the prepared carrier resin has some problems during use, one of which is that the viscosity is relatively high and it is difficult to thicken. The high viscosity of the carrier resin will cause the pigment paste to have poor fluidity during use, and it is not easy to apply or mix. In addition, since it cannot be thickened effectively, a large amount of diluent is often required to adjust the viscosity, which not only increases the cost, but also may affect the performance and quality of the pigment paste. Therefore, in order to solve the problem that the carrier resin manufactured in the prior art has high viscosity and cannot be thickened, it is necessary to develop a new preparation method so that the obtained carrier resin has an appropriate viscosity and can be thickened by a simple method to improve the performance of the pigment paste and reduce production costs.
[0004] The "Preparation Method of Thickening Dicyclopentadiene Unsaturated Polyester Resin" disclosed in the patent application number CN200710051048.5 introduces a preparation method of thickening dicyclopentadiene unsaturated polyester resin, which comprises adding the reaction raw materials dibasic acid (anhydride) and deionized water into a reactor in a molar ratio of 1:1.0 to 1.2, heating to 100°C to 140°C for hydrolysis reaction for 0.5 to 1h; adding 0.05% ethanol at 110°C to 180°C; .4-0.8 mol of dicyclopentadiene is subjected to hydrogen ion shift addition reaction and diene addition reaction, and after the addition is completed, the reaction is continued at this temperature for 1-2 hours; 0.3-0.7 mol of diol and 0.07%-0.30% of the total weight of the material catalyst and 0.03%-0.07% of the total weight of the material inhibitor are added, and the temperature is gradually raised to 200℃-210℃ for condensation reaction for 0.5-1 hour; after vacuum dehydration, styrene is added for dilution to obtain the product. However, the unsaturated polyester resin synthesized by this method has a high viscosity and needs to use styrene as a diluent, which cannot meet the requirements of the pigment paste carrier resin. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a pigment paste thickening carrier resin to solve the following technical problems raised in the background technology:
[0006] The pigment paste carrier resin produced by the existing technology has the problem of high viscosity and difficulty in thickening.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0008] A method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0009] S1: adding the reaction raw materials of dibasic acid or / and dibasic acid anhydride and deionized water into the reactor in a molar ratio of 1:1.1-1.3; raising the temperature in the reactor to 110°C-140°C, and hydrolyzing the reaction raw materials for 1-2h;
[0010] S2: Control the temperature in the reactor at 120°C to 180°C; gradually add 0.3 to 0.5 mol of dicyclopentadiene into the reactor within 2 to 3 hours to perform a hydrogen ion shift addition reaction; after the addition is complete, react for another 2 to 4 hours;
[0011] S3: Control the temperature in the reactor at 120°C to 180°C, add 0.6 to 0.8 mol of diol into the reactor; let the total mass of the materials in the reactor be M, add 0.0005M to 0.003M of catalyst and 0.0002M to 0.0006M of inhibitor into the reactor; gradually raise the temperature of the reactor to 190°C to 215°C for condensation reaction for 2 to 4 hours;
[0012] S4: vacuum dehydrating the product obtained after the polycondensation reaction for 2 to 4 hours to obtain a pigment paste carrier resin.
[0013] Furthermore, the dibasic acid is fumaric acid, and the dibasic acid anhydride is maleic anhydride.
[0014] Furthermore, the diol is at least one of 1,2-propylene glycol, isobutylene glycol, isoprene glycol and dipropylene glycol.
[0015] Furthermore, the catalyst is at least one of sodium dodecylbenzene sulfonate, sodium p-toluene sulfonate, and dibutyltin oxide.
[0016] Furthermore, the polymerization inhibitor is at least one of hydroquinone, p-benzoquinone, and 2,6-di-tert-butyl-p-methylphenol.
[0017] Further, in step S2, 0.4 mol of dicyclopentadiene is added dropwise into the reactor step by step within 2.5 hours.
[0018] Furthermore, the reactor comprises a tank body and a tank cover; a temperature transmitter is arranged on the tank body, a discharge port is arranged at the bottom of the tank body, and a resistance wire is arranged in the bottom of the tank body; the tank cover is arranged on the top of the tank body, and an exhaust port, a material discharge port, a water filling port and a liquid dripping port are arranged on the tank cover;
[0019] The tank cover is also provided with a mounting seat, on which a stirring motor and a stirring shaft are provided, wherein the stirring shaft is rotatably connected to the mounting seat and the bottom of the stirring shaft extends into the tank body, a stirring blade is provided at the bottom of the stirring shaft, and the top of the stirring shaft is connected to the stirring motor;
[0020] A feeding device is arranged outside the tank body and connected to the feeding port; an insulation shell is arranged on one side of the tank body close to the bottom, and an insulation cavity is formed between the insulation shell and the tank body; a gas circulation device is also arranged outside the tank body, and the gas circulation device is used to introduce and circulate gas into the tank body or the insulation cavity.
[0021] Furthermore, a workbench is provided outside the reactor, a ladder is provided on one side of the workbench, a guardrail is provided on the periphery of the top of the workbench, and a material stacking area is provided on one side of the top of the workbench; a loading device is provided on the workbench;
[0022] Furthermore, the feeding device includes a feeding frame, a filter screen, a feeding barrel, a conveying roller, a conveying blade and a feeding motor; wherein, the feeding frame is arranged on a workbench, and the interior of the feeding frame has an inner cavity with an inverted triangle structure; one end of the feeding barrel is connected to the bottom of the feeding frame and communicates with the inner cavity of the feeding frame, and the other end of the feeding barrel extends to the blanking port, and the feeding barrel has an opening facing the blanking port; the conveying roller is rotatably connected in the feeding barrel, and the feeding motor is connected to one side of the feeding barrel and connected to the conveying roller; the conveying blade is fixedly connected to the outer side of the conveying roller, and the conveying blade is in a spiral structure on the outer side of the conveying roller.
[0023] Furthermore, an air inlet connector, an air guide connector and an air outlet connector are provided on one side of the tank body, the air inlet connector is located near the top of the tank body and is connected to the inner cavity of the tank body, the air outlet connector is located near the bottom of the tank body and is connected to the inner cavity of the tank body, and the air guide connector is connected to the heat preservation cavity; the gas circulation device comprises a mounting shell, a pressure transmission member, a piston cylinder, a piston, a connecting rod, a driving disk and a driving motor; the pressure transmission member is arranged in the mounting shell, one side of the pressure transmission member is connected to a main pipe, and the other side of the pressure transmission member is connected to an air supply pipe; an air inlet pipe, an air guide pipe and an air outlet pipe are connected to the main pipe, the air inlet pipe is connected to the air inlet connector, the air guide pipe is connected to the air guide connector, and the air outlet pipe is connected to the air outlet connector; a first one-way valve is provided on the air inlet pipe, a second one-way valve is provided on the air outlet pipe, and a stop valve is provided on the air supply pipe;
[0024] The piston cylinder is connected to the pressure transmission part and is located between the main pipe and the air supply pipe, and the piston is movably sealed and connected in the piston cylinder; the driving disk is rotatably connected to the mounting shell, the top of the connecting rod is hinged to the piston, and the bottom of the connecting rod is hinged to one side of the driving disk; the driving motor is arranged in the mounting shell, and the driving motor is connected to the driving disk and is used to drive the driving disk to rotate.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The present invention adds dibasic acid or / and dibasic acid anhydride and deionized water into a reactor according to a certain molar ratio and heats up, so that the reaction raw materials undergo a hydrolysis reaction. This step helps to adjust the structure and functionality of the reactants and lays a foundation for subsequent reactions. By dripping dicyclopentadiene step by step to carry out a hydrogen ion shift addition reaction, the reaction temperature and time are controlled to promote the reaction. This step helps to introduce specific structural units and improve the performance of the carrier resin. By adding diols, catalysts and inhibitors into the reactor and gradually heating up to carry out a polycondensation reaction. This step helps to increase the degree of crosslinking between the reactants. The carrier resin finally obtained has a uniform and low molecular weight, and has the advantages of low viscosity, stable acid value and thickening.
