In-situ cured two-component conductive hydrogel as well as preparation method and application thereof
The two-component hydrogel composed of polyaniline-oxidized polysaccharide and polyamino polymer solves the problems of insufficient conductivity, uniformity and antibacterial properties of existing conductive hydrogels, and realizes a hydrogel with high conductivity and biocompatibility, which is suitable for use in the human body.
Patent Information
- Application Number
- CN202411267680.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-26
AI Technical Summary
Existing conductive hydrogels have shortcomings in conductivity, uniformity, and antibacterial properties, and some materials have toxicity issues, making it difficult to meet the requirements for high conductivity and biocompatibility.
A two-component hydrogel composed of polyaniline-oxidized polysaccharide and polyamino polymers such as polylysine hydrochloride, polyethyleneimine, and chitosan quaternary ammonium salt is formed through in-situ curing to create a hydrogel with excellent electrical conductivity and antibacterial properties. This utilizes the conjugated π electrons of polyaniline and the antibacterial properties of polyamino polymers, combined with the biocompatibility of natural polysaccharides.
A highly conductive hydrogel with a conductivity of 1–4 S/m was achieved, exhibiting excellent biocompatibility and antibacterial properties, making it suitable for use in the human body. Furthermore, it is biodegradable in vivo, reducing the long-term toxicity risk of the material.
Smart Images

Figure BDA0005037629830000071 
Figure BDA0005037629830000081 
Figure BDA0005037629830000082
Abstract
Description
Technical Field
[0001] The present invention relates to the field of hydrogels, in particular to the field of C08F251 / 00, and specifically to an in-situ cured two-component conductive hydrogel and a preparation method and application thereof. Background Art
[0002] Conductive hydrogel, as the name implies, has both the gel properties of hydrogel and the conductive properties of conductive medium. The gel properties make conductive hydrogel have good biocompatibility and high diffusivity of small molecules, while the conductive properties make conductive hydrogel have some properties of conductive medium. The organic combination of the two breaks the bottleneck that electroactive materials cannot be used in the biomedical field. Therefore, conductive hydrogel has a high application value in the field of medical devices.
[0003] Natural polymers are common hydrogel matrices, including gelatin, dextran, chitosan, hyaluronic acid and pectin. Dextran is a natural polysaccharide formed by dehydration polymerization of glucose. The three hydroxyl groups on each glucose unit are more conducive to the modification and modification of dextran. The modified dextran hydrogel has the advantages of low biological toxicity and good biodegradability.
[0004] Tetraaniline is a tetramer of aniline that can be linked to the main chain through covalent bonds. The linked polymer has good electrical activity and renal clearance, and is a material with broad application prospects.
[0005] The prior art (DOI: 10.1016 / j.biomaterials.2022.121479) uses silver nanowires (AgNW) and methacrylate alginate (MAA) to synthesize conductive hydrogels, and applies electrical stimulation to wounds, which can promote re-epithelialization, enhance angiogenesis, mediate immune responses, and prevent infection in the wound microenvironment. Although its conductivity is high, nanosilver has certain toxicity, and its distribution has uniformity problems. In order to solve the problem of uniform conductivity, patent CN108210940A provides a hydrogel that uses salt ions for conduction, but salt ion conduction may face the problem of long-term conduction; patent CN116675879A also provides an antibacterial conductive hydrogel, but its conductivity can only reach 0.29S / m at most, which is not suitable for scenarios requiring high conductivity gels; patent CN115820099A provides an antibacterial conductive hydrogel, but its antibacterial property is achieved by the release of iodine, and it is inevitable to encounter the toxicity that iodine itself may bring.
[0006] The existing technology (DOI: 10.1016 / j.cej.2022.141110) uses polyaniline-modified sodium hyaluronate and amino-modified sodium hyaluronate to form a conductive hydrogel through chemical cross-linking, but it does not have antibacterial properties and the maximum conductivity can only reach 6.21×10 -2 S / m.
[0007] The prior art (DOI: 10.1039 / C5RA19467A) uses polyaniline-modified gelatin, oxidized dextran and chitosan to form a conductive hydrogel through chemical crosslinking. Although it has antibacterial properties, its conductivity is less than 0.8 S / m. Summary of the invention
[0008] In order to solve the above technical problems, the first aspect of the present invention provides an in-situ cured two-component conductive hydrogel, comprising: polyaniline-oxidized polysaccharide, and polyamino polymer; both polyaniline-oxidized dextran and polyamino polymer are in the form of aqueous solution; the conductivity of the in-situ cured two-component conductive hydrogel is 1 to 4 S / m.
