Preparation method and application of space-irradiation-resistant polyimide-mica nanosheet composite interlayer material

By coating mica nanosheets on the upper and lower surfaces of the polyimide intermediate layer, the polyimide-mica nanosheet composite interlayer material is formed, and the deterioration problem of single polyimide under the action of high-energy particles is solved and the material is improved The breakdown and dielectric properties of the company have expanded its application range and are suitable for industrial production.

CN119019729AInactive Publication Date: 2024-11-26HARBIN UNIV OF SCI & TECH
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411284541.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

As a protective material for satellite-borne electronic components, single polyimide is easily deteriorated under the action of high-energy particles, resulting in the operation of electronic components being affected.

Method used

Using polyimide-mica nanosheet composite interlayer material, the polyimide-mica nanosheet composite layer is coated on the upper and lower surfaces of the polyimide intermediate layer, and the mica nanosheets account for 0.2 mass fraction of the polyimide nanosheets %, 0.4%, 0.6% or 0.8%, and ball milling, ultrasonic, centrifugation and curing are carried out through specific preparation processes to form a composite material that is resistant to space irradiation.

Benefits of technology

Improve the breakdown and dielectric properties of polyimide materials, maintain good interface compatibility, broaden its application range in aerospace and other fields, and maintains excellent performance after a variety of irradiation treatments. It is suitable for 大规模工业化生产。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019729A_ABST
    Figure CN119019729A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a space-irradiation-resistant polyimide-mica nanosheet composite interlayer material, and relates to the technical field of polyimide composite films. The invention aims to solve the problem that when single polyimide is used as a satellite-borne electronic component protection material in the prior art, the normal operation of electronic components is affected due to the fact that polyimide is easy to degrade. According to the invention, a polyimide matrix doped mica nanosheet is used as an outer layer, and a pure polyimide film is used as a middle layer. As a high-performance flexible insulating layer, the polyimide film with the interlayer structure has huge application potential in the fields of microelectronics, 5G communication, aerospace and the like. The invention can obtain the preparation method and application of the polyimide-mica nanosheet composite interlayer material capable of resisting space irradiation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyimide composite films, and in particular to a preparation method and application of a space radiation-resistant polyimide-mica nanosheet composite sandwich material. Background Art

[0002] In recent years, with the rapid development of my country's aerospace industry, higher requirements have been put forward for the performance of spacecraft-related materials. Various high-energy charged particle radiations in geosynchronous orbit, such as high-energy electron radiation, ultraviolet radiation and atomic oxygen radiation, will cause a certain degree of damage to the running spacecraft equipment. The development of radiation-proof composite materials with good insulation performance and light weight can greatly improve the on-orbit operation life of satellite-borne electronic components. Based on this, polyimide (PI) with a highly conjugated benzene ring structure has been widely used in the aerospace industry due to its excellent anti-aging, high temperature resistance and electrical insulation properties. However, polyimide, as a commonly used protective material for satellite-borne electronic components, will not only be degraded by polyimide itself, but also affect the normal operation of the electronic components it shields once it produces charge deposition under the action of high-energy particles, thus causing charging and discharging. Therefore, it is necessary to study the protective modification of polyimide in space radiation environment. Summary of the invention

[0003] The purpose of the present invention is to solve the problem that when single polyimide is used as a protective material for space-borne electronic components in the past, the normal operation of the electronic components is affected because the polyimide itself is easily degraded, and a preparation method and application of a polyimide-mica nanosheet composite sandwich material that is resistant to space radiation is provided.

[0004] A space radiation resistant polyimide-mica nanosheet composite sandwich material comprises a polyimide middle layer and a polyimide-mica nanosheet composite layer coated on the upper and lower surfaces of the polyimide middle layer, wherein the mass fraction of mica nanosheets in the polyimide-mica nanosheet composite layer is 0.2%, 0.4%, 0.6% or 0.8%.

