Low-dielectric polyimide film and preparation method thereof

By adjusting the raw material ratio and introducing materials such as adamantane-containing diamines of specific structures, the dielectric constant of the polyimide film is reduced, and the problem of high dielectric constant of traditional films is solved, and high frequency, high speed and high density are achieved Applications in electronic devices.

CN119019686APending Publication Date: 2024-11-26HEFEI SINOPISE MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411293173.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Traditional polyimide films have a high dielectric constant, which limits their application in high-frequency, high-speed, and high-density electronic devices and cannot meet the demand for low dielectric constants of integrated circuit designs with higher requirements in the future.

Method used

By adjusting the raw material ratio, diamines containing adamantane, octa-aminophenyl cage silsesquioxane, ammonized titanium dioxide and surfactant are introduced to form a low-dielectric polyimide film, reducing the dielectric constant and increasing the pull Extension and heat resistance.

Benefits of technology

Effectively reduce the dielectric constant and improve the comprehensive performance of polyimide films, including mechanical properties and thermal stability, and is suitable for high-frequency, high-speed, and high-density electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019686A_ABST
    Figure CN119019686A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of polyimide materials, and particularly discloses a low-dielectric polyimide film and a preparation method thereof. According to the low-dielectric polyimide film, the raw materials of the low-dielectric polyimide film comprise a dianhydride monomer, diamine containing adamantane, octa-aminophenyl polyhedral oligomeric silsesquioxane, ammoniated titanium dioxide, N-phenyl-3-aminopropyltrimethoxysilane, a surfactant and the like, and the dielectric constant can be effectively reduced by regulating and controlling the proportion of all the components in the raw materials; the mechanical property and the thermal property of the polyimide film are improved, and the comprehensive performance of the prepared polyimide film is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyimide materials, and in particular relates to a low-dielectric polyimide film and a preparation method thereof. Background Art

[0002] With the rapid development of information technology, especially in the field of information and microelectronics, the requirements for integrated circuits are increasing day by day. Not only do we pursue higher performance and versatility to adapt to increasingly complex application scenarios, but we also pursue thinner and lighter designs to meet the urgent needs of portability and flexibility in emerging markets such as portable devices and wearable technologies.

[0003] This trend has greatly promoted the development of integrated circuits towards ultra-high density and ultra-large scale, which in turn has posed unprecedented challenges to key materials and technologies. Therefore, reducing the resistance-capacitance (RC) delay of devices, reducing crosstalk, and controlling power loss have become key factors in improving the efficiency and performance of integrated circuits.

[0004] As a high-performance polymer material, polyimide (PI) is widely used in many fields, especially in the field of microelectronics. Its film products, as key interlayer dielectric materials (ILD) in flexible copper clad laminates (FCCL), play a fundamental supporting role in the overall performance and function of flexible printed circuit boards (FPCB). However, the dielectric constant of traditional PI films is relatively high, which cannot fully meet the urgent demand for low dielectric constants in current and future integrated circuit designs with higher requirements.

[0005] At present, the invention patent CN117430949A discloses a polyimide film having both high thermal conductivity and low thermal expansion coefficient and a preparation method thereof. In terms of weight, the polyimide film comprises: 5-40 parts of organic amine modified thermal conductive filler, 50-120 parts of polar solvent, 2-10 parts of biphenyl dianhydride, and 2-12 parts of p-phenylenediamine. The preparation method of the polyimide film is as follows: under nitrogen protection, biphenyl dianhydride and p-phenylenediamine are first placed in a polar solvent, stirred evenly for polycondensation reaction, the reaction temperature is 30-50°C, the reaction time is 30-60 minutes, and then the organic amine modified thermal conductive filler is added, followed by stirring and ultrasonic degassing, and then casting treatment is performed, and finally heating and curing treatment is performed in a vacuum drying oven; the polyimide film prepared by the invention has the advantages of high thermal conductivity and low thermal expansion coefficient, but still has a relatively high dielectric constant and loss factor, which limits its application in high-frequency, high-speed, and high-density electronic devices. Summary of the invention

[0006] The purpose of the present invention is to overcome the above problems existing in the prior art and provide a low dielectric polyimide film and a preparation method thereof, so as to ensure that the prepared polyimide film not only has good mechanical and thermal properties but also has a low dielectric constant.

[0007] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0008] The embodiment of the first aspect of the present invention provides a low dielectric polyimide film, comprising the following raw materials in parts by weight: 20-40 parts of dianhydride monomer, 60-80 parts of adamantane-containing diamine, 10-20 parts of octaaminophenyl cage silsesquioxane, 5-15 parts of aminated titanium dioxide, 10-20 parts of N-phenyl-3-aminopropyltrimethoxysilane, 3-7 parts of surfactant, and 50-100 parts of solvent;

[0009] Wherein, the preparation method of the diamine containing adamantane is:

[0010] S1: At room temperature, 4,6-bis(1-adamantyl)-1,3-diglycidyl ether benzene and sodium borohydride are added to N,N-dimethylformamide. After fully dissolved, the temperature is lowered to 8-12°C, and the reaction is kept warm for 8-10 hours. The temperature is returned to room temperature, and compound A is obtained after filtering, washing, and rotary evaporation;

[0011] S2: Add compound A obtained in step S1 and acetanilide to concentrated sulfuric acid, and react at room temperature with stirring for 10-15 hours to form a mixed system 1, add water to the mixed system 1, stir evenly, and stand for 4-8 hours, and obtain compound B after vacuum filtration, water washing, recrystallization, and vacuum drying;

[0012] S3: adding compound B obtained in step S2 to ethylene glycol and stirring to dissolve, adjusting the pH to 8-12 with alkali, heating to 120-130° C. and stirring to react for 4-6 hours, cooling to room temperature to form a mixed system II, adding the mixed system II to water, stirring evenly, standing for 4-8 hours, vacuum filtering, washing with water, recrystallizing, and vacuum drying to obtain a diamine containing adamantane;

[0013] Wherein, the preparation method of the ammoniated titanium dioxide is:

[0014] The nano-titanium dioxide is treated with electron beam irradiation for 8-10 seconds to obtain hydroxylated titanium dioxide, the hydroxylated titanium dioxide and lysine are added to dimethyl sulfoxide, ultrasonically stirred for 5-10 minutes, stirred and reacted at 30-55° C. for 10-20 hours, filtered, and dried to obtain ammoniated titanium dioxide.

