Polyamide copolymer with narrow molecular weight distribution and preparation method thereof
By controlling the reaction between fat chain diamine and fat chain diacid, the polymerization uniformity is ensured, and the problems of wide molecular weight distribution and unstable melting point of polyamide copolymer are solved, and the molecular weight distribution and physical properties of polyamide copolymer are achieved. Supports its industrial applications.
Patent Information
- Application Number
- CN202411356151.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-27
AI Technical Summary
During the polymerization process, existing polyamide copolymers have uneven polymerization due to the difference in reactivity of alicyclic dibasic acid and fat chain dibasic acid, resulting in wide molecular weight distribution and unstable melting point, which hinders its industrial application.
By controlling the reaction of fat chain diamine and fat chain diacid, the activity of fat chain monomers is reduced, making it similar to the reaction activity of alicyclic monomers. Prepolymers are prepared and at high temperatures are used for specific molar ratios and reaction conditions. Polymerization is carried out to ensure the uniformity of the reaction and obtain a polyamide copolymer with a narrow molecular weight distribution.
The polyamide copolymer has achieved narrow molecular weight distribution, improved physical properties, and stable melting point, supporting its large-scale production and industrial applications.
Smart Images

Figure CN119019677A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyamide preparation, in particular to a polyamide copolymer with narrow molecular weight distribution and a preparation method thereof. Background Art
[0002] Since the melting point of alicyclic high temperature resistant polyamide can reach 300-350℃, it is difficult to apply it in industry, so it is often copolymerized with long carbon chain nylon to lower the melting point. The most common method is to copolymerize a fatty chain diamine with a fatty chain diacid and alicyclic diacid. However, alicyclic dibasic acid is often affected by steric hindrance, and its reaction activity is different from that of fatty chain dibasic acid during polymerization. Competition will occur during the polymerization process, resulting in uneven polymerization. Specifically, it may lead to that in the early stage of polymerization, a large amount of fatty chain diacids participate in the polymerization, and after a large amount of aliphatic chain diacids are consumed, alicyclic diacids begin to participate in the polymerization in large amounts. Microscopically, it manifests as a certain molecular chain containing a high proportion of PA106 segments, and another containing a high proportion of PA10C segments. Macroscopically, it manifests as a blend of two different polymers with a large difference in melting points. This leads to the fact that the prepared high-temperature resistant polyamide copolymers always have the phenomenon that the ratio of diacids in the molecular chain is inconsistent with the feed, the molecular weight distribution is wide, and the GPC spectrum has multiple peaks, which greatly affects the stability of the polymer, and thus makes the thermal and mechanical properties unstable, seriously hindering its large-scale production and industrial application. Summary of the invention
[0003] In order to solve the problems existing in the prior art, the present invention provides a polyamide copolymer with narrow molecular weight distribution and a preparation method thereof. The present invention firstly reduces the activity of the fatty chain monomer through the reaction of the fatty chain diamine monomer and the fatty chain diacid monomer, so that the activity of the fatty chain monomer is close to that of the alicyclic monomer, so that the subsequent reaction can be carried out uniformly, the molecular weight distribution is reduced, and the physical properties are improved.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0005] In one aspect, the present invention provides a method for preparing a polyamide copolymer having a narrow molecular weight distribution, comprising:
[0006] Step 1: according to actual production needs, weigh aliphatic chain diamine monomer, aliphatic chain diacid monomer, deionized water, and alicyclic binary substances; add the aliphatic chain diacid monomer and deionized water into a reaction kettle, continuously pass nitrogen, heat to 60-90° C., stir at a constant temperature to completely dissolve the aliphatic chain diacid monomer in water, then heat to 180-220° C., add the aliphatic chain diamine monomer, keep the temperature constant for 1-3 hours after the addition is completed, and obtain a prepolymer solid with the same end group as the alicyclic binary substance;
[0007] Wherein, the alicyclic dibasic substance is an alicyclic dibasic acid or an alicyclic diamine;
[0008] When the alicyclic binary substance is an alicyclic binary acid having 1 alicyclic ring, the molar ratio of the alicyclic diamine monomer to the alicyclic diacid monomer is 1:2-3, and the prepolymer solid is a dicarboxyl-terminated prepolymer;
[0009] Alternatively, in the alicyclic binary substance, the alicyclic diamine containing alicyclic diamine has 1 alicyclic ring, the molar ratio of the alicyclic diamine monomer to the alicyclic diacid monomer is 2-3:1, and the prepolymer solid is a diamino-terminated prepolymer;
[0010] Alternatively, in the alicyclic binary substance, the alicyclic binary acid has 2 alicyclic rings, the molar ratio of the alicyclic diamine monomer to the alicyclic diacid monomer is 2:3-6, and the prepolymer solid is a dicarboxyl-terminated prepolymer;
[0011] Alternatively, in the alicyclic binary substance, the alicyclic diamine has 2 alicyclic rings, the molar ratio of the alicyclic diamine monomer to the alicyclic diacid monomer is 3-6:2, and the prepolymer solid is a diamino-terminated prepolymer;
[0012] Step 2: weighing the prepolymer, composite additives and binary monomers prepared in step 1, wherein the amount of the binary monomers is the sum of the molar amounts of the prepolymer and the alicyclic binary substance;
[0013] The prepolymer, the alicyclic binary substance, the composite additive and the binary monomer are polymerized at 220-240° C. for 1-3 hours according to the proportion, and the pressure is vented to be lower than 0.5 MPa, and the temperature reaches 260-300° C. and polymerized for 1-5 hours;
[0014] Wherein, the alicyclic binary substance is an alicyclic dibasic acid, and the binary monomer is the same aliphatic chain diamine as in step 1;
[0015] Alternatively, when the alicyclic binary substance is an alicyclic diamine, the binary monomer is the same aliphatic chain diacid as in step 1;
[0016] Step 3: exhaust the gas, evacuate the mixture, continue polymerization at 280-320°C, break it up and dry it to obtain the final polymerization product. Preferably, the polymerization time in step 4 is 0.5-2 hours; or the polymerization time is 5-8 hours. If the polymerization time in this step is 5-8 hours, a product with higher randomness and narrower molecular weight distribution can be obtained by amide exchange reaction, but the product obtained by 0.5-2 hours polymerization time has excellent regularity and lower molecular weight distribution.