[0005] A method for preparing a space radiation resistant polyimide-mica nanosheet composite sandwich material is carried out according to the following steps:

[0006] Step S1: peeling off mica nanosheets;

[0007] Mixing dry mica powder and lithium chloride, adding methanol and placing in a planetary ball mill, and fully ball milling to obtain a mixed solution a; washing and drying the mixed solution a, adding isopropanol solution, and stirring evenly to obtain a mixed solution b; firstly subjecting the mixed solution b to ultrasonication, and then subjecting it to two-step centrifugation to obtain a mica nanosheet precipitate; washing the mica nanosheet precipitate and freeze-drying it to obtain a mica nanosheet;

[0008] Step S2: preparing a polyimide-mica nanosheet composite sandwich material;

[0009] 4,4'-diaminodiphenyl ether is added to N,N-dimethylacetamide solution, and ultrasonically dispersed to obtain a mixed solution c; the mixed solution c is divided into two parts, and the mica nanosheets obtained in step S1 are added to one of the mixed solutions c, and mixed evenly to obtain a mixed solution d; two equal parts of pyromellitic anhydride are added to the other mixed solution c and the mixed solution d, respectively, and mechanically stirred until viscous to obtain mixed solutions e and f; the mixed solution e and the mixed solution f are evacuated respectively, and then the mixed solution f is evenly coated on one surface of the pretreated glass substrate, and the mixed solution e is evenly coated after solidification, and the mixed solution f is evenly coated after solidification again, and the substrate is gradually heated to 350°C after further solidification, and is kept at 350°C for 50 to 70 minutes; after the insulation is completed, it is cooled to room temperature, and the film on the substrate is peeled off to obtain a polyimide-mica nanosheet composite interlayer material resistant to space radiation.

[0010] The invention discloses an application of a polyimide-mica nanosheet composite sandwich material resistant to space radiation, and an application of the polyimide-mica nanosheet composite sandwich material resistant to space radiation in the preparation of space radiation shielding materials.

[0011] Beneficial effects of the present invention:

[0012] (1) The present invention provides a method for preparing a polyimide-mica nanosheet composite sandwich material, which innovatively uses a polyimide matrix doped with mica nanosheets as the outer layer, and a pure polyimide film as the middle layer. The sandwich structure polyimide (PI) film, as a high-performance flexible insulating layer, will show great application potential in the fields of microelectronics, 5G communications, and aerospace; at the same time, it effectively utilizes the advantages of mica in electrical, mechanical, and radiation properties, and maintains good interface compatibility. On the basis of maintaining the original performance of polyimide, it further broadens its application range in the fields of aerospace and the like.

[0013] (2) The polyimide-mica nanosheet composite interlayer material prepared by the process of the present invention has improved breakdown and dielectric properties compared to pure polyimide, and can still maintain excellent performance after various irradiation treatments, and can be widely used in advanced fields such as electrical, electronic, and aerospace.

[0014] (3) The preparation process of the present invention is simple, economical and practical, effectively saves resources, is suitable for large-scale industrial production, and provides a good strategy for developing new application paths for polyimide insulating composite dielectrics.

[0015] The invention can obtain a preparation method and application of a polyimide-mica nanosheet composite sandwich material resistant to space radiation. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The SEM image of the polyimide-mica nanosheet composite sandwich material prepared in Example 1 is shown;

[0017] Figure 2 The figure represents the DC breakdown Weibull distribution result of the polyimide-mica nanosheet composite sandwich material (without irradiation treatment) prepared by using mica nanosheets with different mass fractions of the present invention, ■ represents a pure polyimide-based film, ● represents a mica nanosheet with a mass fraction of 0.2%, ▲ represents a mica nanosheet with a mass fraction of 0.4%, ▼ represents a mica nanosheet with a mass fraction of 0.6%, and ◆ represents a mica nanosheet with a mass fraction of 0.8%;

[0018] Figure 3 The figure represents the DC breakdown Weibull distribution result of the polyimide-mica nanosheet composite sandwich material (irradiated with ultraviolet light for 9 days) prepared by using mica nanosheets with different mass fractions of the present invention, ■ represents a pure polyimide-based film, ● represents a mica nanosheet with a mass fraction of 0.2%, ▲ represents a mica nanosheet with a mass fraction of 0.4%, ▼ represents a mica nanosheet with a mass fraction of 0.6%, and ◆ represents a mica nanosheet with a mass fraction of 0.8%;