[0027] The present invention adopts a multi-step synthesis technology, which is easy to operate, has a uniform molecular weight of the carrier resin, stable product quality, simple process, easy to expand industrial production, and strong practicality.
[0028] The invention adopts industrial byproduct dicyclopentadiene as raw material, which has a relatively low price and low product cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic diagram of the overall structure of the reactor of the present invention;
[0030] Figure 2 It is a schematic diagram of the overall structure of the tank body and the tank cover of the present invention;
[0031] Figure 3 It is a schematic diagram of the internal structure of the tank body of the present invention;
[0032] Figure 4 It is a schematic diagram of the internal structure of the gas circulation device of the present invention.
[0033] Markings in the figure: 1-reactor, 2-guardrail, 3-workbench, 4-feeding device, 5-ladder, 6-stack area, 7-gas circulation device, 8-discharge port, 9-cover, 10-conveying blade, 11-feeding frame, 12-filter, 13-exhaust port, 14-feeding barrel, 15-mounting seat, 16-stirring motor, 17-feeding motor, 18-drip port, 19-water inlet, 20-temperature transmitter, 21-feeding port, 22-tank, 23-reducer, 24-bearing, 25- A one-way valve, 26-inlet pipe, 27-main pipe, 28-installation shell, 29-air supply pipe, 30-stop valve, 31-pressure transmission member, 32-second one-way valve, 33-outlet pipe, 34-outlet connector, 35-air guide connector, 36-air guide pipe, 37-inlet connector, 38-stirring shaft, 39-stirring blade, 40-insulation shell, 41-insulation chamber, 42-rotating shaft, 43-piston, 44-belt, 45-drive motor, 46-drive disk, 47-connecting rod, 48-piston cylinder. DETAILED DESCRIPTION
[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Example:
[0036] A method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0037] S1: Add the reaction raw materials dibasic acid or / and dibasic acid anhydride and deionized water to the reactor 1 in a molar ratio of 1:1.1 to 1.3; raise the temperature in the reactor 1 to 110°C to 140°C to hydrolyze the reaction raw materials for 1 to 2 hours; in step S1, the reaction raw materials are hydrolyzed by adding the dibasic acid or / and dibasic acid anhydride and deionized water to the reactor 1 in a certain molar ratio and raising the temperature. This step helps to adjust the structure and functionality of the reactants and lays the foundation for subsequent reactions.
[0038] S2: Control the temperature in the reactor 1 at 120°C to 180°C; within 2 to 3 hours, drop 0.3 to 0.5 mol of dicyclopentadiene into the reactor 1 step by step to carry out hydrogen ion displacement addition reaction; after the dropwise addition, react for another 2 to 4 hours; in step S2, the reaction temperature and time are controlled by dropwise adding dicyclopentadiene step by step to carry out hydrogen ion displacement addition reaction, and the reaction is promoted. This step helps to introduce specific structural units and improve the performance of the carrier resin.
[0039] S3: Control the temperature in reactor 1 at 120℃~180℃, add 0.6~0.8mol diol into reactor 1; let the total mass of the materials in reactor 1 be M, take 0.0005M~0.003M catalyst and 0.0002M~0.0006M inhibitor and add them into reactor 1; gradually heat reactor 1 to 190℃~215℃ for polycondensation reaction for 2~4h; in step S3, add diol, catalyst and inhibitor into reactor 1, and gradually heat up for polycondensation reaction. This step helps to increase the degree of crosslinking between reactants. The carrier resin finally obtained has low molecular weight, low viscosity, stable acid value, and the resin can be thickened, thus solving the problem that the original carrier resin has high viscosity and cannot be thickened.
[0040] S4: The product obtained after the polycondensation reaction is vacuum dehydrated for 2 to 4 hours to obtain a pigment paste carrier resin. Finally, in step S4, the product obtained after the polycondensation reaction is vacuum dehydrated. This step helps to remove residual solvents and impurities, ensuring that the final pigment paste carrier resin has good purity and stability.
[0041] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0042] S1.01: Add 150 g (1.53 mol) of maleic anhydride and 30.2 g (1.68 mol) of deionized water into reactor 1 and stir; raise the temperature in reactor 1 to 110°C to 120°C to allow the raw materials to undergo hydrolysis for 1 hour;
[0043] S2.01: Control the temperature in reactor 1 to 110°C to 140°C; add 80.6 g (0.61 mol) of dicyclopentadiene stepwise into reactor 1 within 2.5 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 3 hours;
[0044] S3.01: Control the temperature in reactor 1 at 120°C to 140°C, add 81.4g (1.07mol) of propylene glycol into reactor 1; add 0.68g (0.0020mol) of sodium dodecylbenzene sulfonate as a catalyst into reactor 1, and add 0.14g (0.0013mol) of hydroquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for polycondensation reaction for 3h;
[0045] S4.01: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 hours.
[0046] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0047] Resin thickening experiment, the specific steps are as follows:
[0048] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours, and measure the viscosity of the resin. The specific properties of the resin product prepared in this example are shown in the following table:
[0049] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 20.5 1858 8756
[0050] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0051] S1.02: Add 150 g (1.53 mol) of maleic anhydride and 30.2 g (1.68 mol) of deionized water into reactor 1 and stir; raise the temperature in reactor 1 to 110°C to 120°C to allow the raw materials to undergo hydrolysis for 1 hour;
[0052] S2.02: Control the temperature in reactor 1 to 110°C to 140°C; add 101.8 g (0.77 mol) of dicyclopentadiene into reactor 1 stepwise over 2.5 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 3 hours;
[0053] S3.02: Control the temperature in reactor 1 at 120°C to 140°C, add 70g (0.92mol) of propylene glycol into reactor 1; add 0.68g (0.0020mol) of sodium dodecylbenzene sulfonate as a catalyst into reactor 1, and add 0.14g (0.0013mol) of hydroquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for condensation reaction for 3h;
[0054] S4.02: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 hours.