[0009] Preferably, the raw materials for preparing the polyaniline-oxidized polysaccharide include: polyaniline, an oxidant, and polysaccharide.
[0010] Preferably, the polysaccharide comprises: one of starch, dextran, hyaluronic acid, cellulose and sodium hyaluronate.
[0011] Further preferably, the polysaccharide comprises dextran.
[0012] Preferably, the oxidant includes one or more of sodium periodate, sodium hypochlorite, hydrogen peroxide, and potassium permanganate.
[0013] More preferably, the oxidant is sodium periodate.
[0014] More preferably, the mass ratio of the polysaccharide to the oxidant is 5:(1-8); as an implementable case, the mass ratio of the polysaccharide to the oxidant includes 5:1.32 or 5:6.6.
[0015] Preferably, the preparation method of the polyaniline-oxidized polysaccharide comprises: placing the polysaccharide in ice water and stirring to dissolve, then adding an oxidant, stirring and reacting at room temperature in the dark, and dialyzing in pure water to obtain the oxidized polysaccharide; dissolving the oxidized polysaccharide, then dropping the dissolved polyaniline into the oxidized polysaccharide, adjusting the system pH to 7-8, stirring and reacting at 50-60°C for 24-48h, then centrifuging, washing with pure water to obtain a supernatant, dialyzing in pure water, and freeze-drying to obtain the polysaccharide.
[0016] Further preferably, the preparation method of the polyaniline-oxidized polysaccharide comprises: placing 5g of polyglucan in 40mL of ice water and stirring to dissolve, then adding 1-8g of sodium periodate, stirring and reacting at room temperature of 25°C in a dark place for 4h, and dialyzing in pure water to obtain oxidized glucan; dissolving 1g of oxidized glucan in 10mL of water, and then dropping 10mL of polyaniline dissolved in DMSO into the oxidized polysaccharide, adjusting the system pH to 7.8, stirring and reacting at 60°C for 24h, then centrifuging and washing with pure water to obtain a supernatant, dialyzing in pure water for 3 days, and freeze-drying to obtain.
[0017] Dextran is a natural polysaccharide, which is formed by dehydration polymerization of glucose units and has good biocompatibility. The hydrogel using it as a raw material will not cause obvious rejection reaction in the body. The hydrogel can be completely biodegraded and has no toxic side effects. When used in the body, it can be gradually absorbed or excreted by the body over time, reducing the long-term impact on the body. The molecular structure of dextran contains a large number of hydroxyl groups, which are easy to react with other chemical groups, thereby realizing the modification and cross-linking of dextran; sodium periodate is used as an oxidant in the present invention, which can oxidize part of the hydroxyl groups (-OH) in the dextran molecule into aldehyde groups (-CHO), and the amount of the oxidant can be reasonably selected according to the degree of oxidation; the oxidized aldehyde group can react with the amino group in polyaniline to generate polyaniline-oxidized polysaccharide; because the main chain of the polyaniline molecule contains a large number of conjugated π electrons, these electrons are easy to move in the molecular chain, so polyaniline has a certain conductivity, and the corresponding polyaniline-oxidized polysaccharide can not only be used as a raw material for conductive hydrogel, but also can give the hydrogel a certain conductivity.
[0018] The polyamino polymer includes one or more of polylysine, polylysine hydrochloride, polyethyleneimine and chitosan quaternary ammonium salt.
[0019] As a natural antibacterial polypeptide, polylysine hydrochloride has broad-spectrum antibacterial properties against bacteria and fungi, and can be converted into essential amino acids for the human body. The preparation of hydrogels using it as a raw material is highly safe and has excellent antibacterial properties.
[0020] The polyethyleneimine molecular chain contains a large number of primary, secondary and tertiary amine groups. These groups carry positive charges and can effectively act on the cell membranes of Gram-positive and Gram-negative bacteria through "contact sterilization", causing the destruction of the bacterial membrane structure and thus killing the bacteria; however, it is difficult for polyethyleneimine and polyaniline-oxidized polysaccharides to form a hydrogel with a certain strength through chemical cross-linking. Therefore, in actual use, polyethyleneimine can be compounded with other polyamino polymers to prepare conductive hydrogels to ensure the mechanical properties and antibacterial properties of the conductive hydrogels.