[0019] Figure 4 The polyimide-mica nanosheet composite sandwich material prepared by the present invention using mica nanosheets with different mass fractions (irradiated with 1 MeV electrons at 7.0 × 10 15 e / cm 2 ), ■ represents pure polyimide-based film, ● represents mica nanosheets with a mass fraction of 0.2%, ▲ represents mica nanosheets with a mass fraction of 0.4%, ▼ represents mica nanosheets with a mass fraction of 0.6%, and ◆ represents mica nanosheets with a mass fraction of 0.8%;

[0020] Figure 5 A graph showing the dielectric constant test results of the polyimide-mica nanosheet composite sandwich material prepared by using mica nanosheets with different mass fractions of the present invention, wherein ■ represents a pure polyimide-based film, ● represents a mica nanosheet with a mass fraction of 0.2%, ▲ represents a mica nanosheet with a mass fraction of 0.4%, ▼ represents a mica nanosheet with a mass fraction of 0.6%, and ◆ represents a mica nanosheet with a mass fraction of 0.8%;

[0021] Figure 6A graph showing dielectric loss test results of a polyimide-mica nanosheet composite sandwich material prepared by using mica nanosheets with different mass fractions of the present invention, wherein ■ represents a pure polyimide-based film, ● represents a mica nanosheet with a mass fraction of 0.2%, ▲ represents a mica nanosheet with a mass fraction of 0.4%, ▼ represents a mica nanosheet with a mass fraction of 0.6%, and ◆ represents a mica nanosheet with a mass fraction of 0.8%;

[0022] Figure 7 The figure represents the Fourier infrared spectrum characterization result of the polyimide-mica nanosheet composite interlayer material prepared by the present invention using mica nanosheets with different mass fractions, A represents a pure polyimide-based composite film, B represents a mica nanosheet with a mass fraction of 0.2%, C represents a mica nanosheet with a mass fraction of 0.4%, D represents a mica nanosheet with a mass fraction of 0.6%, and E represents a mica nanosheet with a mass fraction of 0.8%. DETAILED DESCRIPTION

[0023] Specific implementation method 1: This implementation method is a space radiation resistant polyimide-mica nanosheet composite sandwich material, which is composed of a polyimide intermediate layer and a polyimide-mica nanosheet composite layer coated on the upper and lower surfaces of the polyimide intermediate layer. The mass fraction of mica nanosheets in the polyimide-mica nanosheet composite layer is 0.2%, 0.4%, 0.6% or 0.8%.

[0024] Specific implementation method 2: This implementation method is a method for preparing a polyimide-mica nanosheet composite sandwich material resistant to space radiation, which is carried out according to the following steps:

[0025] Step S1: peeling off mica nanosheets;

[0026] Mixing dry mica powder and lithium chloride, adding methanol and placing in a planetary ball mill, and fully ball milling to obtain a mixed solution a; washing and drying the mixed solution a, adding isopropanol solution, and stirring evenly to obtain a mixed solution b; firstly subjecting the mixed solution b to ultrasonication, and then subjecting it to two-step centrifugation to obtain a mica nanosheet precipitate; washing the mica nanosheet precipitate and freeze-drying it to obtain a mica nanosheet;

[0027] Step S2: preparing a polyimide-mica nanosheet composite sandwich material;

[0028] 4,4'-diaminodiphenyl ether is added to N,N-dimethylacetamide solution, and ultrasonically dispersed to obtain a mixed solution c; the mixed solution c is divided into two parts, and the mica nanosheets obtained in step S1 are added to one of the mixed solutions c, and mixed evenly to obtain a mixed solution d; two equal parts of pyromellitic anhydride are added to the other mixed solution c and the mixed solution d, respectively, and mechanically stirred until viscous to obtain mixed solutions e and f; the mixed solution e and the mixed solution f are evacuated respectively, and then the mixed solution f is evenly coated on one surface of the pretreated glass substrate, and the mixed solution e is evenly coated after solidification, and the mixed solution f is evenly coated after solidification again, and the substrate is gradually heated to 350°C after further solidification, and is kept at 350°C for 50 to 70 minutes; after the insulation is completed, it is cooled to room temperature, and the film on the substrate is peeled off to obtain a polyimide-mica nanosheet composite interlayer material resistant to space radiation.