[0015] Furthermore, the reaction formula of the preparation method of the adamantane-containing diamine is as follows:

[0016]

[0017] Further, in step S1, the ratio of 4,6-bis(1-adamantyl)-1,3-diglycidyl ether benzene, sodium borohydride, and N,N-dimethylformamide is 4.6-5.1 g: 0.75-1 g: 50-80 mL;

[0018] In step S2, the ratio of compound A, acetanilide, concentrated sulfuric acid and water is 4.6-5.1 g: 2.2-2.5 g: 10-20 mL: 40-60 mL;

[0019] In step S3, the ratio of compound B, ethylene glycol and water is 6.7-7 g: 25-30 mL: 100 mL.

[0020] Furthermore, in the preparation method of the ammoniated titanium dioxide, the ratio of the amount of the hydroxylated titanium dioxide, lysine, and dimethyl sulfoxide is 20-30 g: 3-9 g: 40-60 mL.

[0021] Furthermore, in the method for preparing ammoniated titanium dioxide, during the irradiation treatment, the irradiation dose of the electron beam is 400-450 kGy.

[0022] Furthermore, the dianhydride monomer is prepared by mixing 1,2,3,4-cyclobutanetetracarboxylic dianhydride and bisphenol A diether dianhydride in a mass ratio of 10:2-5.

[0023] Furthermore, the surfactant is any one or more of perfluoroalkyl betaine, erucamide, sodium dodecyl sulfate, didodecyl dimethyl ammonium bromide, and octadecyl trimethyl ammonium bromide mixed in any proportion.

[0024] Furthermore, the solvent is any one or more of ethanol, ethyl acetate, N,N-dimethylacetamide, furfuryl alcohol, diethylene glycol, ethylene glycol butyl ether, and methyl lactate mixed in any proportion.

[0025] The embodiment of the second aspect of the present invention provides a method for preparing a low dielectric polyimide film, the method comprising the following steps:

[0026] A dianhydride monomer, adamantane-containing diamine, octaaminophenyl cage silsesquioxane, aminated titanium dioxide, N-phenyl-3-aminopropyltrimethoxysilane and a surfactant are added to a solvent, stirred and reacted at 60-70°C for 8-12 hours, and a film-forming liquid is obtained after degassing; the film-forming liquid is subjected to a film-forming treatment to obtain a liquid film, the liquid film is subjected to programmed heating, cooled to room temperature, and the liquid film is irradiated with an ultraviolet light source to obtain a low dielectric polyimide film.

[0027] Furthermore, the specific process of the programmed temperature increase is: first increase the temperature to 130-190°C, keep warm for 30-60 minutes, then increase the temperature to 210-250°C, keep warm for 30-60 minutes, and finally increase the temperature to 280-330°C, keep warm for 30-60 minutes.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] 1. In the present invention, the raw materials of the polyimide film include dianhydride monomers, adamantane-containing diamines, octaaminophenyl cage silsesquioxane, ammoniated titanium dioxide, N-phenyl-3-aminopropyltrimethoxysilane, surfactants, etc. By adjusting the proportion of each component in the raw materials, the dielectric constant can be effectively reduced, the tensile strength and heat resistance can be improved, thereby obtaining a polyimide film with excellent comprehensive performance.

[0030] 2. In the present invention, an adamantane-containing diamine is introduced into the structure of the polyimide film. The adamantane-containing diamine has two cage-like adamantyl groups and three phenyl groups, and has the characteristics of large free volume, low polarity and high rigidity. It can destroy the symmetry and regularity of the polyimide molecular structure, increase the distance between molecular chains, and increase the degree of distortion of single molecular chains, thereby reducing the packing density of the molecular chains, inhibiting the formation of intermolecular charge transfer complexes, and effectively reducing the dielectric constant. At the same time, the introduction of large-volume side groups has little effect on the rigidity of the main chain, so that the polyimide film can also maintain good thermal stability and mechanical properties.

[0031] 3. In the present invention, aminated titanium dioxide is grafted with lysine on the surface of nano-titanium dioxide. Aminated titanium dioxide can participate in the polymerization reaction of diamine and dianhydride, form a special microstructure in the polyimide film, improve the glass transition temperature of the polyimide film, and the titanium dioxide structure with greater rigidity can effectively loosen the network structure of the polyimide, block the dipole polarization between molecular chains, and improve the stability of the dielectric properties of the polyimide film to a certain extent.

[0032] 4. In the present invention, the dianhydride monomer is obtained by mixing 1,2,3,4-cyclobutanetetracarboxylic dianhydride and bisphenol A diether dianhydride in a specific ratio. The two synergistically enhance each other and can regulate the molecular structure and polarity of the polyimide film. While maintaining excellent mechanical properties, the polyimide film has a lower dielectric constant.