[0021] Chitosan quaternary ammonium salt is a derivative of chitosan. By replacing the amino groups in chitosan with quaternary ammonium salt groups, its antibacterial properties are significantly improved. Chitosan quaternary ammonium salt has good biocompatibility and biodegradability, so it will not cause adverse reactions when in contact with organisms, and can be gradually degraded into non-toxic and harmless substances in the body. In addition, the addition of chitosan quaternary ammonium salt can further improve the physical and chemical properties of conductive hydrogels and expand the application range of in-situ cured two-component conductive hydrogels.
[0022] Preferably, the mass concentration of the polyaniline-oxidized polysaccharide in the polyaniline-oxidized polysaccharide aqueous solution is 0.25-10%.
[0023] Preferably, the mass concentration of the polyamino polymer in the polyamino polymer aqueous solution is 2.5-10%.
[0024] The second aspect of the present invention provides a method for preparing an in-situ cured two-component conductive hydrogel, comprising:
[0025] The polyaniline-oxidized polysaccharide and the polyamino polymer are dissolved, and mixed and solidified at the target site for 10s-20h through a double-mixed drug package combined with a needle or a nozzle or a double-lumen microcatheter to obtain the drug.
[0026] The third aspect of the present invention provides an application of an in-situ cured two-component conductive hydrogel, which is applied to intravascular gel electrode wires, antibacterial conductive dressings, and conductive gel sheets for defibrillators.
[0027] Beneficial Effects
[0028] (i) The in-situ cured two-component conductive hydrogel provided by the present invention has excellent conductive properties, and the conductivity of the conductive hydrogel can reach 1 to 4 S / m.
[0029] (ii) The raw materials of the in-situ cured two-component conductive hydrogel of the present invention include polyaniline-oxidized polysaccharide, so the conductive hydrogel provided by the present invention not only has the properties of a hydrogel, but also has the conductive properties of a conductive medium.
[0030] (III) The raw materials of the in-situ cured two-component conductive hydrogel of the present invention also include polyamino polymers, which can not only chemically cross-link with polyaniline-oxidized polysaccharide to form a gel network, but also give the conductive hydrogel excellent antibacterial properties.
[0031] (iv) The in-situ cured two-component conductive hydrogel provided by the present invention can be degraded at 37°C and is applied in the field of human treatment. It has high biosafety and is green and environmentally friendly.
[0032] (V) The present invention can reasonably adjust the curing performance and conductive performance of the conductive hydrogel by adjusting the oxidation degree of the polyaniline-oxidized polysaccharide and the mass concentration of the polyamino polymer in the polyamino polymer aqueous solution, thereby improving the application range of the conductive hydrogel. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 Schematic diagram of conductivity testing method.
[0034] Figure 2 Schematic diagram of the appearance of the in-situ cured two-component conductive hydrogel prepared in Example 4. DETAILED DESCRIPTION
[0035] The polyaniline-oxidized polysaccharide is polyaniline-oxidized dextran, including polyaniline-low-oxidized dextran and polyaniline-high-oxidized dextran.
[0036] 1. Preparation method of polyaniline-low-oxidized dextran:
[0037] Take 5g of dextran and dissolve it in 40mL of pure water, stir and dissolve it in an ice-water bath, then take another 1.32g of sodium periodate and add it to the solution in the ice-water bath, stir and react at room temperature at 25°C in a dark place for 4h, and dialyze in pure water to obtain oxidized dextran; weigh 1g of oxidized dextran and dissolve it in 10mL of water, then dissolve 1.5g of tetraaniline in 10mL of DMSO and add it dropwise to the oxidized dextran, adjust the pH value of the solution to 7.8, stir and react at 60°C for 24h, then centrifuge and wash with pure water to obtain the supernatant, dialyze in pure water for 3 days, and lyophilize to obtain polyaniline-low-oxidized dextran.