[0029] Specific implementation method three: The difference between this implementation method and specific implementation method one or two is that: the ratio of the mass of the dry mica powder, the mass of lithium chloride and the volume of methanol described in step S1 is (4.9~5.1) g: (4.9~5.1) g: (5~15) mL; the ratio of the mass of the mixed solution a after washing and drying in step S1 to the volume of the isopropanol solution is (0.45~0.55) g: (340~360) mL.

[0030] The other steps are the same as those in the first or second embodiment.

[0031] Specific implementation mode four: The difference between this implementation mode and specific implementation modes one to three is that: the ball milling time in step S1 is 8 to 12 hours; the two-step centrifugation in step S1 is: first, the mixed solution b after ultrasound is centrifuged at a speed of 1800 to 2000 rpm for 19 to 21 minutes, and the obtained supernatant is centrifuged again at a speed of 8000 to 9000 rpm for 8 to 10 minutes; in step S1, the mica nanosheet precipitate is washed 3 to 5 times with deionized water.

[0032] The other steps are the same as those in Specific Embodiments 1 to 3.

[0033] Specific embodiment 5: The difference between this embodiment and specific embodiments 1 to 4 is that the ratio of the mass of 4,4'-diaminodiphenyl ether described in step S2, the volume of N,N-dimethylacetamide solution and the total mass of pyromellitic dianhydride is (2.9-3.1) g: (39.5-40.5) mL: (3.27-3.29) g.

[0034] The other steps are the same as those in Specific Embodiments 1 to 4.

[0035] Specific embodiment six: The difference between this embodiment and specific embodiments one to five is that the time of ultrasonic dispersion in step S2 is 15 to 45 minutes; the time of mechanical stirring in step S2 is 3 to 5 hours; the temperature of the three curings in step S2 is 79 to 81°C, the time of the first two curings is 30 to 40 minutes, and the time of the third curing is 8 to 12 hours.

[0036] The other steps are the same as those in Specific Embodiments 1 to 5.

[0037] Specific embodiment seven: The difference between this embodiment and any one of specific embodiments one to six is ​​that before adding isophthalic anhydride to another mixed solution c and mixed solution d in step S2, it is first dried in a vacuum environment at 60°C for 7 to 9 hours; after the insulation in step S2 is completed, the substrate is first immersed in deionized water for 10 to 15 minutes, and then the film on the substrate is peeled off.

[0038] The other steps are the same as those in Specific Embodiments 1 to 6.

[0039] Specific embodiment eight: The difference between this embodiment and specific embodiments one to seven is that the pretreated glass substrate described in step S2 is processed according to the following steps: first, the substrate is cleaned with clean water for 1 to 3 times, then rinsed with deionized water for 3 to 5 times, and then cleaned with anhydrous ethanol for 3 to 5 times, and finally dried at 50 to 60°C for 45 to 75 minutes to obtain a pretreated substrate, which is a glass plate.

[0040] The other steps are the same as those in Specific Embodiments 1 to 7.

[0041] Specific embodiment nine: The difference between this embodiment and specific embodiments one to eight is that: in step S2, pyromellitic anhydride is added to another mixed solution c and mixed solution d in four times, 1 / 2 of the total mass is added for the first time, 1 / 4 of the total mass is added for the second time, 1 / 8 of the total mass is added for the third and fourth times, and the interval time of the four additions is 25 to 35 minutes; the gradient heating described in step S2 is to first place the substrate in a blast oven and heat it to 80 to 82°C, and keep it at 80 to 82°C for 8 to 12 hours; then heat it to 109 to 111°C, 139 to 141°C, 169 to 171°C, 199 to 201°C, 229 to 231°C, 259 to 261°C, 289 to 291°C and 319 to 321°C in sequence, and keep it for 25 to 35 minutes; finally heat it to 350°C.

[0042] The other steps are the same as those in Specific Embodiments 1 to 8.

[0043] Specific implementation method ten: This implementation method provides an application of a polyimide-mica nanosheet composite sandwich material that is resistant to space radiation, and the application of the polyimide-mica nanosheet composite sandwich material that is resistant to space radiation in the preparation of space radiation shielding materials.