[0055] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0056] Resin thickening experiment, the specific steps are as follows:
[0057] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours. The specific properties of the resin product prepared in this example are shown in the following table:
[0058] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 22.8 1030 5172
[0059] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0060] S1.03: 150 g (1.53 mol) of maleic anhydride and 30.2 g (1.68 mol) of deionized water were added to the reactor 1 and stirred; the temperature in the reactor 1 was raised to 110°C to 120°C, and the reaction materials were hydrolyzed for 1 hour;
[0061] S2.03: Control the temperature in the reactor 1 at 110°C to 140°C; add 60.8 g (0.46 mol) of dicyclopentadiene into the reactor 1 stepwise over 2.5 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 3 hours;
[0062] S3.03: Control the temperature in reactor 1 at 120°C to 140°C, add 92.7g (1.22mol) of propylene glycol into reactor 1; add 0.68g (0.0020mol) of sodium dodecylbenzene sulfonate as a catalyst into reactor 1, and add 0.14g (0.0013mol) of hydroquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for condensation reaction for 3h;
[0063] S4.03: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 hours.
[0064] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0065] Resin thickening experiment, the specific steps are as follows:
[0066] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours. The specific properties of the resin product prepared in this example are shown in the following table:
[0067] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 18.2 2496 9983
[0068] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0069] S1.04: 150 g (1.53 mol) of maleic anhydride and 33.1 g (1.99 mol) of deionized water were added to the reactor 1 and stirred; the temperature in the reactor 1 was raised to 110°C to 120°C to allow the reaction materials to undergo a hydrolysis reaction for 1 hour;
[0070] S2.04: Control the temperature in the reactor 1 at 110°C to 140°C; add 80.6 g (0.61 mol) of dicyclopentadiene into the reactor 1 stepwise over 2.5 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 3 hours;
[0071] S3.04: Control the temperature in reactor 1 at 120°C to 140°C, add 81.4g (1.07mol) of propylene glycol into reactor 1; add 0.68g (0.0020mol) of sodium dodecylbenzene sulfonate as a catalyst into reactor 1, and add 0.14g (0.0013mol) of hydroquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for polycondensation reaction for 3h;
[0072] S4.04: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 hours.
[0073] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0074] Resin thickening experiment, the specific steps are as follows:
[0075] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours, and measure the viscosity of the resin. The specific properties of the resin product prepared in this example are shown in the following table:
[0076] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 19.8 1733 8062
[0077] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0078] S1.05: 150 g (1.53 mol) of maleic anhydride and 30.2 g (1.68 mol) of deionized water were added to the reactor 1 and stirred; the temperature in the reactor 1 was raised to 110°C to 120°C to allow the reaction materials to undergo a hydrolysis reaction for 1 hour;
[0079] S2.05: Control the temperature in the reactor 1 at 110°C to 140°C; add 80.6 g (0.61 mol) of dicyclopentadiene stepwise into the reactor 1 within 2.5 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 3 hours;
[0080] S3.05: Control the temperature in reactor 1 at 120°C to 140°C, add 81.4g (1.07mol) of propylene glycol into reactor 1; add 1.02g (0.0029mol) of sodium dodecylbenzene sulfonate as a catalyst into reactor 1, and add 0.14g (0.0013mol) of hydroquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for polycondensation reaction for 3h;
[0081] S4.05: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 hours.
[0082] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0083] Resin thickening experiment, the specific steps are as follows:
[0084] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours, and measure the viscosity of the resin. The specific properties of the resin product prepared in this example are shown in the following table:
[0085] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 19.5 2127 9165
[0086] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0087] S1.06: 150 g (1.53 mol) of maleic anhydride and 30.2 g (1.68 mol) of deionized water were added to the reactor 1 and stirred; the temperature in the reactor 1 was raised to 110°C to 120°C, and the reaction materials were hydrolyzed for 1 hour;
[0088] S2.06: Control the temperature in the reactor 1 at 110°C to 140°C; add 80.6 g (0.61 mol) of dicyclopentadiene stepwise into the reactor 1 within 2.5 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 3 hours;
[0089] S3.06: Control the temperature in reactor 1 at 120°C to 140°C, add 81.4g (1.07mol) of propylene glycol into reactor 1; add 0.17g (0.0005mol) of sodium dodecylbenzene sulfonate as a catalyst into reactor 1, and add 0.14g (0.0013mol) of hydroquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for condensation reaction for 3h;
[0090] S4.06: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 hours.
[0091] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0092] Resin thickening experiment, the specific steps are as follows:
[0093] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours, and measure the viscosity of the resin. The specific properties of the resin product prepared in this example are shown in the following table:
[0094] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 22.3 1963 7825
[0095] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0096] S1.07: 150 g (1.53 mol) of maleic anhydride and 30.2 g (1.68 mol) of deionized water were added to the reactor 1 and stirred; the temperature in the reactor 1 was raised to 110°C to 120°C to allow the reaction materials to undergo a hydrolysis reaction for 1 hour;
[0097] S2.07: Control the temperature in the reactor 1 at 110°C to 140°C; add 80.6 g (0.61 mol) of dicyclopentadiene stepwise into the reactor 1 within 2.5 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 3 hours;
[0098] S3.07: Control the temperature in reactor 1 at 120°C to 140°C, add 81.4g (1.07mol) of propylene glycol into reactor 1; add 0.68g (0.0035mol) of sodium toluenesulfonate as a catalyst into reactor 1, and add 0.14g (0.0013mol) of hydroquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for polycondensation reaction for 3h;
[0099] S4.07: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 hours.
[0100] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0101] Resin thickening experiment, the specific steps are as follows:
[0102] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours, and measure the viscosity of the resin. The specific properties of the resin product prepared in this example are shown in the following table:
[0103] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 20.3 1822 8243
[0104] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0105] S1.08: 150 g (1.53 mol) of maleic anhydride and 30.2 g (1.68 mol) of deionized water were added to the reactor 1 and stirred; the temperature in the reactor 1 was raised to 110°C to 120°C to allow the reaction materials to undergo a hydrolysis reaction for 1 hour;
[0106] S2.08: Control the temperature in the reactor 1 at 110°C to 140°C; add 80.6 g (0.61 mol) of dicyclopentadiene stepwise into the reactor 1 within 2.5 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 3 hours;
[0107] S3.08: Control the temperature in reactor 1 at 120°C to 140°C, add 81.4g (1.07mol) of propylene glycol into reactor 1; add 0.68g (0.0035mol) of sodium p-toluenesulfonate as a catalyst into reactor 1, and add 0.14g (0.0013mol) of hydroquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for polycondensation reaction for 3h;
[0108] S4.08: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 hours.
[0109] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0110] Resin thickening experiment, the specific steps are as follows:
[0111] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours, and measure the viscosity of the resin. The specific properties of the resin product prepared in this example are shown in the following table:
[0112] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 20.9 1928 8763
[0113] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0114] S1.09: 150 g (1.53 mol) of maleic anhydride and 30.2 g (1.68 mol) of deionized water were added to the reactor 1 and stirred; the temperature in the reactor 1 was raised to 110°C to 120°C to allow the reaction materials to undergo a hydrolysis reaction for 1 hour;
[0115] S2.09: Control the temperature in the reactor 1 at 110°C to 140°C; add 80.6 g (0.61 mol) of dicyclopentadiene stepwise into the reactor 1 within 2.5 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 3 hours;
[0116] S3.09: Control the temperature in reactor 1 at 120°C to 140°C, add 81.4g (1.07mol) of propylene glycol into reactor 1; add 0.68g (0.0027mol) of dibutyltin oxide as a catalyst into reactor 1, and add 0.14g (0.0013mol) of hydroquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for condensation reaction for 3h;
[0117] S4.09: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 hours.