[0038] 2. Preparation method of polyaniline-highly oxidized dextran:
[0039] Take 5g of dextran and dissolve it in 40mL of pure water, stir and dissolve it in an ice-water bath, then take another 6.6g of sodium periodate and add it to the solution in the ice-water bath, stir and react at room temperature in the dark for 4h, and dialyze in pure water to obtain oxidized dextran; weigh 1g of oxidized dextran and dissolve it in 10mL of water, then dissolve 1.5g of tetraaniline in 10mL of DMSO and add it dropwise to the oxidized dextran, adjust the pH value of the solution to 7.8, stir and react at 60°C for 24h, then centrifuge and wash with pure water to obtain the supernatant, dialyze in pure water for 3 days, and obtain polyaniline-highly oxidized dextran after freeze-drying.
[0040] The dextran described in the present invention was purchased from Titan and has a molecular weight of 70,000.
[0041] The polyaniline was purchased from Titan and was a tetramer.
[0042] The molecular weight of the polylysine hydrochloride is 3000 and is purchased from Aladdin.
[0043] The polyethyleneimine was purchased from Titan, with a weight average molecular weight of 2000.
[0044] The chitosan quaternary ammonium salt was purchased from MacLean, with a degree of substitution of 98%.
[0045] Example 1
[0046] The first aspect of this example provides an in-situ cured two-component conductive hydrogel, comprising: polyaniline-low-oxidized dextran, and polyamino polymer polylysine hydrochloride; the polyaniline-low-oxidized dextran and the polyamino polymer are both in the form of aqueous solutions, with a volume ratio of 1:1; the mass concentration of the polyaniline-low-oxidized dextran aqueous solution is 10%, and the mass concentration of the polyamino polymer aqueous solution is 1%; the conductivity of the in-situ cured two-component conductive hydrogel is 1.27S / m.
[0047] The second aspect of the present invention provides a method for preparing an in-situ cured two-component conductive hydrogel, comprising:
[0048] The polyaniline-oxidized polysaccharide and the polyamino polymer are dissolved in pure water, and mixed and solidified at the target site by a double-mixing drug package combined with a needle for 10 hours to obtain the product.
[0049] The third aspect of the present invention provides an application of an in-situ cured two-component conductive hydrogel, which is applied in an intravascular gel electrode wire.
[0050] Example 2
[0051] This example provides an in-situ cured two-component conductive hydrogel, including: polyaniline-highly oxidized dextran, polyamino polymer polylysine hydrochloride; polyaniline-lowly oxidized dextran and polyamino polymer are both in the form of aqueous solution, with a volume ratio of 1:1, the mass concentration of the polyaniline-lowly oxidized dextran aqueous solution is 10%, and the mass concentration of the polyamino polymer aqueous solution is 1%; the conductivity of the in-situ cured two-component conductive hydrogel is 2.00S / m.
[0052] Example 3
[0053] This example provides an in-situ cured two-component conductive hydrogel, comprising: polyaniline-low-oxidized dextran, and polyamino polymer polylysine hydrochloride; both polyaniline-low-oxidized dextran and polyamino polymer are in the form of aqueous solution, with a volume ratio of 1:1; the mass concentration of the polyaniline-low-oxidized dextran aqueous solution is 10%, and the mass concentration of the polyamino polymer aqueous solution is 20%; the conductivity of the in-situ cured two-component conductive hydrogel is 1.96S / m.
[0054] Example 4
[0055] This example provides an in-situ cured two-component conductive hydrogel, comprising: polyaniline-highly oxidized dextran, and polyamino polymer polylysine hydrochloride; polyaniline-highly oxidized dextran and polyamino polymer are both in the form of aqueous solutions, with a volume ratio of 1:1; the mass concentration of the polyaniline-highly oxidized dextran aqueous solution is 10%, and the mass concentration of the polyamino polymer aqueous solution is 20%; the conductivity of the in-situ cured two-component conductive hydrogel is 3.17S / m.
[0056] The schematic diagram of the in-situ cured two-component conductive hydrogel prepared in this example is as follows: Figure 2 shown.
[0057] Example 5
[0058] This example provides an in-situ cured two-component conductive hydrogel, including: polyaniline-high oxidized dextran, polyamino polymer polyethyleneimine; polyaniline-high oxidized dextran and polyamino polymer are both in the form of aqueous solution, with a volume ratio of 1:1; the mass concentration of the polyaniline-high oxidized dextran aqueous solution is 10%, and the mass concentration of the polyamino polymer aqueous solution is 1%; the hydrogel cannot be cured and formed normally.