[0044] The following examples are used to verify the beneficial effects of the present invention:

[0045] Example 1: A method for preparing a space radiation resistant polyimide-mica nanosheet composite sandwich material, comprising the following steps:

[0046] Step S1: peeling off mica nanosheets;

[0047] 5 g of dry mica powder was mixed with 5 g of lithium chloride, 10 mL of methanol was added, and the mixture was placed in a planetary ball mill for 8 h. After sufficient ball milling, a mixed solution a was obtained; after washing and drying the mixed solution a, 350 mL of isopropanol solution was added, and the mixture was stirred evenly to obtain a mixed solution b; the mixed solution b was first subjected to ultrasound, and then centrifuged at a speed of 2000 rpm for 20 min, and the obtained supernatant was centrifuged again at a speed of 8700 rpm for 8 min to obtain a mica nanosheet precipitate; the mica nanosheet precipitate was washed 3 times with deionized water, and then freeze-dried to obtain a mica nanosheet;

[0048] Step S2: preparing a polyimide-mica nanosheet composite sandwich material;

[0049] 3 g of 4,4'-diaminodiphenyl ether was added to 40 mL of N,N-dimethylacetamide solution, and ultrasonically dispersed for 30 min to obtain a mixed solution c; the mixed solution c was divided into two parts, and the mica nanosheets obtained in step S1 were added to one of the mixed solutions c, and mixed evenly to obtain a mixed solution d; two equal parts of pyromellitic dianhydride (total amount of 3.28 g) were first dried under a vacuum environment of 60° C. for 7 h, and then added to the other mixed solution c and the mixed solution d respectively, and mechanically stirred for 3 h until viscous, to obtain mixed solutions e and f; the mixed solutions e and f were evacuated respectively, and then the mixed solution f was evenly coated on one surface of the pretreated glass substrate, and then the mixed solution e was evenly coated after curing at 80° C. for 30 min, and then After curing at 80°C for 30 minutes, the mixed solution f is evenly coated, and after continuing to cure at 80°C for 8 hours, the substrate is placed in a blast oven, and then heated to 110°C, 140°C, 170°C, 200°C, 230°C, 260°C, 290°C and 320°C in sequence, and kept warm for 30 minutes; finally, it is heated to 350°C and kept warm at 350°C for 60 minutes; after the insulation, the substrate is first immersed in deionized water for 15 minutes, and then the film on the substrate is peeled off to obtain a polyimide-mica nanosheet composite sandwich material resistant to space radiation; the mass fraction of mica nanosheets in the polyimide in the polyimide-mica nanosheet composite sandwich material resistant to space radiation is 0.2%.

[0050] The pretreated glass substrate described in step S2 is processed according to the following steps: first prepare a glass plate with a size of 200 mm×16 mm×4 mm, and before use, wash the glass plate with clean water for 3 times, then rinse with deionized water for 5 times, and then wash with anhydrous ethanol for 5 times, and finally dry at 60°C for 60 minutes to obtain a pretreated glass plate.

[0051] In step S2, pyromellitic anhydride is added to another mixed solution c and mixed solution d in four times, the first time adding 1 / 2 of the total mass, the second time adding 1 / 4 of the total mass, the third and fourth times adding 1 / 8 of the total mass, and the interval time of the four additions is 30 minutes.

[0052] Example 2: In the polyimide-mica nanosheet composite sandwich material, the mass fraction of mica nanosheets in the polyimide is 0.4%. Other experimental conditions are the same as those in Example 1.

[0053] Example 3: In the polyimide-mica nanosheet composite sandwich material in the example, the mass fraction of mica nanosheets in the polyimide is 0.6%. Other experimental conditions are the same as those in Example 1.

[0054] Example 4: In the polyimide-mica nanosheet composite sandwich material, the mass fraction of mica nanosheets in the polyimide is 0.8%. Other experimental conditions are the same as those in Example 1.

[0055] Comparative Example 1: In this comparative example, step S1 is not performed, and mica nanosheets are not added in step S2. Other experimental conditions are the same as those in Example 1.