[0118] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0119] Resin thickening experiment, the specific steps are as follows:
[0120] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours, and measure the viscosity of the resin. The specific properties of the resin product prepared in this example are shown in the following table:
[0121] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 21.3 2259 9377
[0122] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0123] S1.10: 150 g (1.53 mol) of maleic anhydride and 30.2 g (1.68 mol) of deionized water were added to the reactor 1 and stirred; the temperature in the reactor 1 was raised to 110°C to 120°C, and the reaction materials were hydrolyzed for 1 hour;
[0124] S2.10: Control the temperature in the reactor 1 at 110°C to 140°C; add 80.6 g (0.61 mol) of dicyclopentadiene stepwise into the reactor 1 within 2.5 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 3 hours;
[0125] S3.10: Control the temperature in reactor 1 at 120°C to 140°C, add 81.4g (1.07mol) of propylene glycol into reactor 1; add 0.68g (0.0020mol) of sodium dodecylbenzene sulfonate as a catalyst into reactor 1, and add 0.21g (0.0019mol) of hydroquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for polycondensation reaction for 3h;
[0126] S4.10: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 h.
[0127] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0128] Resin thickening experiment, the specific steps are as follows:
[0129] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours, and measure the viscosity of the resin. The specific properties of the resin product prepared in this example are shown in the following table:
[0130] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 20.3 1876 8491
[0131] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0132] S1.11: 150 g (1.53 mol) of maleic anhydride and 30.2 g (1.68 mol) of deionized water were added to the reactor 1 and stirred; the temperature in the reactor 1 was raised to 110°C to 120°C, and the reaction materials were hydrolyzed for 1 hour;
[0133] S2.11: Control the temperature in the reactor 1 at 110°C to 140°C; add 80.6 g (0.61 mol) of dicyclopentadiene stepwise into the reactor 1 within 2.5 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 3 hours;
[0134] S3.11: Control the temperature in reactor 1 at 120°C to 140°C, add 81.4g (1.07mol) of propylene glycol into reactor 1; add 0.68g (0.0020mol) of sodium dodecylbenzene sulfonate as a catalyst into reactor 1, and add 0.07g (0.0006mol) of hydroquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for condensation reaction for 3h;
[0135] S4.11: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 hours.
[0136] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0137] Resin thickening experiment, the specific steps are as follows:
[0138] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours, and measure the viscosity of the resin. The specific properties of the resin product prepared in this example are shown in the following table:
[0139] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 20.7 1698 7634
[0140] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0141] S1.12: 150 g (1.53 mol) of maleic anhydride and 30.2 g (1.68 mol) of deionized water were added to the reactor 1 and stirred; the temperature in the reactor 1 was raised to 110°C to 120°C, and the reaction materials were hydrolyzed for 1 hour;
[0142] S2.12: Control the temperature in the reactor 1 at 110°C to 140°C; add 80.6 g (0.61 mol) of dicyclopentadiene stepwise into the reactor 1 within 2.5 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 3 hours;
[0143] S3.12: Control the temperature in reactor 1 at 120°C to 140°C, add 81.4g (1.07mol) of propylene glycol into reactor 1; add 0.68g (0.0020mol) of sodium dodecylbenzene sulfonate as a catalyst into reactor 1, and add 0.14g (0.0013mol) of benzoquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for condensation reaction for 3h;
[0144] S4.12: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 hours.
[0145] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0146] Resin thickening experiment, the specific steps are as follows:
[0147] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours, and measure the viscosity of the resin. The specific properties of the resin product prepared in this example are shown in the following table:
[0148] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 19.6 1718 7867
[0149] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0150] S1.13: 150 g (1.53 mol) of maleic anhydride and 30.2 g (1.68 mol) of deionized water were added to the reactor 1 and stirred; the temperature in the reactor 1 was raised to 110°C to 120°C, and the reaction materials were hydrolyzed for 1 hour;
[0151] S2.13: Control the temperature in the reactor 1 at 110°C to 140°C; add 80.6 g (0.61 mol) of dicyclopentadiene stepwise into the reactor 1 within 2.5 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 3 hours;
[0152] S3.13: Control the temperature in reactor 1 at 120°C to 140°C, add 81.4g (1.07mol) of propylene glycol into reactor 1; add 0.68g (0.0020mol) of sodium dodecylbenzene sulfonate as a catalyst into reactor 1, and add 0.14g (0.0006mol) of 2,6-di-tert-butyl-p-methylphenol as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for condensation reaction for 3h;
[0153] S4.13: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 hours.
[0154] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0155] Resin thickening experiment, the specific steps are as follows:
[0156] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours, and measure the viscosity of the resin. The specific properties of the resin product prepared in this example are shown in the following table:
[0157] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 21.4 1913 8044
[0158] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0159] S1.14: 150 g (1.53 mol) of maleic anhydride and 30.2 g (1.68 mol) of deionized water were added to the reactor 1 and stirred; the temperature in the reactor 1 was raised to 110°C to 120°C, and the reaction materials were hydrolyzed for 1 hour;
[0160] S2.14: Control the temperature in the reactor 1 at 110°C to 140°C; add 80.6 g (0.61 mol) of dicyclopentadiene stepwise into the reactor 1 within 3 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 2 hours;
[0161] S3.14: Control the temperature in reactor 1 at 120°C to 140°C, add 81.4g (1.07mol) of propylene glycol into reactor 1; add 0.68g (0.0020mol) of sodium dodecylbenzene sulfonate as a catalyst into reactor 1, and add 0.14g (0.0013mol) of hydroquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for polycondensation reaction for 3h;
[0162] S4.14: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 hours.
[0163] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0164] Resin thickening experiment, the specific steps are as follows:
[0165] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours, and measure the viscosity of the resin. The specific properties of the resin product prepared in this example are shown in the following table:
[0166] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 21.8 2096 9181
[0167] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0168] S1.15: 150 g (1.53 mol) of maleic anhydride and 30.2 g (1.68 mol) of deionized water were added to the reactor 1 and stirred; the temperature in the reactor 1 was raised to 110°C to 120°C, and the reaction materials were hydrolyzed for 1 hour;
[0169] S2.15: Control the temperature in the reactor 1 at 110°C to 140°C; add 80.6 g (0.61 mol) of dicyclopentadiene stepwise into the reactor 1 within 2 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 4 hours;
[0170] S3.15: Control the temperature in reactor 1 at 120°C to 140°C, add 81.4g (1.07mol) of propylene glycol into reactor 1; add 0.68g (0.0020mol) of sodium dodecylbenzene sulfonate as a catalyst into reactor 1, and add 0.14g (0.0013mol) of hydroquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for polycondensation reaction for 3h;
[0171] S4.15: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 hours.