[0017] Furthermore, the fatty chain dibasic acid monomer is a dibasic acid with a carbon chain length of 3 to 18; the fatty chain diamine monomer is a diamine with a carbon chain length of 4 to 18;
[0018] The alicyclic dibasic acid is a hexacyclic dibasic acid substituted at the para-position or meta-position, preferably 1,4-cyclohexanedicarboxylic acid (1,4CHDA), 1,4-cyclohexanediacetic acid or 1,3-cyclohexanedicarboxylic acid (1,3CHDA); the alicyclic diamine is a hexacyclic diamine substituted at the para-position or meta-position, preferably 1,4-cyclohexanedimethylamine, 1,4-cyclohexanediethylamine (1,4CBMA), 1,3-cyclohexanedimethylamine, 4,4'-diaminodicyclohexylmethane (PACM), 3,3'-dimethyl-4,4-diaminodicyclohexylmethane (MACM) or 4,4'-diaminodicyclohexylpropane (PACP).
[0019] Further, the composite additive comprises an antioxidant, a stabilizer and a catalyst; the amount of the catalyst is 0.6-1wt‰ of the total mass of the fatty chain diamine monomer, the fatty chain diacid monomer, the alicyclic binary substance and the binary monomer, the antioxidant is 1-2wt‰ of the total mass of the fatty chain diamine monomer, the fatty chain diacid monomer, the alicyclic binary substance and the binary monomer, and the stabilizer is 0.6-1wt‰ of the total mass of the fatty chain diamine monomer, the fatty chain diacid monomer, the alicyclic binary substance and the binary monomer. Preferably, the catalyst is one or more of phosphoric acid, calcium hypophosphite, sodium hypophosphite, antimony trioxide, sodium antimonate, titanium tetrachloride, and tetraethyl titanate; the antioxidant is one or more of antioxidant 1098, antioxidant 1010, antioxidant B215, and antioxidant seed; the stabilizer is one or more of stabilizer H10, stabilizer 3322, stabilizer ANSEED, and stabilizer N392.
[0020] In the present invention, the molar ratio of acid to amine is the same. If the monomer used is volatile, such as pentamethylenediamine, it should be slightly excessive, with a ratio of 1:1.02 to 1:1.05.
[0021] On the other hand, the present invention also provides a polyamide copolymer prepared by the above method.
[0022] Assume that the alicyclic dibasic acid is A, the aliphatic chain dibasic acid is B, and the aliphatic chain diamine is C. The copolymer prepared this time has a ratio of cyclic acid to chain acid of 1:9. Further assume that 0.1 mol of cyclic acid and 0.9 mol of chain acid are used this time, then the ratios of each step are as follows:
[0023] S1: The prepared microblock is BCB, in which the total amount of B is set to 0.9 mol, and C is half of B, i.e., 0.45 mol. In order to ensure the formation of BCB, the B used can be excessive. For example, the molar amount of B used here is less than 1.35 mol, but since only 0.45 mol C is input, the BCB block finally prepared is also 0.45 mol, which can be regarded as a new diacid, and the structural formula is as follows:
[0024]
[0025] Wherein, m is 1, R1 is a C4-C18 alkyl group, and R2 is C3-C18;
[0026] S2: The diacid units in the system now have 0.45 mol BCB and 0.1 mol A, totaling 0.55 mol diacid, so 0.55 mol diamine monomer needs to be added. Considering that the diamine may volatilize, 1.02 to 1.05 times the diamine is usually added.
[0027] If the alicyclic diamine is copolymerized with a fatty chain diamine and a fatty chain diacid, the positions of the above-mentioned acid and amine can be switched.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The present invention firstly controls the amount of monomer addition through the reaction of aliphatic chain diamine monomers and aliphatic chain diacid monomers to obtain prepolymers with different repeating units, thereby reducing the reactivity of the aliphatic chain monomers to make them similar to the reactivity of alicyclic monomers, thereby facilitating a uniform reaction in the subsequent reaction process, reducing the molecular weight distribution and improving the physical properties.