[0056] Figure 1 : represents the SEM image of the polyimide-mica nanosheet composite sandwich material prepared in Example 1; Figure 1 As shown, the peeled mica nanosheets are evenly dispersed on the upper and lower surfaces of the polyimide-mica nanosheet composite sandwich material, and because the matrix of the outer layer and the inner layer are both polyimide, the interface compatibility is good and no obvious stratification occurs.

[0057] Figure 2 The diagram shows the DC breakdown Weibull distribution results of the polyimide-mica nanosheet composite sandwich material (without irradiation treatment) prepared by using mica nanosheets with different mass fractions in the present invention, Figure 3 The diagram shows the DC breakdown Weibull distribution results of the polyimide-mica nanosheet composite sandwich material (irradiated with ultraviolet light for 9 days) prepared by using mica nanosheets with different mass fractions in the present invention, Figure 4 The polyimide-mica nanosheet composite sandwich material prepared by the present invention using mica nanosheets with different mass fractions (irradiated with 1 MeV electrons at 7.0 × 10 15 e / cm 2 ), ■ represents pure polyimide-based film, ● represents mica nanosheets with a mass fraction of 0.2%, ▲ represents mica nanosheets with a mass fraction of 0.4%, ▼ represents mica nanosheets with a mass fraction of 0.6%, and ◆ represents mica nanosheets with a mass fraction of 0.8%.

[0058] like Figure 2-4 As shown in the figure, when not irradiated, as the mass fraction of mica nanosheets increases, the breakdown field strength first increases and then decreases. The breakdown field strength of pure polyimide is 513 kV / mm. When the mass fraction of mica nanosheets is 0.6%, the breakdown field strength reaches the maximum value of 657 kV / mm. However, with ultraviolet irradiation for 9 days and 1 MeV electron irradiation for 7.0×10 15 e / cm 2After the irradiation, the breakdown field strength of the pure polyimide film dropped to 327kV / mm and 408kV / mm, respectively, while the polyimide-mica nanosheet composite sandwich material with a mass fraction of 0.6% mica nanosheets only slightly dropped to 620kV / mm and 610kV / mm due to its excellent radiation shielding performance. This shows that with the addition of inorganic filler mica nanosheets with good insulation and radiation resistance, the breakdown field strength of the polyimide-mica nanosheet composite sandwich material has not only been intrinsically improved, but also has a strong space radiation shielding performance.

[0059] Figure 5 The dielectric constant test results of the polyimide-mica nanosheet composite sandwich material prepared by the present invention using different mass fractions of mica nanosheets are shown in the figure, ■ represents a pure polyimide-based film, ● represents a mica nanosheet with a mass fraction of 0.2%, ▲ represents a mica nanosheet with a mass fraction of 0.4%, ▼ represents a mica nanosheet with a mass fraction of 0.6%, and ◆ represents a mica nanosheet with a mass fraction of 0.8%. Figure 5 As shown in the figure, at a frequency of 100 Hz, with the increase of the mass fraction of mica nanosheets, the dielectric constant shows an increasing trend. When the mass fraction of mica nanosheets is 0.8%, the dielectric constant reaches a maximum of 3.44.

[0060] Figure 6 A graph showing the dielectric loss test results of the polyimide-mica nanosheet composite interlayer material prepared by the present invention using mica nanosheets with different mass fractions, wherein ■ represents a pure polyimide-based film, ● represents a mica nanosheet with a mass fraction of 0.2%, ▲ represents a mica nanosheet with a mass fraction of 0.4%, ▼ represents a mica nanosheet with a mass fraction of 0.6%, and ◆ represents a mica nanosheet with a mass fraction of 0.8%.

[0061] like Figure 6 As shown in the figure, with the increase of the mass fraction of mica nanosheets, the dielectric loss satisfies the trend of first decreasing and then rising. In the low frequency band, the inhibitory effect of mica nanosheets on dielectric loss is not obvious; while in the high frequency band, the introduction of mica nanosheets induces space charge polarization and inhibits the orientation polarization of polymer chains to a certain extent. In addition, the interface polarization between the interlayer films also plays a role to a certain extent. The combined effect of multiple polarization behaviors significantly reduces the dielectric loss of the composite film.