[0059] Example 6
[0060] This example provides an in-situ cured two-component conductive hydrogel, comprising: polyaniline-highly oxidized dextran, and polyamino polymer chitosan quaternary ammonium salt; polyaniline-highly oxidized dextran and polyamino polymer are both in the form of aqueous solution, with a volume ratio of 1:1; the mass concentration of the polyaniline-highly oxidized dextran aqueous solution is 10%, and the mass concentration of the polyamino polymer aqueous solution is 5%; the conductivity of the in-situ cured two-component conductive hydrogel is 3.42S / m.
[0061] Example 7
[0062] This example provides an in-situ cured two-component conductive hydrogel, comprising: polyaniline-highly oxidized dextran and polyamino polymer, the polyamino polymer comprising chitosan quaternary ammonium salt and polylysine hydrochloride; polyaniline-highly oxidized dextran and polyamino polymer are both in the form of aqueous solution, with a volume ratio of 1:1; the mass concentration of the polyaniline-highly oxidized dextran aqueous solution is 10%; the mass concentration of the chitosan quaternary ammonium salt in the polyamino polymer aqueous solution is 2.5%, and the mass concentration of the polylysine hydrochloride is 10%; the conductivity of the in-situ cured two-component conductive hydrogel is 3.37S / m.
[0063] Example 8
[0064] This example provides an in-situ cured two-component conductive hydrogel, comprising: polyaniline-highly oxidized dextran and polyamino polymer, the polyamino polymer comprising polyethyleneimine and polylysine hydrochloride; the polyaniline-highly oxidized dextran and the polyamino polymer are both in the form of aqueous solution, with a volume ratio of 1:1; the mass concentration of the polyaniline-highly oxidized dextran aqueous solution is 10%, the mass concentration of polyethyleneimine in the polyamino polymer aqueous solution is 2.5%, and the mass concentration of polylysine hydrochloride is 10%; the conductivity of the in-situ cured two-component conductive hydrogel is 3.37S / m.
[0065] Example 9
[0066] Pure water was used to prepare solutions of 10% oxidized dextran, 10% polyaniline-highly oxidized dextran, 5% polyethyleneimine, and 5% polylysine, and the conductivity of the solutions was tested with a conductivity tester. The test results are shown in Table 1.
[0067] Table 1
[0068]
[0069]
[0070] Performance Testing
[0071] Test object: the in-situ cured two-component conductive hydrogel prepared in Examples 1-8. The test results are shown in Table 2.
[0072] Test items and methods:
[0073] 1. 60℃ degradation collection: The prepared hydrogel was immersed in 10 times the mass of PBS solution and placed in a 60℃ oven for accelerated degradation experiment. The gel morphology was observed daily and the time of complete gel degradation was recorded.
[0074] 2. 37°C degradation collection: The prepared hydrogel was immersed in 10 times the mass of PBS solution and placed in a 37°C water bath shaker for degradation experiment. The gel morphology was observed every week and the time of complete degradation of the gel was recorded.
[0075] 3. Test method for curing time: Place polyaniline-highly oxidized dextran, polyamino polymer and 2.5mL vial in a 37±0.5℃ water bath. After standing for 5 minutes, use a pipette to take polyaniline-highly oxidized dextran into a 2.5mL vial. Then use another pipette tip to take 200μL of polyamino polymer and add it to the vial containing polyaniline-highly oxidized dextran. Vibrate the vial for 1s by shaking the wrist, then repeatedly tilt the vial to observe until the liquid stops flowing. Start timing at the same time as adding polyamino polymer, and end timing when the liquid stops flowing. The timing duration is the curing time.
[0076] IV. Antibacterial test: Refer to Section 5.1.4 of "WST650-2019 Antibacterial and Antibacterial Effect Evaluation Method" and set the concentration to 5×10 5 to 5×10 6 CFU / mL of Staphylococcus aureus was smeared on the culture medium, and then the conductive hydrogel was prepared into a cylinder with a diameter of 5 mm and inoculated on the culture medium. After culturing for 16-18 hours, the diameter of the formed antibacterial ring was observed.
[0077] 5. Conductivity test method:
[0078] 1. Use a vernier caliper to measure the diameter and length of the sample;
[0079] 2. Connect the sample to be tested in series with a known resistor, and test the voltage across the known resistor and the voltage across the sample to be tested respectively. According to the voltage across the known resistor = the resistance of the sample to be tested: the known resistance, calculate the resistance of the sample to be tested, such as Figure 1 described.