[0033] 5. The octaaminophenyl cage silsesquioxane and ammoniated titanium dioxide of the present invention are both rigid particles. They assist each other and increase the steric hindrance with different spatial structures at the microscopic level, thereby better inhibiting the formation of intermolecular charge transfer complexes and reducing the dielectric properties of the obtained polyimide film. At the same time, both can be combined with the dianhydride monomer by chemical bonds to form a network structure, which helps to improve the heat resistance and mechanical properties of the polyimide film. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0035] Figure 1 This is a microstructure diagram of the polyimide film prepared in Example 1. DETAILED DESCRIPTION

[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] In a first aspect, the present invention provides a low dielectric polyimide film, comprising the following raw materials in parts by weight: 20-40 parts of dianhydride monomer, 60-80 parts of adamantane-containing diamine, 10-20 parts of octaaminophenyl cage silsesquioxane, 5-15 parts of aminated titanium dioxide, 10-20 parts of N-phenyl-3-aminopropyltrimethoxysilane, 3-7 parts of surfactant, and 50-100 parts of solvent;

[0038] The dianhydride monomer is prepared by mixing 1,2,3,4-cyclobutane tetracarboxylic dianhydride and bisphenol A type diether dianhydride in a mass ratio of 10:2-5;

[0039] Wherein, the preparation method of the diamine containing adamantane is:

[0040] S1: At room temperature, 4,6-bis(1-adamantyl)-1,3-diglycidyl ether benzene and sodium borohydride are added to N,N-dimethylformamide. After fully dissolved, the temperature is lowered to 8-12°C, and the reaction is kept warm for 8-10 hours. The temperature is returned to room temperature, and compound A is obtained after filtering, washing, and rotary evaporation;

[0041] In step S1, the ratio of 4,6-bis(1-adamantyl)-1,3-diglycidyl ether benzene, sodium borohydride, and N,N-dimethylformamide is 4.6-5.1 g: 0.75-1 g: 50-80 mL;

[0042] S2: Add compound A obtained in step S1 and acetanilide to concentrated sulfuric acid, and react at room temperature with stirring for 10-15 hours to form a mixed system 1, add water to the mixed system 1, stir evenly, and stand for 4-8 hours, and obtain compound B after vacuum filtration, water washing, recrystallization, and vacuum drying;

[0043] In step S2, the ratio of compound A, acetanilide, concentrated sulfuric acid and water is 4.6-5.1 g: 2.2-2.5 g: 10-20 mL: 40-60 mL;

[0044] S3: adding compound B obtained in step S2 to ethylene glycol and stirring to dissolve, adjusting the pH to 8-12 with alkali, heating to 120-130° C. and stirring to react for 4-6 hours, cooling to room temperature to form a mixed system II, adding the mixed system II to water, stirring evenly, standing for 4-8 hours, vacuum filtering, washing with water, recrystallizing, and vacuum drying to obtain a diamine containing adamantane;

[0045] In step S3, the ratio of compound B, ethylene glycol and water is 6.7-7 g: 25-30 mL: 100 mL;

[0046] The reaction formula of the preparation method of the diamine containing adamantane is as follows:

[0047]

[0048] Wherein, the preparation method of ammoniated titanium dioxide is:

[0049] Treating nano titanium dioxide with electron beam irradiation at a dose of 400-450 kGy for 8-10 seconds to obtain hydroxylated titanium dioxide, adding hydroxylated titanium dioxide and lysine into dimethyl sulfoxide, stirring with ultrasound for 5-10 minutes, stirring and reacting at 30-55° C. for 10-20 hours, filtering, and drying to obtain ammoniated titanium dioxide;

[0050] In the preparation method of aminated titanium dioxide, the ratio of hydroxylated titanium dioxide, lysine and dimethyl sulfoxide is 20-30 g: 3-9 g: 40-60 mL;

[0051] Wherein, the surfactant is any one or more of perfluoroalkyl betaine, erucamide, sodium dodecyl sulfate, didodecyl dimethyl ammonium bromide, octadecyl trimethyl ammonium bromide mixed in any proportion;

[0052] The solvent is any one or more of ethanol, ethyl acetate, N,N-dimethylacetamide, furfuryl alcohol, diethylene glycol, ethylene glycol butyl ether, and methyl lactate mixed in any proportion;

[0053] In a second aspect, the present invention provides a method for preparing a low dielectric polyimide film, the method comprising the following steps:

[0054] Adding dianhydride monomer, adamantane-containing diamine, octaaminophenyl cage silsesquioxane, aminated titanium dioxide, N-phenyl-3-aminopropyltrimethoxysilane, and a surfactant into a solvent, stirring and reacting at 60-70° C. for 8-12 hours, and degassing to obtain a film-forming solution; subjecting the film-forming solution to a film-forming treatment to obtain a liquid film, subjecting the liquid film to programmed temperature rise, cooling to room temperature, and irradiating the liquid film with an ultraviolet light source to obtain a low dielectric polyimide film;

[0055] The specific process of programmed heating is: first heat to 130-190°C, keep warm for 30-60 minutes, then heat to 210-250°C, keep warm for 30-60 minutes, and finally heat to 280-330°C, keep warm for 30-60 minutes.

[0056] The following preparation examples 1-3 provide methods for preparing adamantane-containing diamines. In the following preparation examples, 4,6-bis(1-adamantyl)-1,3-diglycidyl ether benzene, CAS No. 1030386-18-5, was purchased from Xuzhou Bokang Information Chemicals Co., Ltd.

[0057] Preparation Example 1

[0058] This preparation example provides a method for preparing a diamine containing adamantane, and the preparation method comprises the following steps:

[0059] S1: At room temperature, 4.6 g of 4,6-bis(1-adamantyl)-1,3-diglycidyl ether benzene and 0.75 g of sodium borohydride were added into 50 mL of N,N-dimethylformamide. After fully dissolved, the temperature was lowered to 8°C, and the reaction was kept warm for 8 hours. The temperature was returned to room temperature, filtered, washed, and rotary evaporated to obtain compound A.

[0060] S2: Add 4.6 g of compound A obtained in step S1 and 2.2 g of acetanilide to 10 mL of concentrated sulfuric acid with a concentration of 98 wt %, and react at room temperature with stirring for 10 h to form a mixed system 1. Add 40 mL of water to the mixed system 1, stir evenly, let stand for 4 h, vacuum filter, wash with water, recrystallize with ethanol / water (in ethanol / water, the volume ratio of ethanol to water is 1 / 3, and the amount of ethanol / water added is 100 mL), and vacuum dry at 100° C. for 10 h to obtain compound B;

[0061] S3: Add 6.7 g of compound B obtained in step S2 to 25 mL of ethylene glycol and stir to dissolve, add 10 wt % sodium hydroxide solution to adjust the pH to 8, heat to 120° C. and stir to react for 4 h, cool to room temperature to form mixed system II, add mixed system II to 100 mL of water, stir evenly, let stand for 4 h, vacuum filter, wash with water, recrystallize with ethanol (100 mL), and vacuum dry at 100° C. for 10 h to obtain a diamine containing adamantane.