[0062] Figure 7The figure represents the Fourier infrared spectrum characterization result of the polyimide-mica nanosheet composite interlayer material prepared by the present invention using mica nanosheets with different mass fractions, A represents a pure polyimide-based composite film, B represents a mica nanosheet with a mass fraction of 0.2%, C represents a mica nanosheet with a mass fraction of 0.4%, D represents a mica nanosheet with a mass fraction of 0.6%, and E represents a mica nanosheet with a mass fraction of 0.8%.

[0063] like Figure 7 As shown in the figure, the polyimide-mica nanosheet composite sandwich materials prepared with different mass fractions of mica nanosheets have a wavelength of 2930 cm -1 and 3745cm -1 The characteristic absorption peaks of COOH and NH in PAA were not present at all, which clearly indicated that the thermal imidization reaction was basically completed in the film. By comparing the infrared absorption peak positions of polyimide-mica nanosheet composite sandwich materials prepared with different mass fractions of mica nanosheets, it was found that the increase in the content of mica nanosheets did not lead to significant changes in the characteristic peaks of the composite film, among which the film at 725cm -1 、1080cm -1 、1230cm -1 、1380cm -1 、1720cm -1 and 1780cm -1 Obvious absorption peaks appeared at the same wave number positions, which corresponded to the C=O bending vibration in the imide ring, the symmetric and asymmetric stretching vibration of COC, the CN stretching vibration, and the symmetric and asymmetric stretching vibration of the C=O bond, indicating that the introduction of mica nanosheets did not change the polyimide matrix itself. However, when the intensity of the above characteristic peaks was further compared, many characteristic peaks showed lower intensities when the content of mica nanosheets increased, which reflected that the addition of mica nanosheets may have weakened the effectiveness of these chemical bonds to a certain extent, which may be closely related to the presence of Si-O and other stretching vibration peaks in mica nanosheets.

Claims

1. A space radiation resistant polyimide-mica nanosheet composite sandwich material, characterized in that The space radiation resistant polyimide-mica nanosheet composite sandwich material consists of a polyimide middle layer and a polyimide-mica nanosheet composite layer coated on the upper and lower surfaces of the polyimide middle layer. The mass fraction of mica nanosheets in the polyimide-mica nanosheet composite layer is 0.2%, 0.4%, 0.6% or 0.8%.

2. The method for preparing a space radiation resistant polyimide-mica nanosheet composite sandwich material according to claim 1, characterized in that The preparation method is carried out according to the following steps: Step S1: peeling off mica nanosheets; Mixing dry mica powder and lithium chloride, adding methanol and placing in a planetary ball mill, and fully ball milling to obtain a mixed solution a; washing and drying the mixed solution a, adding isopropanol solution, and stirring evenly to obtain a mixed solution b; firstly subjecting the mixed solution b to ultrasonication, and then subjecting it to two-step centrifugation to obtain a mica nanosheet precipitate; washing the mica nanosheet precipitate and freeze-drying it to obtain a mica nanosheet; Step S2: preparing a polyimide-mica nanosheet composite sandwich material; 4,4'-diaminodiphenyl ether is added to N,N-dimethylacetamide solution, and ultrasonically dispersed to obtain a mixed solution c; the mixed solution c is divided into two parts, and the mica nanosheets obtained in step S1 are added to one of the mixed solutions c, and mixed evenly to obtain a mixed solution d; two equal parts of pyromellitic anhydride are added to the other mixed solution c and the mixed solution d, respectively, and mechanically stirred until viscous to obtain mixed solutions e and f; the mixed solution e and the mixed solution f are evacuated respectively, and then the mixed solution f is evenly coated on one surface of the pretreated glass substrate, and the mixed solution e is evenly coated after solidification, and the mixed solution f is evenly coated after solidification again, and the substrate is gradually heated to 350°C after further solidification, and is kept at 350°C for 50 to 70 minutes; after the insulation is completed, it is cooled to room temperature, and the film on the substrate is peeled off to obtain a polyimide-mica nanosheet composite interlayer material resistant to space radiation.