[0030] The present invention determines the number of repeating units of the prepolymer according to the structure of the binary substance containing an alicyclic ring, and then ensures the structure of the generated prepolymer by making one of the aliphatic chain monomers excessive, thereby effectively preventing the problem of uneven reaction caused by different monomers. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The DSC graph of the copolymer prepared in Example 1;
[0032] Figure 2 is the TGA graph of the copolymer prepared in Example 1;
[0033] Figure 3 is the GPC chart of the copolymer prepared in Example 1;
[0034] Figure 4 is the GPC chart of the copolymer prepared in Example 2;
[0035] Figure 5 is the GPC chart of the copolymer prepared in Example 3;
[0036] Figure 6 is the GPC chart of the copolymer prepared in Example 5;
[0037] Figure 7 This is the GPC chart of the copolymer prepared in Example 6. DETAILED DESCRIPTION
[0038] In order to make the technical problems to be solved, technical solutions and advantages of the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.
[0039] In the present invention, the materials and reagents used can be obtained from commercial sources unless otherwise specified.
[0040] The present invention provides a polyamide copolymer with narrow molecular weight distribution and a preparation method thereof, and specific embodiments are as follows.
[0041] Example 1 (10C-5:5)
[0042] A method for preparing a polyamide copolymer with a narrow molecular weight distribution comprises:
[0043] S1: Weigh 86 parts by weight of decanediamine, 219 parts by weight of adipic acid and 122 parts by weight of deionized water, add the adipic acid and deionized water into a glass reactor, continue to flow nitrogen, heat to 90°C, stir at constant temperature for 20 minutes to completely dissolve the adipic acid in the water, heat to 180°C, slowly add decanediamine, keep constant temperature for 2 hours after the addition is completed, discharge the material to obtain a solid prepolymer, then wash it with water and ethanol for multiple times, and dry it in an oven at 60°C;
[0044] S2: Weigh 172 parts by weight of 1,4-cyclohexanedicarboxylic acid, 258 parts by weight of decanediamine, 0.66 parts by weight of calcium hypophosphite, 0.66 parts by weight of stabilizer 3322, and 1.32 parts by weight of antioxidant seed, and put them into a high-temperature reactor together with the prepolymer, turn on the condensation water, start stirring, and polymerize at 230°C for 2h. At this time, slowly release the gas, adjust the rate of temperature increase and exhaust by detecting the pressure change and the mass of the discharged water, and set the program temperature to 300°C. When the pressure drops below 0.5MPa and the temperature reaches 300°C;
[0045] S3: exhaust the gas and start vacuuming. During this process, the temperature continues to increase to 320°C. The polymerization is continued for 5 hours and the material is discharged. After crushing, it is dried in a vacuum oven for 12 hours to obtain a uniformly polymerized copolymer polyamide product.
[0046] Depend on Figure 1-3 It can be seen that the melting point of the copolymer prepared in Example 1 is 289.9°C, the starting decomposition temperature is 375.8°C, the maximum thermal decomposition temperature is 457.17°C, the molecular weight distribution is only 1.86, and the relative molecular weight is 16206. The molecular weight distribution of the copolymer prepared in this example is narrow and has only one melting point, which proves that the continuous reading distribution of the copolymer prepared by the present invention is more uniform.
[0047] Example 2 (6C-1:9)
[0048] A method for preparing a polyamide copolymer with a narrow molecular weight distribution comprises:
[0049] S1: Weigh 54 parts by weight of hexamethylenediamine, 131 parts by weight of adipic acid and 74 parts by weight of deionized water, add adipic acid and deionized water into a glass reactor, continue to flow nitrogen, heat to 90°C, stir at constant temperature for 10 minutes to completely dissolve adipic acid in water, heat to 180°C, slowly add hexamethylenediamine, keep constant temperature for 1.5 hours after the addition is completed, discharge to obtain a solid prepolymer, then wash with water and ethanol for multiple times, and dry in an oven at 60°C;
[0050] S2: Weigh 17 parts by weight of 1,4-cyclohexanedicarboxylic acid, 64 parts by weight of hexamethylenediamine, 0.22 parts by weight of calcium hypophosphite, 0.22 parts by weight of stabilizer 3322, and 0.44 parts by weight of antioxidant 1010, and put them into a high-temperature reactor together with the prepolymer. Turn on the condensation water, start stirring, and polymerize at 220°C for 2 hours. At this time, start to slowly release the gas, and adjust the rate of heating and exhaust by detecting the pressure change and the mass of the discharged water. At the same time, set the program temperature to 260°C. Wait until the pressure drops below 0.5MPa and the temperature reaches 260°C.
[0051] S3: exhaust the gas and start vacuuming. During this process, the temperature continues to increase to 280°C. The polymerization is continued for 5 hours and the material is discharged. After crushing, it is dried in a vacuum oven for 12 hours to obtain a uniformly polymerized copolymer polyamide product.
[0052] Depend on Figure 4 It can be seen that the weight distribution of the copolymer prepared in this example is 1.98.