[0062] Preparation Example 2

[0063] This preparation example provides a method for preparing a diamine containing adamantane, and the preparation method comprises the following steps:

[0064] S1: At room temperature, 4.8 g of 4,6-bis(1-adamantyl)-1,3-diglycidyl ether benzene and 0.88 g of sodium borohydride were added to 75 mL of N,N-dimethylformamide. After fully dissolved, the temperature was lowered to 10°C, and the reaction was kept warm for 9 hours. The temperature was returned to room temperature, filtered, washed, and rotary evaporated to obtain compound A;

[0065] S2: Add 4.9 g of compound A obtained in step S1 and 2.4 g of acetanilide to 15 mL of concentrated sulfuric acid with a concentration of 98 wt %, and react at room temperature with stirring for 13 h to form a mixed system 1. Add 50 mL of water to the mixed system 1, stir evenly, let stand for 6 h, vacuum filter, wash with water, recrystallize with ethanol / water (in ethanol / water, the volume ratio of ethanol to water is 1 / 3, and the amount of ethanol / water added is 100 mL), and vacuum dry at 100° C. for 10 h to obtain compound B;

[0066] S3: Add 6.9 g of compound B obtained in step S2 to 28 mL of ethylene glycol and stir to dissolve, add 10 wt % sodium hydroxide solution to adjust the pH to 10, heat to 125 ° C and stir to react for 5 hours, cool to room temperature to form a mixed system II, add the mixed system II to 100 mL of water, stir evenly, let stand for 6 hours, vacuum filter, wash with water, recrystallize with ethanol (100 mL), and vacuum dry at 100 ° C for 10 hours to obtain a diamine containing adamantane.

[0067] Preparation Example 3

[0068] This preparation example provides a method for preparing a diamine containing adamantane, and the preparation method comprises the following steps:

[0069] S1: At room temperature, 5.1 g of 4,6-bis(1-adamantyl)-1,3-diglycidyl ether benzene and 1 g of sodium borohydride were added to 80 mL of N,N-dimethylformamide. After fully dissolved, the temperature was lowered to 12°C, and the reaction was kept warm for 10 hours. The temperature was returned to room temperature, filtered, washed, and rotary evaporated to obtain compound A;

[0070] S2: Add 5.1 g of compound A obtained in step S1 and 2.5 g of acetanilide to 20 mL of concentrated sulfuric acid with a concentration of 98 wt %, and react at room temperature with stirring for 15 h to form a mixed system 1. Add 60 mL of water to the mixed system 1, stir evenly, let stand for 8 h, vacuum filter, wash with water, recrystallize with ethanol / water (in ethanol / water, the volume ratio of ethanol to water is 1 / 3, and the amount of ethanol / water added is 100 mL), and vacuum dry at 100° C. for 10 h to obtain compound B;

[0071] S3: Add 7 g of compound B obtained in step S2 to 30 mL of ethylene glycol and stir to dissolve, add 10 wt % sodium hydroxide solution to adjust the pH to 12, heat to 130° C. and stir to react for 6 h, cool to room temperature to form mixed system II, add mixed system II to 100 mL of water, stir evenly, let stand for 8 h, vacuum filter, wash with water, recrystallize with ethanol (100 mL), and vacuum dry at 100° C. for 10 h to obtain a diamine containing adamantane.

[0072] The following preparation examples 4-6 provide methods for preparing ammoniated titanium dioxide. Unless otherwise specified, all raw materials in the following preparation examples can be obtained commercially.

[0073] Preparation Example 4

[0074] This preparation example provides a method for preparing ammoniated titanium dioxide, which comprises the following steps:

[0075] 20g of nano titanium dioxide was irradiated with an electron beam at a dose of 400kGy for 8s to obtain hydroxylated titanium dioxide; 20g of hydroxylated titanium dioxide and 3g of lysine were added to 40mL of dimethyl sulfoxide, and ultrasonically stirred for 5min. After stirring at 30°C for 10h, the mixture was filtered and dried to obtain ammoniated titanium dioxide.

[0076] Preparation Example 5

[0077] This preparation example provides a method for preparing ammoniated titanium dioxide, which comprises the following steps:

[0078] 25g of nano titanium dioxide was irradiated with electron beam at a dose of 420kGy for 9s to obtain hydroxylated titanium dioxide; 25g of hydroxylated titanium dioxide and 6g of lysine were added to 50mL of dimethyl sulfoxide, and ultrasonically stirred for 8min. After stirring at 45°C for 15h, the mixture was filtered and dried to obtain ammoniated titanium dioxide.

[0079] Preparation Example 6

[0080] This preparation example provides a method for preparing ammoniated titanium dioxide, which comprises the following steps:

[0081] 30g of nano titanium dioxide was irradiated with an electron beam at a dose of 450kGy for 10s to obtain hydroxylated titanium dioxide; 30g of hydroxylated titanium dioxide and 9g of lysine were added to 60mL of dimethyl sulfoxide, and ultrasonically stirred for 10min. After stirring at 55°C for 20h, the mixture was filtered and dried to obtain ammoniated titanium dioxide.

[0082] The following Examples 1-3 and Comparative Examples 1-6 provide a low dielectric polyimide film and a preparation method thereof. In the following Examples and Comparative Examples, unless otherwise specified, all raw materials can be obtained commercially.