3. The method for preparing a space radiation resistant polyimide-mica nanosheet composite sandwich material according to claim 2, characterized in that The ratio of the mass of the dry mica powder, the mass of lithium chloride and the volume of methanol described in step S1 is (4.9-5.1) g: (4.9-5.1) g: (5-15) mL; the ratio of the mass of the mixed solution a after washing and drying in step S1 to the volume of the isopropanol solution is (0.45-0.55) g: (340-360) mL.

4. The method for preparing a space radiation resistant polyimide-mica nanosheet composite sandwich material according to claim 2, characterized in that The ball milling time in step S1 is 8 to 12 hours; the two-step centrifugation in step S1 is: first, the mixed solution b after ultrasound is centrifuged at a speed of 1800 to 2000 rpm for 19 to 21 minutes, and the obtained supernatant is centrifuged again at a speed of 8000 to 9000 rpm for 8 to 10 minutes; in step S1, the mica nanosheet precipitate is washed 3 to 5 times with deionized water.

5. The method for preparing a space radiation resistant polyimide-mica nanosheet composite sandwich material according to claim 2, characterized in that The ratio of the mass of 4,4'-diaminodiphenyl ether, the volume of N,N-dimethylacetamide solution and the total mass of pyromellitic dianhydride described in step S2 is (2.9-3.1) g: (39.5-40.5) mL: (3.27-3.29) g.

6. The method for preparing a space radiation resistant polyimide-mica nanosheet composite sandwich material according to claim 2, characterized in that The time of ultrasonic dispersion in step S2 is 15 to 45 minutes; the time of mechanical stirring in step S2 is 3 to 5 hours; the temperature of three curings in step S2 is 79 to 81° C., the time of the first two curings is 30 to 40 minutes, and the time of the third curing is 8 to 12 hours.

7. The method for preparing a space radiation resistant polyimide-mica nanosheet composite sandwich material according to claim 2, characterized in that Before adding pyromellitic anhydride to another mixed solution c and mixed solution d in step S2, it is first dried in a vacuum environment at 60° C. for 7 to 9 hours; after the insulation in step S2 is completed, the substrate is first immersed in deionized water for 10 to 15 minutes, and then the film on the substrate is peeled off.

8. The method for preparing a space radiation resistant polyimide-mica nanosheet composite sandwich material according to claim 2 or 7, characterized in that The pretreated glass substrate described in step S2 is treated according to the following steps: first, the substrate is cleaned with clean water for 1 to 3 times, then rinsed with deionized water for 3 to 5 times, then cleaned with anhydrous ethanol for 3 to 5 times, and finally dried at 50 to 60° C. for 45 to 75 minutes to obtain a pretreated substrate, wherein the substrate is a glass plate.

9. The method for preparing a space radiation resistant polyimide-mica nanosheet composite sandwich material according to claim 2 or 7, characterized in that In step S2, pyromellitic anhydride is added to another mixed solution c and a mixed solution d in four times, wherein 1 / 2 of the total mass is added in the first time, 1 / 4 of the total mass is added in the second time, 1 / 8 of the total mass is added in the third and fourth times, and the interval time of the four additions is 25 to 35 minutes. The gradient heating described in step S2 is to first place the substrate in a blast oven and heat it to 80 to 82° C., and keep it at 80 to 82° C. for 8 to 12 hours; then heat it to 109 to 111° C., 139 to 141° C., 169 to 171° C., 199 to 201° C., 229 to 231° C., 259 to 261° C., 289 to 291° C. and 319 to 321° C. in sequence, and keep it at this temperature for 25 to 35 minutes; and finally heat it to 350° C.

10. The use of a space radiation resistant polyimide-mica nanosheet composite sandwich material as claimed in claim 1, characterized in that Application of the space radiation resistant polyimide-mica nanosheet composite sandwich material in the preparation of space radiation shielding material.

Citation Information

Patent Citations

  • Preparation method of sericite nanosheets

    CN104743562A

  • Polyimide composite material with double-layer structure with extreme environmental tolerance and preparation method thereof

    CN111499911A

  • Phosphoric acid-based nano thermal insulation material and preparation method thereof

    CN113816719A

  • Radiation-resistant polyimide with sandwich structure as well as preparation method and application of radiation-resistant polyimide

    CN114316324A

  • Preparation method and application of acceptor doped filler / polyimide insulating composite film

    CN114539771A