[0080] 3. According to the formula:
[0081]
[0082] Conductance = 1 / resistance
[0083] Calculate the conductivity of the conductive hydrogel.
[0084] Taking Example 1 as an example, the results are shown in Table 2.
[0085] Table 2
[0086] Sample length 0.02m Known resistance value 200000Ω Sample interface radius 0.0015m Known resistor voltage divider 14.36V Voltage across the sample 0.16V Resistance value of the sample to be tested 2228.41Ω
[0087]
[0088] The test results of all the above test items are detailed in Table 3.
[0089] Table 3
[0090]
[0091] The “ / ” indicates not tested.
[0092] Comparative Example 1 and Example 2 show that the high aldehyde density dextran can couple more polyaniline, and the conductivity of the conductive hydrogel formed is also higher. Comparative Example 1 / Example 3 and Example 2 / Example 4 show that the concentration of the polyamino polymer-polylysine hydrochloride of the cross-linking agent is improved, which can improve the conductivity of the conductive hydrogel. From Examples 4, 6, and 7, it can be seen that the conductivity of the conductive hydrogel formed by chitosan quaternary ammonium salt and polylysine hydrochloride as cross-linking agents is higher. From the antibacterial experimental results, it can be seen that polylysine hydrochloride and chitosan quaternary ammonium salt all have stronger antibacterial property. From all embodiments, the swelling rate of conductive hydrogel is generally lower, particularly high-oxidation dextran samples, which may be because the polyaniline modification rate is higher, giving the conductive hydrogel higher hydrophobicity.
Claims
1. An in-situ cured two-component conductive hydrogel, characterized in that: include: Polyaniline-oxidized polysaccharide, polyamino polymer; polyaniline-oxidized dextran and polyamino polymer are both in the form of aqueous solution; the conductivity of the in-situ cured two-component conductive hydrogel is 1-4S / m.
2. The in-situ cured two-component conductive hydrogel according to claim 1, characterized in that: The raw materials for preparing the polyaniline-oxidized polysaccharide include: polyaniline, oxidant and polysaccharide.
3. The in-situ cured two-component conductive hydrogel according to claim 2, characterized in that: The polysaccharide comprises: one of starch, dextran, hyaluronic acid, cellulose and sodium hyaluronate.
4. The in-situ cured two-component conductive hydrogel according to claim 2, characterized in that: The oxidant includes one or more of sodium periodate, sodium hypochlorite, hydrogen peroxide and potassium permanganate.
5. The in-situ cured two-component conductive hydrogel according to claim 2, characterized in that: The mass ratio of the polysaccharide to the oxidant is 5:(1-8).
6. The in-situ cured two-component conductive hydrogel according to claim 2, characterized in that: The preparation method of the polyaniline-oxidized polysaccharide comprises: placing the polysaccharide in ice water and stirring to dissolve, then adding an oxidant, stirring and reacting at room temperature in the dark, and dialyzing in pure water to obtain the oxidized polysaccharide; dissolving the oxidized polysaccharide, then dripping the dissolved polyaniline into the oxidized polysaccharide, adjusting the system pH to 7-8, stirring and reacting at 50-60°C for 24-48h, then centrifuging, washing with pure water to obtain a supernatant, dialyzing in pure water, and freeze-drying to obtain the polyaniline-oxidized polysaccharide.
7. The in-situ cured two-component conductive hydrogel according to claim 1, characterized in that: The polyamino polymer includes one or more of polylysine hydrochloride, polyethyleneimine and chitosan quaternary ammonium salt.
8. The in-situ cured two-component conductive hydrogel according to claim 1, characterized in that: The mass concentration of the polyamino polymer in the polyamino polymer aqueous solution is 2.5-10%.
9. A method for preparing an in-situ cured two-component conductive hydrogel according to any one of claims 1 to 8, characterized in that: include: The polyaniline-oxidized polysaccharide and the polyamino polymer are dissolved, and mixed and solidified at the target site for 10s-20h through a double-mixed drug package combined with a needle or a nozzle or a double-lumen microcatheter to obtain the drug.
10. An application of the in-situ cured two-component conductive hydrogel according to any one of claims 1 to 8, characterized in that: It is used in intravascular gel electrode wires, antibacterial conductive dressings, and conductive gel sheets for defibrillators.