[0083] Example 1

[0084] This embodiment provides a low dielectric polyimide film, comprising the following raw materials in parts by weight: 20 parts of dianhydride monomer, 60 parts of adamantane-containing diamine, 10 parts of octaaminophenyl cage silsesquioxane, 5 parts of aminated titanium dioxide, 10 parts of N-phenyl-3-aminopropyltrimethoxysilane, 3 parts of surfactant, and 50 parts of solvent;

[0085] The dianhydride monomer is obtained by mixing 1,2,3,4-cyclobutanetetracarboxylic dianhydride and bisphenol A diether dianhydride in a mass ratio of 5:1; the adamantane-containing diamine is prepared by Preparation Example 1; the aminated titanium dioxide is prepared by Preparation Example 4; the surfactant is perfluoroalkyl betaine; and the solvent is obtained by mixing N,N-dimethylacetamide and ethylene glycol butyl ether in a mass ratio of 4:1.

[0086] This embodiment also provides a method for preparing a low dielectric polyimide film, the method comprising the following steps:

[0087] A dianhydride monomer, adamantane-containing diamine, octaaminophenyl cage silsesquioxane, aminated titanium dioxide, N-phenyl-3-aminopropyltrimethoxysilane and a surfactant are added to a solvent, stirred and reacted at 60°C for 8 hours, and a film-forming solution is obtained after degassing; the film-forming solution is subjected to a film-forming treatment to obtain a liquid film, and the liquid film is subjected to a programmed temperature increase, first to 130°C, kept warm for 60 minutes, then to 210°C, kept warm for 60 minutes, and finally to 280°C, kept warm for 60 minutes, then cooled to room temperature, and the liquid film is irradiated with an ultraviolet light source to obtain a low dielectric polyimide film.

[0088] Example 2

[0089] This embodiment provides a low dielectric polyimide film, comprising the following raw materials in parts by weight: 30 parts of dianhydride monomer, 70 parts of adamantane-containing diamine, 15 parts of octaaminophenyl cage silsesquioxane, 10 parts of aminated titanium dioxide, 15 parts of N-phenyl-3-aminopropyltrimethoxysilane, 5 parts of surfactant, and 80 parts of solvent;

[0090] The dianhydride monomer is obtained by mixing 1,2,3,4-cyclobutanetetracarboxylic dianhydride and bisphenol A diether dianhydride in a mass ratio of 10:3; the adamantane-containing diamine is obtained by Preparation Example 2; the ammoniated titanium dioxide is obtained by Preparation Example 5; the surfactant is didodecyl dimethyl ammonium bromide; and the solvent is obtained by mixing ethyl acetate and ethylene glycol butyl ether in a mass ratio of 4:1;

[0091] This embodiment also provides a method for preparing a low dielectric polyimide film, the method comprising the following steps:

[0092] A dianhydride monomer, adamantane-containing diamine, octaaminophenyl cage silsesquioxane, aminated titanium dioxide, N-phenyl-3-aminopropyltrimethoxysilane and a surfactant are added to a solvent, stirred and reacted at 65°C for 10 hours, and a film-forming solution is obtained after degassing; the film-forming solution is subjected to a film-forming treatment to obtain a liquid film, and the liquid film is subjected to a programmed temperature increase, first to 160°C, kept warm for 45 minutes, then to 230°C, kept warm for 45 minutes, and finally to 300°C, kept warm for 45 minutes, then cooled to room temperature, and the liquid film is irradiated with an ultraviolet light source to obtain a low dielectric polyimide film.

[0093] Example 3

[0094] This embodiment provides a low dielectric polyimide film, comprising the following raw materials in parts by weight: 40 parts of dianhydride monomer, 80 parts of adamantane-containing diamine, 20 parts of octaaminophenyl cage silsesquioxane, 15 parts of aminated titanium dioxide, 20 parts of N-phenyl-3-aminopropyltrimethoxysilane, 7 parts of surfactant, and 100 parts of solvent;

[0095] The dianhydride monomer is obtained by mixing 1,2,3,4-cyclobutanetetracarboxylic dianhydride and bisphenol A diether dianhydride in a mass ratio of 2:1; the adamantane-containing diamine is obtained by Preparation Example 3; the ammoniated titanium dioxide is obtained by Preparation Example 6; the surfactant is octadecyltrimethylammonium bromide; and the solvent is obtained by mixing N,N-dimethylacetamide and methyl lactate in a mass ratio of 4:1;

[0096] This embodiment also provides a method for preparing a low dielectric polyimide film, the method comprising the following steps:

[0097] A dianhydride monomer, adamantane-containing diamine, octaaminophenyl cage silsesquioxane, aminated titanium dioxide, N-phenyl-3-aminopropyltrimethoxysilane and a surfactant are added to a solvent, stirred and reacted at 70°C for 12 hours, and a film-forming solution is obtained after degassing; the film-forming solution is subjected to a film-forming treatment to obtain a liquid film, and the liquid film is subjected to a programmed temperature increase, first to 190°C, kept warm for 30 minutes, then to 250°C, kept warm for 30 minutes, and finally to 330°C, kept warm for 30 minutes, then cooled to room temperature, and the liquid film is irradiated with an ultraviolet light source to obtain a low dielectric polyimide film.

[0098] Comparative Example 1

[0099] This comparative example provides a low dielectric polyimide film, which is different from Example 1 only in that this comparative example uses an equal mass of 4,4'-diaminodiphenylmethane to replace the diamine containing adamantane, specifically as follows:

[0100] A low dielectric polyimide film comprises the following raw materials in parts by weight: 20 parts of dianhydride monomer, 60 parts of 4,4'-diaminodiphenylmethane, 10 parts of octaaminophenyl cage silsesquioxane, 5 parts of ammoniated titanium dioxide, 10 parts of N-phenyl-3-aminopropyltrimethoxysilane, 3 parts of surfactant, and 50 parts of solvent;

[0101] The dianhydride monomer is obtained by mixing 1,2,3,4-cyclobutanetetracarboxylic dianhydride and bisphenol A diether dianhydride in a mass ratio of 5:1; ammoniated titanium dioxide is prepared by Preparation Example 4; the surfactant is perfluoroalkyl betaine; and the solvent is obtained by mixing N,N-dimethylacetamide and ethylene glycol butyl ether in a mass ratio of 4:1;

[0102] This comparative example also provides a method for preparing a low dielectric polyimide film, comprising the following steps:

[0103] A dianhydride monomer, 4,4'-diaminodiphenylmethane, octaaminophenyl cage silsesquioxane, aminated titanium dioxide, N-phenyl-3-aminopropyltrimethoxysilane and a surfactant are added to a solvent, stirred and reacted at 60°C for 8 hours, and a film-forming solution is obtained after degassing; the film-forming solution is subjected to a film-forming treatment to obtain a liquid film, and the liquid film is subjected to a programmed temperature increase, first to 130°C, kept warm for 60 minutes, then to 210°C, kept warm for 60 minutes, and finally to 280°C, kept warm for 60 minutes, then cooled to room temperature, and the liquid film is irradiated with an ultraviolet light source to obtain a low dielectric polyimide film.