[0172] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0173] Resin thickening experiment, the specific steps are as follows:
[0174] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours, and measure the viscosity of the resin. The specific properties of the resin product prepared in this example are shown in the following table:
[0175] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 18.8 2257 9722
[0176] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0177] S1.16: Add 75 g (0.77 mol) of maleic anhydride, 75 g (1.02 mol) of fumaric acid and 15.1 g (0.84 mol) of deionized water into reactor 1 and stir; raise the temperature in reactor 1 to 110°C to 120°C to allow the reaction materials to undergo hydrolysis for 1 hour;
[0178] S2.16: Control the temperature in the reactor 1 at 110°C to 140°C; add 80.6 g (0.61 mol) of dicyclopentadiene stepwise into the reactor 1 within 2.5 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 3 hours;
[0179] S3.16: Control the temperature in reactor 1 at 120°C to 140°C, add 81.4g (1.07mol) of propylene glycol into reactor 1; add 0.68g (0.0020mol) of sodium dodecylbenzene sulfonate as a catalyst into reactor 1, and add 0.14g (0.0013mol) of hydroquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for condensation reaction for 3h;
[0180] S4.16: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 hours.
[0181] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0182] Resin thickening experiment, the specific steps are as follows:
[0183] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours, and measure the viscosity of the resin. The specific properties of the resin product prepared in this example are shown in the following table:
[0184] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 22.5 2413 9829
[0185] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0186] S1.17: 75 g (0.77 mol) of fumaric acid and 75 g (1.02 mol) of fumaric acid were added to the reactor 1 and stirred; the temperature in the reactor 1 was raised to 110°C to 120°C, and the reaction materials were hydrolyzed for 1 hour;
[0187] S2.17: Control the temperature in the reactor 1 at 110°C to 140°C; add 80.6 g (0.61 mol) of dicyclopentadiene stepwise into the reactor 1 within 2.5 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 3 hours;
[0188] S3.17: Control the temperature in reactor 1 at 120°C to 140°C, add 81.4g (1.07mol) of propylene glycol into reactor 1; add 0.68g (0.0020mol) of sodium dodecylbenzene sulfonate as a catalyst into reactor 1, and add 0.14g (0.0013mol) of hydroquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for polycondensation reaction for 3h;
[0189] S4.17: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 hours.
[0190] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0191] Resin thickening experiment, the specific steps are as follows:
[0192] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours, and measure the viscosity of the resin. The specific properties of the resin product prepared in this example are shown in the following table:
[0193] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 19.1 1158 5835
[0194] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0195] S1.18: 150 g (1.53 mol) of maleic anhydride and 30.2 g (1.68 mol) of deionized water were added to the reactor 1 and stirred; the temperature in the reactor 1 was raised to 110°C to 120°C, and the reaction materials were hydrolyzed for 1 hour;
[0196] S2.18: Control the temperature in the reactor 1 at 110°C to 140°C; add 80.6 g (0.61 mol) of dicyclopentadiene stepwise into the reactor 1 within 2 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 4 hours;
[0197] S3.18: Control the temperature in reactor 1 at 120°C to 140°C, add 96.4 (1.07 mol) of isobutylene glycol into reactor 1; add 0.68 g (0.0020 mol) of sodium dodecylbenzene sulfonate as a catalyst into reactor 1, and add 0.14 g (0.0013 mol) of hydroquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for condensation reaction for 3 hours;
[0198] S4.18: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 hours.
[0199] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0200] Resin thickening experiment, the specific steps are as follows:
[0201] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours, and measure the viscosity of the resin. The specific properties of the resin product prepared in this example are shown in the following table:
[0202] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 19.7 1233 6241
[0203] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0204] S1.19: 150 g (1.53 mol) of maleic anhydride and 30.2 g (1.68 mol) of deionized water were added to the reactor 1 and stirred; the temperature in the reactor 1 was raised to 110°C to 120°C, and the reaction materials were hydrolyzed for 1 hour;
[0205] S2.19: Control the temperature in the reactor 1 at 110°C to 140°C; add 80.6 g (0.61 mol) of dicyclopentadiene stepwise into the reactor 1 within 2 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 4 hours;
[0206] S3.19: Control the temperature in reactor 1 at 120°C to 140°C, add 111.3 g (1.07 mol) of isopentyl glycol into reactor 1; add 0.68 g (0.0020 mol) of sodium dodecylbenzene sulfonate as a catalyst into reactor 1, and add 0.14 g (0.0013 mol) of hydroquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for condensation reaction for 3 hours;
[0207] S4.19: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 hours.
[0208] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0209] Resin thickening experiment, the specific steps are as follows:
[0210] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours, and measure the viscosity of the resin. The specific properties of the resin product prepared in this example are shown in the following table:
[0211] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 19.9 2373 6693
[0212] In a preferred embodiment, a method for preparing a pigment paste thickening carrier resin comprises the following steps:
[0213] S1.20: 150 g (1.53 mol) of maleic anhydride and 30.2 g (1.68 mol) of deionized water were added to the reactor 1 and stirred; the temperature in the reactor 1 was raised to 110°C to 120°C, and the reaction materials were hydrolyzed for 1 hour;
[0214] S2.20: Control the temperature in the reactor 1 at 110°C to 140°C; add 80.6 g (0.61 mol) of dicyclopentadiene stepwise into the reactor 1 within 2 hours to carry out hydrogen ion shift addition reaction; after the addition is complete, react for another 4 hours;
[0215] S3.20: Control the temperature in reactor 1 at 120°C to 140°C, add 63.2g (0.82mol) of propylene glycol and 33.5g (0.25mol) of dipropylene glycol into reactor 1; add 0.68g (0.0020mol) of sodium dodecylbenzene sulfonate as a catalyst into reactor 1, and add 0.14g (0.0013mol) of hydroquinone as a polymerization inhibitor into reactor 1. Gradually raise the temperature of reactor 1 to 190°C to 215°C for polycondensation reaction for 3h;
[0216] S4.20: Measure the acid value of the reactants in reactor 1. When the acid value of the reactants reaches 30 mgKOH / g, vacuum dehydrate the reactants for 2 h.
[0217] Continue to measure the acid value of the reactants. When the acid value of the reactants reaches 18 mgKOH / g to 23 mgKOH / g, release the vacuum and cool to below 60°C to obtain the carrier resin product. When the acid value of the reactants is greater than 23 mgKOH / g, continue to vacuum dehydration until the acid value of the reactants is less than 23 mgKOH / g.
[0218] Resin thickening experiment, the specific steps are as follows:
[0219] To prepare the resin, add 150 g of aluminum hydroxide with a particle size of 15 μm and 1 g of active magnesium oxide to every 100 g of the resin, stir evenly, and store at 40° C. for 24 hours, and measure the viscosity of the resin. The specific properties of the resin product prepared in this example are shown in the following table:
[0220] Acid value mgKOH / g Viscosity (25℃) mPa.S Viscosity after thickening (25℃) mPa.S 21.7 2404 8769
[0221] Specifically, the viscosity of the carrier resin product manufactured by the above embodiments is 1000-2500 mPa·s (25°C), and the acid value is 18-23 mgKOH / g. After the resin thickening test (150 g of aluminum hydroxide with a particle size of 10 μm and 1 g of active magnesium oxide were added to 100 g of resin, stirred evenly, and stored at 40°C for 24 hours), the viscosity of the resin paste increased to 5000-10000 mPa·s (25°C). Therefore, the carrier resin manufactured by the present application can effectively solve the problem of high initial viscosity and difficulty in thickening of the carrier resin in the prior art.