[0053] Example 3 (PA46 / 41,4-cyclohexanediacetic acid-8:2)
[0054] A method for preparing a polyamide copolymer with a narrow molecular weight distribution comprises:
[0055] S1: Weigh 36 parts by weight of butanediamine, 146 parts by weight of adipic acid and 121 parts by weight of deionized water, add the adipic acid and deionized water into a glass reactor, continue to flow nitrogen, heat to 90°C, stir at constant temperature for 10 minutes to completely dissolve the adipic acid in the water, then heat to 180°C, slowly add butanediamine, keep constant temperature for 1.5 hours after the addition is completed, discharge the material to obtain a solid prepolymer, then wash it with water and ethanol for multiple times, and dry it in an oven at 60°C;
[0056] S2: Weigh 28 parts by weight of 1,4-cyclohexanediacetic acid, 53 parts by weight of hexamethylenediamine, 0.22 parts by weight of calcium hypophosphite, 0.22 parts by weight of stabilizer 3322, and 0.44 parts by weight of antioxidant 1010, and put them into a high-temperature reactor together with the prepolymer. Turn on the condensation water, start stirring, and polymerize at 230°C for 2 hours. At this time, start to slowly release the gas, and adjust the rate of heating and exhaust by detecting the pressure change and the mass of the discharged water. At the same time, set the program temperature to 300°C. Wait until the pressure drops below 0.5MPa and the temperature reaches 280°C.
[0057] S3: exhaust the gas and start vacuuming. During this process, the temperature continues to increase to 330°C. The polymerization is continued for 1 hour and the material is discharged. After crushing, it is dried in a vacuum oven for 12 hours to obtain a uniformly polymerized copolymer polyamide product.
[0058] Depend on Figure 5 It can be seen that the weight distribution of the copolymer prepared in this example is 2.61.
[0059] Example 4: (PA101, 3CHDA / 1010-6:4)
[0060] A method for preparing a polyamide copolymer with a narrow molecular weight distribution comprises:
[0061] The experimental steps are the same as in Example 1, and the proportion of each reactant added is as follows:
[0062] S1: 81 parts by weight of sebacic acid, 35 parts by weight of decanediamine, and 104 parts by weight of deionized water;
[0063] S2: S1 prepolymer, 103 parts by weight of 1,3-cyclohexanedicarboxylic acid, 138 parts by weight of decanediamine, 0.34 parts by weight of calcium hypophosphite, 0.34 parts by weight of stabilizer 3322, and 0.68 parts by weight of antioxidant 1010.
[0064] Example 5 (PA1,4-cyclohexanediamine 10 / 610-8:2)
[0065] A method for preparing a polyamide copolymer with a narrow molecular weight distribution comprises:
[0066] S1: Weigh 21 parts by weight of sebacic acid, 35 parts by weight of hexamethylenediamine and 37 parts by weight of deionized water, add sebacic acid and deionized water into a glass reactor, continue to flow nitrogen, heat to 90°C, stir at constant temperature for 10 minutes to completely dissolve the adipic acid in the water, then heat to 180°C, slowly add hexamethylenediamine, keep constant temperature for 1 hour after the addition is completed, discharge the material to obtain a solid prepolymer, then wash it with water and ethanol for multiple times, and dry it in an oven at 60°C;
[0067] S2: Weigh 90 parts by weight of 1,4-cyclohexanediamine, 182 parts by weight of dodecanedioic acid, 0.31 parts by weight of calcium hypophosphite, 0.31 parts by weight of stabilizer 3322, and 0.62 parts by weight of antioxidant 1010, and put them into a high-temperature reactor together with the prepolymer. Turn on the condensation water, start stirring, and polymerize at 220°C for 2 hours. At this time, start to slowly release the gas, and adjust the rate of heating and exhaust by detecting the pressure change and the mass of the discharged water. At the same time, set the program temperature to 280°C. Wait until the pressure drops below 0.5MPa and the temperature reaches 280°C.
[0068] S3: exhaust the gas, start vacuuming, continue to increase the temperature to 320°C, polymerize for 1 hour, discharge the material, crush it and dry it in a vacuum oven for 12 hours to obtain a uniformly polymerized copolymer polyamide product.
[0069] Depend on Figure 6 It can be seen that the weight distribution of the copolymer prepared in this example is 2.67.
[0070] Example 6: (PA1,3-cyclohexanedimethylamine 6 / 106-5:5)
[0071] A method for preparing a polyamide copolymer with a narrow molecular weight distribution comprises:
[0072] The experimental steps are the same as in Example 1, and the proportion of each reactant added is as follows:
[0073] S1: 36.5 parts by weight of adipic acid, 103 parts by weight of decanediamine, and 94 parts by weight of deionized water;
[0074] S2: S1 prepolymer, 71 parts by weight of 1,3-cyclohexanedimethylamine, 110 parts by weight of adipic acid, 0.29 parts by weight of calcium hypophosphite, 0.29 parts by weight of stabilizer 3322, and 0.58 parts by weight of antioxidant 1010.
[0075] Depend on Figure 7 It can be seen that the weight distribution of the copolymer prepared in this example is 2.52.