[0104] Comparative Example 2

[0105] This comparative example provides a low dielectric polyimide film, which is different from Example 1 only in that an equal mass of nano-titanium dioxide is used to replace ammoniated titanium dioxide, as follows:

[0106] A low dielectric polyimide film comprises the following raw materials in parts by weight: 20 parts of dianhydride monomer, 60 parts of adamantane-containing diamine, 10 parts of octaaminophenyl cage-shaped silsesquioxane, 5 parts of nano titanium dioxide, 10 parts of N-phenyl-3-aminopropyltrimethoxysilane, 3 parts of surfactant, and 50 parts of solvent;

[0107] The dianhydride monomer is obtained by mixing 1,2,3,4-cyclobutanetetracarboxylic dianhydride and bisphenol A diether dianhydride in a mass ratio of 5:1; the adamantane-containing diamine is prepared by Preparation Example 1; the surfactant is perfluoroalkyl betaine; and the solvent is obtained by mixing N,N-dimethylacetamide and ethylene glycol butyl ether in a mass ratio of 4:1;

[0108] A method for preparing a low dielectric polyimide film comprises the following steps:

[0109] A dianhydride monomer, adamantane-containing diamine, octaaminophenyl cage silsesquioxane, nano titanium dioxide, N-phenyl-3-aminopropyltrimethoxysilane and a surfactant are added to a solvent, stirred and reacted at 60°C for 8 hours, and a film-forming solution is obtained after degassing; the film-forming solution is subjected to a film-forming treatment to obtain a liquid film, and the liquid film is subjected to a programmed temperature increase, first to 130°C, kept warm for 60 minutes, then to 210°C, kept warm for 60 minutes, and finally to 280°C, kept warm for 60 minutes, then cooled to room temperature, and the liquid film is irradiated with an ultraviolet light source to obtain a low dielectric polyimide film.

[0110] Comparative Example 3

[0111] This comparative example provides a low dielectric polyimide film, which is different from Example 1 only in that an equal mass of octaaminophenyl cage silsesquioxane is used to replace the aminated titanium dioxide, as follows:

[0112] A low dielectric polyimide film comprises the following raw materials in parts by weight: 20 parts of dianhydride monomer, 60 parts of adamantane-containing diamine, 15 parts of octaaminophenyl cage-shaped silsesquioxane, 10 parts of N-phenyl-3-aminopropyltrimethoxysilane, 3 parts of surfactant, and 50 parts of solvent;

[0113] The dianhydride monomer is obtained by mixing 1,2,3,4-cyclobutanetetracarboxylic dianhydride and bisphenol A diether dianhydride in a mass ratio of 5:1; the adamantane-containing diamine is prepared by Preparation Example 1; the surfactant is perfluoroalkyl betaine; and the solvent is obtained by mixing N,N-dimethylacetamide and ethylene glycol butyl ether in a mass ratio of 4:1;

[0114] A method for preparing a low dielectric polyimide film comprises the following steps:

[0115] A dianhydride monomer, a diamine containing adamantane, octaaminophenyl cage silsesquioxane, N-phenyl-3-aminopropyltrimethoxysilane and a surfactant are added to a solvent, and the mixture is stirred and reacted at 60°C for 8 hours. A film-forming solution is obtained after degassing. The film-forming solution is subjected to a film-forming treatment to obtain a liquid film. The liquid film is subjected to a programmed temperature increase, first to 130°C, and kept warm for 60 minutes, then to 210°C, and kept warm for 60 minutes, and finally to 280°C, and kept warm for 60 minutes, and then cooled to room temperature. The liquid film is irradiated with an ultraviolet light source to obtain a low dielectric polyimide film.

[0116] Comparative Example 4

[0117] This comparative example provides a low dielectric polyimide film, which is different from Example 1 only in that an equal mass of aminated titanium dioxide is used to replace octaaminophenyl cage silsesquioxane, as follows:

[0118] A low dielectric polyimide film comprises the following raw materials in parts by weight: 20 parts of dianhydride monomer, 60 parts of adamantane-containing diamine, 15 parts of ammoniated titanium dioxide, 10 parts of N-phenyl-3-aminopropyltrimethoxysilane, 3 parts of surfactant, and 50 parts of solvent;

[0119] The dianhydride monomer is obtained by mixing 1,2,3,4-cyclobutanetetracarboxylic dianhydride and bisphenol A diether dianhydride in a mass ratio of 5:1; the adamantane-containing diamine is obtained by Preparation Example 1; the aminated titanium dioxide is obtained by Preparation Example 4; the surfactant is perfluoroalkyl betaine; and the solvent is obtained by mixing N,N-dimethylacetamide and ethylene glycol butyl ether in a mass ratio of 4:1;

[0120] A method for preparing a low dielectric polyimide film comprises the following steps:

[0121] A dianhydride monomer, adamantane-containing diamine, aminated titanium dioxide, N-phenyl-3-aminopropyltrimethoxysilane and a surfactant are added to a solvent, stirred and reacted at 60°C for 8 hours, and a film-forming solution is obtained after degassing; the film-forming solution is subjected to a film-forming treatment to obtain a liquid film, and the liquid film is subjected to a programmed temperature increase, first to 130°C, kept warm for 60 minutes, then to 210°C, kept warm for 60 minutes, and finally to 280°C, kept warm for 60 minutes, then cooled to room temperature, and the liquid film is irradiated with an ultraviolet light source to obtain a low dielectric polyimide film.