[0222] In a preferred embodiment, the dibasic acid is fumaric acid, and the dibasic anhydride is maleic anhydride.
[0223] In a preferred embodiment, the diol is at least one of 1,2-propylene glycol, isobutylene glycol, isoprene glycol, and dipropylene glycol. Specifically, the diol can be any of 1,2-propylene glycol, isobutylene glycol, isoprene glycol, or dipropylene glycol. The diol can be a combination of any two of 1,2-propylene glycol, isobutylene glycol, isoprene glycol, or dipropylene glycol in any ratio.
[0224] In a preferred embodiment, the catalyst is at least one of sodium dodecylbenzene sulfonate, sodium p-toluene sulfonate, and dibutyltin oxide. Specifically, the catalyst can be any one of sodium dodecylbenzene sulfonate, sodium p-toluene sulfonate, and dibutyltin oxide. The catalyst can be a combination of any two of sodium dodecylbenzene sulfonate, sodium p-toluene sulfonate, and dibutyltin oxide in any ratio.
[0225] In a preferred embodiment, the polymerization inhibitor is at least one of hydroquinone, p-benzoquinone, and 2,6-di-tert-butyl-p-methylphenol. Specifically, the polymerization inhibitor can be any one of hydroquinone, p-benzoquinone, and 2,6-di-tert-butyl-p-methylphenol. The polymerization inhibitor can be a combination of any two of hydroquinone, p-benzoquinone, and 2,6-di-tert-butyl-p-methylphenol in any ratio.
[0226] In a preferred embodiment, in a better choice, in step S2, 0.4 mol of dicyclopentadiene is added dropwise into reactor 1 step by step within 2.5 hours.
[0227] In a preferred embodiment, Figure 2 As shown, the reactor 1 includes a tank body 22 and a tank cover 9; a temperature transmitter 20 is provided on the tank body 22, a discharge port 8 is provided at the bottom of the tank body 22, and a resistance wire is provided in the bottom of the tank body 22; the tank cover 9 is provided at the top of the tank body 22, and an exhaust port 13, a discharge port 21, a water inlet 19 and a drip port 18 are provided on the tank cover 9. Specifically, the resistance wire in the bottom of the tank body 22 is connected to a power supply, and the power supply is used to supply power to the resistance wire to generate heat, and the tank body 22 heats the reactant through the resistance wire. The temperature transmitter 20 on the tank body 22 can adopt an integrated isolated temperature transmitter 20 of the FST600-203 type. The discharge port 8 at the bottom of the tank body 22 is used for discharge. The discharge port 21 on the tank cover 9 is used for feeding, and the water inlet 19 on the tank cover 9 is used for adding water into the tank body 22. The dripping port 18 on the tank cover 9 is used to install a dripping device and drip dicyclopentadiene into the tank body 22. Specifically, the dripping device can be an automatic raw material dripping device disclosed in the publication number CN213160694U. It should also be noted that the exhaust port 13, the material drop port 21, the water addition port 19 and the dripping port 18 on the tank cover 9 shown in the figure are all open. In actual use, each port should be closed after the addition is completed.
[0228] like Figure 3As shown, a mounting seat 15 is also provided on the tank cover 9, and a stirring motor 16 and a stirring shaft 38 are provided on the mounting seat 15, wherein the stirring shaft 38 is rotatably connected to the mounting seat 15 and the bottom of the stirring shaft 38 extends into the tank body 22, and a stirring blade 39 is provided at the bottom of the stirring shaft 38, and the top of the stirring shaft 38 is connected to the stirring motor 16. Among them, the mounting seat 15 is used to install the stirring motor 16 and the stirring shaft 38. The motor is used to drive the stirring shaft 38 to rotate. More specifically, a reducer 23 is also fixedly connected to the base, and the output shaft of the stirring motor 16 is connected to the reducer 23, and a rotating shaft 42 is provided at the output end of the reducer 23. A bearing 24 is also provided on the mounting seat 15, and the rotating shaft 42 is rotatably connected to the bearing 24. The bearing 24 is used to stabilize the rotation of the rotating shaft 42. The stirring shaft 38 is connected to the rotating shaft 42. In actual use, the stirring motor 16 drives the rotating shaft 42 on the reducer 23 to rotate, and the rotating shaft 42 drives the stirring shaft 38 to rotate, and the stirring shaft 38 stirs the raw materials in the tank body 22 through the stirring blades 39 at the bottom. By providing the reducer 23, the torque of the rotating shaft 42 and the stirring shaft 38 can be increased, so that the raw materials can be stably stirred.
[0229] like Figure 1 As shown, a feeding device 4 is provided outside the tank body 22, and the feeding device 4 is connected to the blanking port 21; a heat preservation shell 40 is provided on one side of the tank body 22 near the bottom, and a heat preservation chamber 41 is formed between the heat preservation shell 40 and the tank body 22; a gas circulation device 7 is also provided outside the tank body 22, and the gas circulation device 7 is used to pass gas into the tank body 22 or the heat preservation chamber 41 and circulate. The feeding device 4 is used to transport the raw materials to the top of the blanking port 21 and put the raw materials into the tank body 22 through the blanking port 21. The heat preservation shell 40 is used to keep the tank body 22 warm, which can achieve energy saving. The gas circulation device 7 is used to pass inert gas into the tank body 22 so that the solution in the tank body 22 is surging, which is beneficial to the reaction of the raw materials. At the same time, the gas circulation device 7 can also recycle the heated inert gas in the tank body 22 into the gas circulation device 7 and introduce the heated inert gas into the heat preservation chamber 41 to keep the tank body 22 warm. Inert gas is used because it will not react with the raw materials. Optimally, since there is a lot of steam in the tank 22, the steam may enter the gas circulation device 7 or the insulation chamber 41. Therefore, a drain port is provided on the gas circulation device 7 and the insulation shell 40, and the drain port is used to discharge the condensed water.
[0230] In a preferred embodiment, Figure 1As shown, a workbench 3 is also provided outside the reactor 1, a ladder 5 is provided on one side of the workbench 3, a guardrail 2 is provided on the periphery of the top of the workbench 3, and a stacking area 6 is provided on one side of the top of the workbench 3; a feeding device 4 is provided on the workbench 3; it should be noted that the reactor 1 shown in this embodiment is a reactor 1 for realizing mass production. The workbench 3 is used to facilitate the staff to operate the reactor 1. The ladder 5 is used to facilitate the staff to climb onto the workbench 3. The guardrail 2 on the periphery of the top of the workbench 3 is used to protect the staff. The stacking area 6 on the top of the workbench 3 is used for temporary stacking of raw materials, and can also cooperate with the feeding device 4 for feeding, so as to facilitate the addition of reaction raw materials into the tank body 22.