[0076] Example 7: (PA1, 4CBMA6 / 66-9: 1)
[0077] A method for preparing a polyamide copolymer with a narrow molecular weight distribution comprises:
[0078] The experimental steps are the same as in Example 5, and the proportion of each reactant added is as follows:
[0079] S1: 36.5 parts by weight of adipic acid, 8 parts by weight of hexamethylenediamine, and 29 parts by weight of deionized water;
[0080] S2: S1 prepolymer, 157 parts by weight of 1,4-cyclohexanediethylamine, 144 parts by weight of adipic acid, 0.33 parts by weight of calcium hypophosphite, 0.33 parts by weight of stabilizer 3322, and 0.66 parts by weight of antioxidant 1010.
[0081] Example 8 (PA612 / PACM12-2: 8)
[0082] A method for preparing a polyamide copolymer with a narrow molecular weight distribution comprises:
[0083] S1: Weigh 23 parts by weight of dodecanedioic acid, 35 parts by weight of hexamethylenediamine and 38 parts by weight of deionized water, add dodecanedioic acid and deionized water into a glass reactor, continue to flow nitrogen, heat to 90°C, stir at constant temperature for 10 minutes to completely dissolve the adipic acid in water, heat to 180°C, slowly add hexamethylenediamine, keep constant temperature for 1 hour after the addition is completed, discharge the material to obtain a solid prepolymer, then wash it with water and ethanol for multiple times, and dry it in an oven at 60°C;
[0084] S2: Weigh 168 parts by weight of PACM, 207 parts by weight of dodecanedioic acid, 0.28 parts by weight of calcium hypophosphite, 0.28 parts by weight of stabilizer 3322, and 0.56 parts by weight of antioxidant 1010, and put them into a high-temperature reactor together with the prepolymer. Turn on the condensation water, start stirring, and polymerize at 200°C for 2 hours. At this time, start to slowly release the gas, and adjust the rate of heating and exhaust by detecting the pressure change and the mass of the discharged water. At the same time, set the program temperature to 230°C. Wait until the pressure drops below 0.5 MPa and the temperature reaches 230°C.
[0085] S3: exhaust the gas, start vacuuming, continue polymerization for 3 hours, discharge the material, crush it and dry it in a vacuum oven for 12 hours to obtain a transparent copolymerized polyamide product with uniform polymerization.
[0086] Example 9: (PA MACM18 / 618-4:6)
[0087] A method for preparing a polyamide copolymer with a narrow molecular weight distribution comprises:
[0088] The experimental steps are the same as in Example 8, and the proportion of each reactant added is as follows:
[0089] S1: Weigh 126 parts by weight of octadecane dioic acid, 70 parts by weight of hexamethylenediamine and 130 parts by weight of deionized water;
[0090] S2: Weigh 84 parts by weight of MACM, 189 parts by weight of octadecane dioic acid, 0.47 parts by weight of calcium hypophosphite, 0.47 parts by weight of stabilizer 3322, and 0.93 parts by weight of antioxidant 1010.
[0091] Example 10: (PA PACP16 / 1016-3:7)
[0092] A method for preparing a polyamide copolymer with a narrow molecular weight distribution comprises:
[0093] The experimental steps are the same as in Example 8, and the proportion of each reactant added is as follows:
[0094] S1: Weigh 134 parts by weight of hexadecanedioic acid, 121 parts by weight of decanediamine and 103 parts by weight of deionized water.
[0095] S2: Weigh 43 parts by weight of PACP, 152 parts by weight of hexadecanedioic acid, 0.35 parts by weight of calcium hypophosphite, 0.35 parts by weight of stabilizer 3322, and 0.7 parts by weight of antioxidant 1010.
[0096] In order to further illustrate the beneficial effects of the present invention, the following comparative example was constructed.
[0097] Comparative Example 1 (10C-5:5)
[0098] A method for preparing a polyamide copolymer comprises:
[0099] S1: Weigh 172 parts by weight of decanediamine, 86 parts by weight of 1,4-cyclohexanedicarboxylic acid, 73 parts by weight of adipic acid, 220 parts by weight of deionized water and a composite additive consisting of 0.22 parts by weight of calcium hypophosphite, 0.22 parts by weight of stabilizer 3322, and 0.44 parts by weight of antioxidant seed, stir evenly and put into a high-temperature reactor, turn on the condensing water, turn on the heating, keep the temperature at 90°C for 60 minutes, then raise the temperature to 220°C and keep the temperature at 2 hours.
[0100] S2: Set the program to 300°C, slowly release the gas, and gradually increase the temperature. When the temperature reaches 300 degrees and the pressure drops below 0.5MPa, evacuate the gas, evacuate the vacuum, and continue the polymerization for 1 hour. Discharge the material, crush it, and dry it in a vacuum oven for 12 hours to obtain a conventionally polymerized copolymer polyamide product.
[0101] Comparative Example 2
[0102] A method for preparing a polyamide copolymer comprises:
[0103] S1: Weigh 173 parts by weight of hexamethylenediamine, 26 parts by weight of 1,4-cyclohexanedicarboxylic acid, 197 parts by weight of adipic acid, 264 parts by weight of deionized water and a composite additive consisting of 0.4 parts by weight of calcium hypophosphite, 0.4 parts by weight of stabilizer 3322 and 1.19 parts by weight of antioxidant 1010, stir well and put into a high-temperature reactor, turn on the condensing water, turn on the heating, keep the temperature at 90°C for 60 minutes, then raise the temperature to 220°C and keep the temperature at 4 hours.