[0122] Comparative Example 5

[0123] This comparative example provides a low dielectric polyimide film, which is different from Example 1 only in that the dianhydride monomer is only 1,2,3,4-cyclobutanetetracarboxylic dianhydride, specifically as follows:

[0124] A low dielectric polyimide film comprises the following raw materials in parts by weight: 20 parts of dianhydride monomer, 60 parts of adamantane-containing diamine, 10 parts of octaaminophenyl cage silsesquioxane, 5 parts of aminated titanium dioxide, 10 parts of N-phenyl-3-aminopropyltrimethoxysilane, 3 parts of surfactant, and 50 parts of solvent;

[0125] The dianhydride monomer is only 1,2,3,4-cyclobutanetetracarboxylic dianhydride; the diamine containing adamantane is prepared by Preparation Example 1; the aminated titanium dioxide is prepared by Preparation Example 4; the surfactant is perfluoroalkyl betaine; and the solvent is obtained by mixing N,N-dimethylacetamide and ethylene glycol butyl ether in a mass ratio of 4:1;

[0126] A method for preparing a low dielectric polyimide film comprises the following steps:

[0127] A dianhydride monomer, adamantane-containing diamine, octaaminophenyl cage silsesquioxane, aminated titanium dioxide, N-phenyl-3-aminopropyltrimethoxysilane and a surfactant are added to a solvent, stirred and reacted at 60°C for 8 hours, and a film-forming solution is obtained after degassing; the film-forming solution is subjected to a film-forming treatment to obtain a liquid film, and the liquid film is subjected to a programmed temperature increase, first to 130°C, kept warm for 60 minutes, then to 210°C, kept warm for 60 minutes, and finally to 280°C, kept warm for 60 minutes, then cooled to room temperature, and the liquid film is irradiated with an ultraviolet light source to obtain a low dielectric polyimide film.

[0128] Comparative Example 6

[0129] This comparative example provides a low dielectric polyimide film, which is different from Example 1 only in that the dianhydride monomer is only bisphenol A diether dianhydride, specifically as follows:

[0130] A low dielectric polyimide film comprises the following raw materials in parts by weight: 20 parts of dianhydride monomer, 60 parts of adamantane-containing diamine, 10 parts of octaaminophenyl cage silsesquioxane, 5 parts of aminated titanium dioxide, 10 parts of N-phenyl-3-aminopropyltrimethoxysilane, 3 parts of surfactant, and 50 parts of solvent;

[0131] The dianhydride monomer is only bisphenol A diether dianhydride; the diamine containing adamantane is prepared by Preparation Example 1; the aminated titanium dioxide is prepared by Preparation Example 4; the surfactant is perfluoroalkyl betaine; the solvent is obtained by mixing N,N-dimethylacetamide and ethylene glycol butyl ether in a mass ratio of 4:1;

[0132] A method for preparing a low dielectric polyimide film comprises the following steps:

[0133] A dianhydride monomer, adamantane-containing diamine, octaaminophenyl cage silsesquioxane, aminated titanium dioxide, N-phenyl-3-aminopropyltrimethoxysilane and a surfactant are added to a solvent, stirred and reacted at 60°C for 8 hours, and a film-forming solution is obtained after degassing; the film-forming solution is subjected to a film-forming treatment to obtain a liquid film, and the liquid film is subjected to a programmed temperature increase, first to 130°C, kept warm for 60 minutes, then to 210°C, kept warm for 60 minutes, and finally to 280°C, kept warm for 60 minutes, then cooled to room temperature, and the liquid film is irradiated with an ultraviolet light source to obtain a low dielectric polyimide film.

[0134] Performance Testing

[0135] The performance of the low dielectric polyimide films prepared in Examples 1-3 and Comparative Examples 1-6 was tested, and the relevant performance parameter detection process was as follows:

[0136] Mechanical properties test: Tested according to GB / T 1040.3-2006, sample size is 20mm×200mm, tensile speed is 20mm / min, gauge length is 50mm;

[0137] Thermal performance test: Thermogravimetric analysis was performed in a nitrogen atmosphere at 40 mL / min, at a heating rate of 10°C / min, in a temperature range of 30-1000°C, and the 5% thermal weight loss temperature was taken as the thermal decomposition temperature;

[0138] Dielectric performance test: first cut the film into 20mm×20mm specifications, then spray gold on both sides, and test the dielectric constant and dielectric loss of the film according to GB / T5594.4-2015;

[0139] The test results are shown in Table 1;

[0140] Table 1

[0141]

[0142]

[0143] It can be seen from the data in Table 1 that, compared with Comparative Examples 1-6, the dielectric constant and dielectric loss tangent of the polyimide film prepared in Example 1-3 are reduced, and still have excellent mechanical properties and thermal stability, and the comprehensive performance is significantly better than that of Comparative Examples 1-6.

[0144] By comparing Example 1 with Comparative Example 1, it can be seen that the present invention adopts a diamine containing adamantane of a special structure, which has a large volume effect, can reduce the dipole moment and polarizability per unit volume, increase the distance between molecular chains, reduce the intermolecular force, and thus reduce the cohesive energy density of polyimide and increase its free volume fraction, thereby greatly contributing to improving the dielectric properties of polyimide.

[0145] By comparing Example 1 with Comparative Example 2, it can be seen that the present invention uses ammoniated titanium dioxide. Compared with nano titanium dioxide, the ammoniated titanium dioxide can be chemically bonded with the dianhydride monomer, thereby improving the compatibility between the components. On the basis of reducing the dielectric constant of the polyimide film, the mechanical properties and thermal properties can still be maintained without being destroyed.

[0146] By comparing Example 1 with Comparative Examples 3 and 4, it can be seen that the present invention selects two different rigid particles, octaaminophenyl cage silsesquioxane and aminated titanium dioxide, which interact with each other to significantly improve the dielectric properties of the polyimide film.