[0231] In a preferred embodiment, if Figure 2 As shown, the feeding device 4 includes a feeding frame 11, a filter screen 12, a feeding barrel 14, a conveying roller, a conveying blade 10 and a feeding motor 17; wherein the feeding frame 11 is arranged on the workbench 3, and the feeding frame 11 has an inner cavity with an inverted triangle structure; one end of the feeding barrel 14 is connected to the bottom of the feeding frame 11 and communicates with the inner cavity of the feeding frame 11, and the other end of the feeding barrel 14 extends to the blanking port 21, and the feeding barrel 14 has an opening facing the blanking port 21; the conveying roller is rotatably connected in the feeding barrel 14, and the feeding motor 17 is connected to one side of the feeding barrel 14 and connected to the conveying roller; the conveying blade 10 is fixed to the outer side of the conveying roller, and the conveying blade 10 is in a spiral structure on the outer side of the conveying roller. The inner cavity with an inverted triangle structure inside the feeding frame 11 is used to allow the raw materials at the bottom of the feeding frame 11 to be concentrated in the middle. In actual use, the raw materials are first poured into the loading frame 11. The filter screen 12 on the top of the loading frame 11 can filter impurities and hardened raw materials. The loading motor 17 drives the conveying roller to rotate, and the conveying roller drives the conveying blade 10 to rotate. The rotating conveying blade 10 can push the raw materials upward and put the raw materials into the tank body 22 through the opening of the loading barrel 14. This design can automatically complete the feeding of raw materials.
[0232] In a preferred embodiment, if Figure 4As shown, an air inlet connector 37, an air guide connector 35 and an air outlet connector 34 are provided on one side of the tank body 22. The air inlet connector 37 is located near the top of the tank body 22 and communicates with the inner cavity of the tank body 22. The air outlet connector 34 is located near the bottom of the tank body 22 and communicates with the inner cavity of the tank body 22. The air guide connector 35 is communicated with the heat preservation cavity 41. The gas circulation device 7 includes a mounting shell 28, a pressure transmission member 31, a piston cylinder 48, a piston 43, a connecting rod 47, a driving disc 46 and a driving motor 45. The pressure transmission member 31 includes a piston cylinder 48, a piston 43, a connecting rod 47, a driving disc 46 and a driving motor 45. The pressure transmitting member 31 is arranged in the mounting shell 28, one side of the pressure transmitting member 31 is connected to the main pipe 27, and the other side of the pressure transmitting member 31 is connected to the air supply pipe 29; the main pipe 27 is connected to the air inlet pipe 26, the air guide pipe 36 and the air outlet pipe 33, the air inlet pipe 26 is connected to the air inlet connector 37, the air guide pipe 36 is connected to the air guide connector 35, and the air outlet pipe 33 is connected to the air outlet connector 34; the air inlet pipe 26 is provided with a first one-way valve 25, the air outlet pipe 33 is provided with a second one-way valve 32, and the air supply pipe 29 is provided with a stop valve 30;
[0233] like Figure 4 As shown, the piston cylinder 48 is connected to the pressure transmission member 31 and is located between the main pipe 27 and the air supply pipe 29, and the piston 43 is movably and sealedly connected in the piston cylinder 48; the driving disk 46 is rotatably connected to the mounting shell 28, the top of the connecting rod 47 is hinged to the piston 43, and the bottom of the connecting rod 47 is hinged to one side of the driving disk 46; the driving motor 45 is arranged in the mounting shell 28, and the driving motor 45 is connected to the driving disk 46 and is used to drive the driving disk 46 to rotate.
[0234] Among them, the first one-way valve 25 is used to allow the gas in the tank body 22 to enter the main pipe 27, and the second one-way valve 32 is used to allow the gas in the main pipe 27 to enter the tank body 22. In actual use, the stop valve 30 is first opened to pass an inert gas, such as argon, through the air supply pipe 29. The argon enters the main pipe 27 after passing through the pressure transmission member 31, and then a part of the argon enters the heat preservation chamber 41 through the air guide pipe 36 and the air guide connector 35. Another part of the argon enters the tank body 22 through the air outlet pipe 33 and the air outlet connector 34. Then stop delivering argon and close the stop valve 30. Turn on the drive motor 45, and the drive motor 45 drives the drive disc 46 to rotate through the belt 44. The piston 43, the connecting rod 47 and the drive disc 46 form a crank connecting rod 47 mechanism. When the drive disc 46 rotates, the drive disc 46 can drive the piston 43 to move up and down in the piston cylinder 48 through the connecting rod 47. When the piston 43 moves downward, the pressure in the pressure transmission part 31 decreases, and the gas in the tank body 22 enters the main pipe 27 and the pressure transmission part 31 through the air inlet connector 37 and the air inlet pipe 26. The gas in the heat preservation chamber 41 enters the main pipe 27 and the pressure transmission part 31 through the air guide connector 35 and the air guide pipe 36. Since the temperature of the gas in the tank body 22 is relatively high, the temperature of the mixed gas will be higher than the temperature of the gas in the heat preservation chamber 41. Subsequently, the piston 43 moves upward, the pressure in the pressure transmission part 31 increases, and part of the gas in the pressure transmission part 31 and the main pipe 27 enters the tank body 22 through the air outlet pipe 33 and the air outlet connector 34. The gas entering the tank body 22 will cause the raw material solution in the tank body 22 to surge, thereby enhancing the stirring effect and facilitating the reaction of the raw materials. Another part of the gas in the pressure transmission part 31 and the main pipe 27 enters the heat preservation chamber 41 through the air guide pipe 36 and the air guide connector 35. As mentioned above, since the temperature of the mixed gas is higher than the gas temperature in the heat preservation chamber 41, the temperature in the heat preservation chamber 41 is improved, thereby improving the heat preservation effect, reducing energy loss, and realizing heat recovery. After the raw material reaction in the tank body 22 is completed, it can be vented by opening the tank cover, and it can also be vented by opening the stop valve 30. In this process, the piston 43 can also be driven to move by the driving motor 45, the driving disk 46 and the connecting rod 47. In the process of the piston 43 constantly going up and down, the air pressure in the pressure transmission part 31 and the main pipe 27 will constantly change. Since the stop valve 30 is open at this time, therefore, when the piston 43 is down, part of the fresh cold air from the outside will enter the pressure transmission part 31 and the main pipe 27 and reduce the temperature of the mixed gas in the pressure transmission part 31 and the main pipe 27. Then, during the upward movement of the piston 43, the mixed gas after cooling will enter the tank body 22 and the heat preservation chamber 41 respectively or be discharged from the air supply pipe 29. Under repeated operation, the temperature in the tank body 22 and the temperature in the heat preservation chamber 41 can be quickly reduced.At the same time, since the gas entering the tank body 22 is in full contact with the reactants in the tank body 22, the heat of the reactants can be taken away to a greater extent, thereby achieving rapid cooling of the reactants. This design can achieve heat preservation of the reactants in the tank body 22 during the reaction, and can achieve rapid cooling of the reactants after the reaction is completed.
[0235] In the description of the present invention, it is necessary to understand that the terms "coaxial", "bottom", "one end", "top", "middle", "the other end", "upper", "one side", "top", "inside", "front", "center", "both ends" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0236] In the present invention, unless otherwise clearly stipulated and limited, the terms such as "installation", "setting", "connection", "fixation" and "screw-on" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium; it can be the internal connection of two elements or the interaction relationship between two elements. Unless otherwise clearly defined, ordinary technicians in this field can understand the specific meanings of the above terms in the present invention according to the specific circumstances.