[0104] S2: Set the program to 260°C, slowly release the gas, and gradually increase the temperature. When the temperature reaches 260°C and the pressure drops below 0.5MPa, evacuate the gas, apply vacuum, and continue polymerization for 2 hours. Discharge the material, crush it, and dry it in a vacuum oven for 12 hours to obtain a conventionally polymerized copolymer polyamide product.
[0105] Comparative Example 3
[0106] A method for preparing a polyamide copolymer comprises:
[0107] S1: Weigh 172 parts by weight of decanediamine, 219 parts by weight of adipic acid and 122 parts by weight of deionized water, add the adipic acid and deionized water into a glass reactor, continue to flow nitrogen, heat to 90°C, stir at constant temperature for 20 minutes to completely dissolve the adipic acid in the water, heat to 180°C, slowly add decanediamine, keep constant temperature for 2 hours after the addition is completed, and discharge the material to obtain a prepolymer.
[0108] S2: Weigh 258 parts by weight of 1,4-cyclohexanedicarboxylic acid, 344 parts by weight of decanediamine, 0.99 parts by weight of calcium hypophosphite, 0.99 parts by weight of stabilizer 3322, and 1.98 parts by weight of antioxidant seed, and put them into a high-temperature reactor together with the prepolymer, turn on the condensation water, start stirring, and polymerize at 230°C for 2h. At this time, slowly release the gas, adjust the rate of temperature increase and exhaust by detecting the pressure change and the quality of the discharged water, and set the program temperature to 300°C at the same time. When the pressure drops below 0.5MPa and the temperature reaches 300°C;
[0109] S3: exhaust the gas and start vacuuming. During this process, the temperature continues to increase to 320°C. The polymerization is continued for 5 hours and the material is discharged. After crushing, it is dried in a vacuum oven for 12 hours to obtain a uniformly polymerized copolymer polyamide product.
[0110] Comparative Example 4
[0111] A method for preparing a polyamide copolymer comprises:
[0112] S1: Weigh 155 parts by weight of decanediamine, 175 parts by weight of adipic acid and 122 parts by weight of deionized water, add the adipic acid and deionized water into a glass reactor, continue to flow nitrogen, heat to 90°C, stir at constant temperature for 20 minutes to completely dissolve the adipic acid in the water, heat to 180°C, slowly add decanediamine, keep constant temperature for 2 hours after the addition is completed, and discharge the material to obtain a prepolymer.
[0113] S2: Weigh 206 parts by weight of 1,4-cyclohexanedicarboxylic acid, 258 parts by weight of decanediamine, 0.79 parts by weight of calcium hypophosphite, 0.79 parts by weight of stabilizer 3322, and 1.58 parts by weight of antioxidant seed, and put them into a high-temperature reactor together with the prepolymer, turn on the condensation water, start stirring, and polymerize at 230°C for 2h. At this time, slowly release the gas, adjust the rate of temperature increase and exhaust by detecting the pressure change and the quality of the discharged water, and set the program temperature to 300°C. When the pressure drops below 0.5MPa and the temperature reaches 300°C;
[0114] S3: exhaust the gas and start vacuuming. During this process, the temperature continues to increase to 320°C. The polymerization is continued for 5 hours and the material is discharged. After crushing, it is dried in a vacuum oven for 12 hours to obtain a uniformly polymerized copolymer polyamide product.
[0115] Comparative Example 5
[0116] A method for preparing a polyamide copolymer with a narrow molecular weight distribution comprises:
[0117] S1: Weigh 172 parts by weight of 1,4-cyclohexanedicarboxylic acid, 258 parts by weight of decanediamine and 122 parts by weight of deionized water, add adipic acid and deionized water into a glass reactor, continue to flow nitrogen, raise the temperature to 90°C, and stir at this constant temperature for 20 minutes to completely dissolve the adipic acid in the water. Then raise the temperature to 180°C, slowly add decanediamine, keep the temperature constant for 2 hours after the addition is completed, and discharge the material to obtain a prepolymer.
[0118] S2: Weigh 86 parts by weight of decanediamine, 219 parts by weight of adipic acid, 0.66 parts by weight of calcium hypophosphite, 0.66 parts by weight of stabilizer 3322, and 1.32 parts by weight of antioxidant seed, and put them into a high-temperature reactor together with the prepolymer. Turn on the condensation water, start stirring, and polymerize at 230°C for 2 hours. At this time, start to slowly release the gas, adjust the rate of temperature increase and exhaust by detecting the pressure change and the quality of the discharged water, and set the program temperature to 300°C. When the pressure drops below 0.5MPa and the temperature reaches 300°C;
[0119] S3: exhaust the gas and start vacuuming. During this process, the temperature continues to increase to 320°C. The polymerization is continued for 5 hours and the material is discharged. After crushing, it is dried in a vacuum oven for 12 hours to obtain a uniformly polymerized copolymer polyamide product.
[0120] The copolymers prepared in the above Examples 1-10 and Comparative Examples 1-5 were tested for their properties. The testing method is as follows. The test results are shown in Table 1-2.