[0147] By comparing Example 1 with Comparative Examples 5 and 6, it can be seen that the dianhydride monomer of the present invention is a mixture of 1,2,3,4-cyclobutanetetracarboxylic dianhydride and bisphenol A diether dianhydride, which helps to adjust the molecular weight and molecular structure of the polyimide, so that the polyimide film has excellent mechanical properties and a lower dielectric constant.

[0148] In addition, the microstructure of the polyimide film prepared in Example 1 was observed using a scanning electron microscope. Figure 1 As shown, it can be seen that the surface of the film is flat and dense, which fully demonstrates that the rigid particle octaaminophenyl cage silsesquioxane and ammoniated titanium dioxide are evenly dispersed in the polymerization reaction system, which is conducive to the formation of a stable polyimide structure, which helps to improve the low dielectric properties of the film and enhance the mechanical and thermal properties.

[0149] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0150] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A low dielectric polyimide film, characterized in that: The method comprises the following raw materials in parts by weight: 20-40 parts of dianhydride monomer, 60-80 parts of adamantane-containing diamine, 10-20 parts of octaaminophenyl cage-shaped silsesquioxane, 5-15 parts of aminated titanium dioxide, 10-20 parts of N-phenyl-3-aminopropyltrimethoxysilane, 3-7 parts of surfactant, and 50-100 parts of solvent; Wherein, the preparation method of the diamine containing adamantane is: S1: At room temperature, 4,6-bis(1-adamantyl)-1,3-diglycidyl ether benzene and sodium borohydride are added to N,N-dimethylformamide. After fully dissolved, the temperature is lowered to 8-12°C, and the reaction is kept warm for 8-10 hours. The temperature is returned to room temperature, and compound A is obtained after filtering, washing, and rotary evaporation; S2: Add compound A obtained in step S1 and acetanilide to concentrated sulfuric acid, and react at room temperature with stirring for 10-15 hours to form a mixed system 1, add water to the mixed system 1, stir evenly, and stand for 4-8 hours, and obtain compound B after vacuum filtration, water washing, recrystallization, and vacuum drying; S3: adding compound B obtained in step S2 to ethylene glycol and stirring to dissolve, adjusting the pH to 8-12 with alkali, heating to 120-130° C. and stirring to react for 4-6 hours, cooling to room temperature to form a mixed system II, adding the mixed system II to water, stirring evenly, standing for 4-8 hours, vacuum filtering, washing with water, recrystallizing, and vacuum drying to obtain a diamine containing adamantane; Wherein, the preparation method of the ammoniated titanium dioxide is: The nano-titanium dioxide is treated with electron beam irradiation for 8-10 seconds to obtain hydroxylated titanium dioxide, the hydroxylated titanium dioxide and lysine are added to dimethyl sulfoxide, ultrasonically stirred for 5-10 minutes, stirred and reacted at 30-55° C. for 10-20 hours, filtered, and dried to obtain ammoniated titanium dioxide.

2. A low dielectric polyimide film according to claim 1, characterized in that: The reaction formula of the preparation method of the adamantane-containing diamine is as follows:

3. A low dielectric polyimide film according to claim 1, characterized in that: In step S1, the ratio of 4,6-bis(1-adamantyl)-1,3-diglycidyl ether benzene, sodium borohydride, and N,N-dimethylformamide is 4.6-5.1 g: 0.75-1 g: 50-80 mL; In step S2, the ratio of compound A, acetanilide, concentrated sulfuric acid and water is 4.6-5.1 g: 2.2-2.5 g: 10-20 mL: 40-60 mL; In step S3, the ratio of compound B, ethylene glycol and water is 6.7-7 g: 25-30 mL: 100 mL.

4. The low dielectric polyimide film according to claim 1, characterized in that: In the preparation method of the aminated titanium dioxide, the usage ratio of the hydroxylated titanium dioxide, lysine and dimethyl sulfoxide is 20-30 g: 3-9 g: 40-60 mL.

5. The low dielectric polyimide film according to claim 1, characterized in that: In the preparation method of ammoniated titanium dioxide, during the irradiation treatment, the irradiation dose of the electron beam is 400-450 kGy.

6. The low dielectric polyimide film according to claim 1, characterized in that: The dianhydride monomer is prepared by mixing 1,2,3,4-cyclobutanetetracarboxylic dianhydride and bisphenol A diether dianhydride in a mass ratio of 10:2-5.

7. The low dielectric polyimide film according to claim 1, characterized in that: The surfactant is any one or more of perfluoroalkyl betaine, erucamide, sodium dodecyl sulfate, didodecyl dimethyl ammonium bromide, and octadecyl trimethyl ammonium bromide mixed in any proportion.

8. The low dielectric polyimide film according to claim 1, characterized in that: The solvent is any one or more of ethanol, ethyl acetate, N,N-dimethylacetamide, furfuryl alcohol, diethylene glycol, ethylene glycol butyl ether, and methyl lactate, mixed in any proportion.

9. A method for preparing a low dielectric polyimide film according to any one of claims 1 to 8, characterized in that: The following steps are involved: A dianhydride monomer, adamantane-containing diamine, octaaminophenyl cage silsesquioxane, aminated titanium dioxide, N-phenyl-3-aminopropyltrimethoxysilane and a surfactant are added to a solvent, stirred and reacted at 60-70°C for 8-12 hours, and a film-forming liquid is obtained after degassing; the film-forming liquid is subjected to a film-forming treatment to obtain a liquid film, the liquid film is subjected to programmed heating, cooled to room temperature, and the liquid film is irradiated with an ultraviolet light source to obtain a low dielectric polyimide film.

10. The method for preparing a low dielectric polyimide film according to claim 9, characterized in that: The specific process of the programmed temperature increase is: first increase the temperature to 130-190° C., keep warm for 30-60 minutes, then increase the temperature to 210-250° C., keep warm for 30-60 minutes, and finally increase the temperature to 280-330° C., keep warm for 30-60 minutes.