[0237] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a pigment paste thickening carrier resin, characterized in that: The following steps are involved: S1: adding the reaction raw materials of dibasic acid or / and dibasic acid anhydride and deionized water into a reactor (1) in a molar ratio of 1:1.1 to 1.3; raising the temperature in the reactor (1) to 110° C. to 140° C. to allow the reaction raw materials to undergo a hydrolysis reaction for 1 to 2 hours; S2: controlling the temperature in the reactor (1) to be between 120°C and 180°C; adding 0.3 to 0.5 mol of dicyclopentadiene dropwise into the reactor (1) within 2 to 3 hours to carry out a hydrogen ion shift addition reaction; after the addition is complete, reacting for another 2 to 4 hours; S3: Control the temperature in the reactor (1) at 120°C to 180°C, add 0.6 to 0.8 mol of diol into the reactor (1); let the total mass of the material in the reactor (1) be M, add 0.0005M to 0.003M of catalyst and 0.0002M to 0.0006M of inhibitor into the reactor (1); gradually raise the temperature of the reactor (1) to 190°C to 215°C to carry out polycondensation reaction for 2 to 4 hours; S4: vacuum dehydrating the product obtained after the polycondensation reaction for 2 to 4 hours to obtain a pigment paste carrier resin.
2. The method for preparing a pigment paste thickening carrier resin according to claim 1, characterized in that: The dibasic acid is fumaric acid, and the dibasic acid anhydride is maleic anhydride.
3. The method for preparing a pigment paste thickening carrier resin according to claim 1, characterized in that: The diol is at least one of 1,2-propylene glycol, isobutylene glycol, isoprene glycol and dipropylene glycol.
4. The method for preparing a pigment paste thickening carrier resin according to claim 1, characterized in that: The catalyst is at least one of sodium dodecylbenzene sulfonate, sodium p-toluene sulfonate and dibutyltin oxide.
5. The method for preparing a pigment paste thickening carrier resin according to claim 1, characterized in that: The polymerization inhibitor is at least one of hydroquinone, p-benzoquinone and 2,6-di-tert-butyl-p-methylphenol.
6. The method for preparing a pigment paste thickening carrier resin according to claim 1, characterized in that: In step S2, 0.4 mol of dicyclopentadiene is added dropwise into the reactor (1) in steps within 2.5 hours.
7. The method for preparing a pigment paste thickening carrier resin according to claim 1, characterized in that: The reactor (1) comprises a tank body (22) and a tank cover (9); a temperature transmitter (20) is arranged on the tank body (22); a discharge port (8) is arranged at the bottom of the tank body (22); a resistance wire is arranged in the bottom of the tank body (22); the tank cover (9) is arranged on the top of the tank body (22); an exhaust port (13), a material discharge port (21), a water supply port (19) and a liquid dripping port (18) are arranged on the tank cover (9); The tank cover (9) is also provided with a mounting seat (15), and a stirring motor (16) and a stirring shaft (38) are provided on the mounting seat (15), wherein the stirring shaft (38) is rotatably connected to the mounting seat (15) and the bottom of the stirring shaft (38) extends into the tank body (22), a stirring blade (39) is provided at the bottom of the stirring shaft (38), and the top of the stirring shaft (38) is connected to the stirring motor (16); A feeding device (4) is arranged outside the tank body (22), and the feeding device (4) is connected to the feeding port (21); a heat-insulating shell (40) is arranged on one side of the tank body (22) close to the bottom, and a heat-insulating chamber (41) is formed between the heat-insulating shell (40) and the tank body (22); a gas circulation device (7) is also arranged outside the tank body (22), and the gas circulation device (7) is used to introduce gas into the tank body (22) or the heat-insulating chamber (41) and circulate the gas.
8. The method for preparing a pigment paste thickening carrier resin according to claim 7, characterized in that: A workbench (3) is also provided outside the reactor (1), a ladder (5) is provided on one side of the workbench (3), a guardrail (2) is provided on the periphery of the top of the workbench (3), and a material stacking area (6) is provided on one side of the top of the workbench (3); a loading device (4) is provided on the workbench (3).
9. The method for preparing a pigment paste thickening carrier resin according to claim 8, characterized in that: The feeding device (4) comprises a feeding frame (11), a filter screen (12), a feeding barrel (14), a conveying roller, a conveying blade (10) and a feeding motor (17); wherein the feeding frame (11) is arranged on a workbench (3), and the interior of the feeding frame (11) has an inner cavity with an inverted triangle structure; one end of the feeding barrel (14) is connected to the bottom of the feeding frame (11) and communicates with the inner cavity of the feeding frame (11), and the other end of the feeding barrel (14) extends to a blanking port (21), and the feeding barrel (14) has an opening facing the blanking port (21); the conveying roller is rotatably connected in the feeding barrel (14), and the feeding motor (17) is connected to one side of the feeding barrel (14) and connected to the conveying roller; the conveying blade (10) is fixedly connected to the outer side of the conveying roller, and the conveying blade (10) is in a spiral structure on the outer side of the conveying roller.
10. The method for preparing a pigment paste thickening carrier resin according to claim 7, characterized in that: An air inlet connector (37), an air guide connector (35) and an air outlet connector (34) are arranged on one side of the tank body (22); the air inlet connector (37) is located near the top of the tank body (22) and is in communication with the inner cavity of the tank body (22); the air outlet connector (34) is located near the bottom of the tank body (22) and is in communication with the inner cavity of the tank body (22); the air guide connector (35) is in communication with the heat preservation cavity (41); the gas circulation device (7) comprises a mounting shell (28), a pressure transmission member (31), a piston cylinder (48), a piston (43), a connecting rod (47), a driving disc (46) and a driving motor (45); the pressure transmission member (31 ) is arranged in the mounting shell (28), one side of the pressure transmission member (31) is connected to the main pipe (27), and the other side of the pressure transmission member (31) is connected to the air supply pipe (29); the main pipe (27) is connected to an air inlet pipe (26), an air guide pipe (36) and an air outlet pipe (33); the air inlet pipe (26) is connected to an air inlet connector (37), the air guide pipe (36) is connected to an air guide connector (35), and the air outlet pipe (33) is connected to an air outlet connector (34); the air inlet pipe (26) is provided with a first one-way valve (25), the air outlet pipe (33) is provided with a second one-way valve (32), and the air supply pipe (29) is provided with a stop valve (30); The piston cylinder (48) is connected to the pressure transmission member (31) and is located between the main pipe (27) and the air supply pipe (29); the piston (43) is movably sealed and connected in the piston cylinder (48); the driving disk (46) is rotatably connected to the mounting shell (28); the top of the connecting rod (47) is hinged to the piston (43); and the bottom of the connecting rod (47) is hinged to one side of the driving disk (46); the driving motor (45) is arranged in the mounting shell (28); the driving motor (45) is connected to the driving disk (46) and is used to drive the driving disk (46) to rotate.
Citation Information
Patent Citations
Method for preparing thickenable dicyclopentadiene unsaturated polyester resin
CN101230131A
Automatic raw material dropping device
CN213160694U