[0121] Relative viscosity test: Using m-cresol as the standard solvent, dissolve 0.25 g of sample in 25 ml of m-cresol, shake well, and measure the relative viscosity using an Ubbelohde viscometer.
[0122] Gel permeation chromatography (GPC): Dissolve 3-5 mg of sample in 1-2 ml of hexafluoroisopropanol and shake thoroughly before testing. The mobile phase is hexafluoroisopropanol, the flow rate is 1 ml / min, and the standard is polymethyl methacrylate (PMMA);
[0123] Thermogravimetric analysis (TG): weigh more than 10 mg of sample, test temperature is 25 ~ 600 ℃, heating rate is 10 ℃ / min, nitrogen protection, obtain the sample mass change curve during the heating process.
[0124] Differential Scanning Calorimetry (DSC): Use less than 10 mg of sample to prepare the sample in an aluminum crucible. The test temperature program is: 30℃~350 / 400℃, heating rate 20℃ / min, 350 / 400℃~30℃, cooling rate 20℃ / min, after eliminating the thermal history, heat up again to 30℃~350 / 400℃, heating rate 10℃ / min, test the melting point and crystallization temperature of the product.
[0125] Table 1
[0126]
[0127] As can be seen from Table 1, in Examples 1-4, the alicyclic dibasic acid containing an alicyclic binary substance with an alicyclic number of 1, the molar ratio of the alicyclic diamine monomer to the alicyclic diacid monomer is regulated to obtain a prepolymer with a dicarboxyl-terminated repeating unit of 1, and then the prepolymer and the alicyclic dibasic acid containing an alicyclic dibasic acid react with the alicyclic diamine at the same time. Since the prepolymer and the alicyclic dibasic acid containing an alicyclic diamine have equivalent reaction activities with the alicyclic diamine, a copolymer with uniform segment distribution can be obtained, and the molecular weight distribution is 1.86-2.35, and the molecular weight distribution is relatively narrow, which also proves that the prepared copolymer is relatively uniform; in Examples 5-7, the alicyclic diamine containing an alicyclic binary substance with an alicyclic number of 1, the molecular weight distribution of the obtained copolymer is also relatively narrow; in Examples 8-10, the alicyclic diamine containing an alicyclic binary substance with an alicyclic number of 2, the molecular weight distribution of the obtained copolymer is 2.18-2.39.
[0128] The copolymers prepared in Examples 1-7 of the present invention have only one melting point, which proves that the prepared copolymer segments are relatively uniform and the tensile strength of the obtained copolymers is also relatively high. In Examples 8-10, because the alicyclic binary substance contains two alicyclic rings, the steric hindrance is very large, which will hinder the crystallization of the system, so there is no melting point, but the prepared copolymers have a high transmittance (Example 8 has a transmittance of 92%, Example 9 has a transmittance of 90%, and Example 10 has a transmittance of 75%), and also have good mechanical properties.
[0129] Table 2
[0130]
[0131] As can be seen from Table 2, in Comparative Examples 1 and 2, all monomers are added to the reactor at one time, and the obtained copolymer has two melting points, the molecular weight distribution reaches 10-12.47, and the tensile strength of the prepared copolymer is also low; in Comparative Examples 3-4, the substances are the same as in Example 1, but the molar ratio of decanediamine and adipic acid is adjusted so that the repeating unit of the prepared prepolymer is 2 or 3, the molecular weight distribution of the obtained copolymer is also wider, and the melting point of the copolymer has two or a melting point with a wide tolerance, and the mechanical properties are also greatly reduced; this is because the reactivity of the prepolymer with different repeating units is different from that of 1,4-cyclohexanedicarboxylic acid. During the reaction of both with decanediamine at the same time, some segments are unevenly distributed due to the different reactivity, resulting in a wider molecular weight distribution of the prepared copolymer and reduced mechanical properties.
[0132] In Comparative Example 5, 1,4-cyclohexanedicarboxylic acid is first reacted with decanediamine to obtain a prepolymer, which is then mixed with adipic acid and reacted with decanediamine at the same time. Due to the serious mismatch between the reaction activity of the prepolymer and the reaction activity of adipic acid, the prepared copolymer has a wide molecular weight distribution and poor mechanical properties.
[0133] In summary, the present invention regulates the molar amounts of the fatty chain diamine monomer and the fatty chain diacid monomer according to the amount of the fatty ring in the alicyclic binary substance, so that the reaction activity of the prepared prepolymer is equivalent to that of the alicyclic binary substance, which facilitates the subsequent reaction process, enables the reaction to proceed uniformly, reduces the molecular weight distribution, and improves the physical properties.
[0134] The above is a preferred embodiment of the present invention. For ordinary technicians in this technical field, making several improvements and modifications without departing from the principles of the present invention should also be regarded as within the protection scope of the present invention.
Claims
1. A method for preparing a polyamide copolymer with a narrow molecular weight distribution, characterized in that: include: Step 1: weighing a fatty chain diamine monomer, a fatty chain diacid monomer, deionized water, and alicyclic binary substances; adding the fatty chain diacid monomer and deionized water into a reaction kettle, continuously passing nitrogen, heating to 60-90° C., stirring at a constant temperature to completely dissolve the fatty chain diacid monomer in the water, then heating to 180-220° C., adding the fatty chain diamine monomer, maintaining the temperature for 1-3 hours after the addition is completed, and discharging to obtain a prepolymer solid with the same end group as the alicyclic binary substance; Wherein, the alicyclic dibasic substance is an alicyclic dibasic acid or an alicyclic diamine; When the alicyclic binary substance is an alicyclic binary acid having 1 alicyclic ring, the molar ratio of the alicyclic diamine monomer to the alicyclic diacid monomer is 1:2-3, and the prepolymer solid is a dicarboxyl-terminated prepolymer; Alternatively, the alicyclic diamine containing alicyclic rings having 1 alicyclic ring number is used in the alicyclic diamine containing alicyclic rings, the molar ratio of the aliphatic chain diamine monomer to the aliphatic chain diacid monomer is 2-3:1, and the prepolymer solid is a diamino-terminated prepolymer; Alternatively, in the alicyclic binary substance, the alicyclic binary acid has 2 alicyclic rings, the molar ratio of the alicyclic diamine monomer to the alicyclic diacid monomer is 2:3-6, and the prepolymer solid is a dicarboxyl-terminated prepolymer; Alternatively, in the alicyclic binary substance, the alicyclic diamine has 2 alicyclic rings, the molar ratio of the alicyclic diamine monomer to the alicyclic diacid monomer is 3-6:2, and the prepolymer solid is a diamino-terminated prepolymer; Step 2: weighing the prepolymer, composite additive and binary monomer prepared in step 1, wherein the amount of the binary monomer is the sum of the molar amounts of the prepolymer and the alicyclic binary substance; polymerizing the prepolymer, the alicyclic binary substance, the composite additive and the binary monomer according to a proportion at 220-240° C. for 1-3 hours, exhausting the gas until the pressure is lower than 0.5 MPa, and polymerizing the mixture at a temperature of 260-300° C. for 1-5 hours; Wherein, the alicyclic binary substance is an alicyclic dibasic acid, and the binary monomer is the same aliphatic chain diamine as in step 1; Alternatively, when the alicyclic binary substance is an alicyclic diamine, the binary monomer is the same aliphatic chain diacid as in step 1; Step 3: exhaust the gas, evacuate the mixture, continue polymerization at 280-320°C, break it up and dry it to obtain the final polymerization product.
2. The preparation method according to claim 1, characterized in that: The polymerization time in step 3 is 0.5 to 2 hours; or the polymerization time is 5 to 8 hours.
3. The preparation method according to claim 2, characterized in that: In the step 1, the fatty chain dibasic acid monomer is a dibasic acid with a carbon chain length of 3 to 18; the fatty chain diamine monomer is a diamine with a carbon chain length of 4 to 18; The alicyclic dibasic acid is a para- or meta-substituted hexacyclic dibasic acid; the alicyclic diamine is a para- or meta-substituted hexacyclic diamine.
4. The preparation method according to claim 3, characterized in that: The alicyclic dibasic acid is 1,4-cyclohexanedicarboxylic acid (1,4CHDA), 1,4-cyclohexanediacetic acid or 1,3-cyclohexanedicarboxylic acid (1,3CHDA); The alicyclic diamine is 1,4-cyclohexanedimethylamine, 1,4-cyclohexanediethylamine (1,4CBMA), 1,3-cyclohexanedimethylamine, 4,4'-diaminodicyclohexylmethane (PACM), 3,3'-dimethyl-4,4-diaminodicyclohexylmethane (MACM) or 4,4'-diaminodicyclohexylpropane (PACP).
5. The preparation method according to claim 2, characterized in that: In the step 1, the composite additive comprises an antioxidant, a stabilizer and a catalyst; The amount of the catalyst is 0.6-1wt‰ of the total mass of the fatty chain diamine monomer, the fatty chain diacid monomer, the alicyclic binary substance and the binary monomer; the amount of the antioxidant is 1-2wt‰ of the total mass of the fatty chain diamine monomer, the fatty chain diacid monomer, the alicyclic binary substance and the binary monomer; and the amount of the stabilizer is 0.6-1wt‰ of the total mass of the fatty chain diamine monomer, the fatty chain diacid monomer, the alicyclic binary substance and the binary monomer.
6. The preparation method according to claim 5, characterized in that: The catalyst is one or more of phosphoric acid, calcium hypophosphite, sodium hypophosphite, antimony trioxide, sodium antimonate, titanium tetrachloride, and tetraethyl titanate.
7. The preparation method according to claim 5, characterized in that: The antioxidant is one or more of antioxidant 1098, antioxidant 1010, antioxidant B215, and antioxidant seed.
8. The preparation method according to claim 5, characterized in that: The stabilizer is one or more of stabilizer H10, stabilizer 3322, stabilizer ANSEED, and stabilizer N392.
9. The polyamide copolymer prepared by the method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Segmented copolymer containing transparent polyamide and polyether and synthetic method of segmented copolymer
CN105348521A
High-temperature-resistant low-water-absorption copolymerized nylon and preparation method thereof
CN108003341A
Polyamide copolymer with regular chain segment structure and preparation method thereof
CN116836383A
Polyamide, preparation method therefor, and use thereof
WO2023122877A1