Scratch-resistant transparent polyimide film and preparation method thereof
By adopting a three-layer transparent polyimide film, the reaction between nano-silicon dioxide and polyimide is used to enhance the surface hardness, and the transparent polyimide in the prior art is solved by solving the impact resistance of ultra-thin glass in the prior art The problem of insufficient results has achieved both scratch resistance and flexibility, and is suitable for large screens and special forms of folding screens.
Patent Information
- Application Number
- CN202411292036.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-26
AI Technical Summary
When existing transparent polyimide CPI and ultra-thin glass UTG are used as flexible display cover materials, the transparent polyimide surface hardness is low and easy to scratch, while ultra-thin glass is insufficient in impact resistance and in large screens and special forms. There are difficulties in making folding screens.
Scratch-resistant transparent polyimide film with a three-layer structure, including a transparent polyimide film containing nano-silica and a middle-layer transparent polyimide film body, through nano-silica and polyimide The reaction enhances surface hardness and prepares the film by a specific imidation process.
It improves the surface hardness and scratch resistance of transparent polyimide films, while maintaining flexibility and light transmittance, and is suitable for large screens and special forms of folding screens.
Smart Images

Figure CN119019733A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electronic materials, and in particular relates to a scratch-resistant transparent polyimide film and a preparation method thereof. Background Art
[0002] At present, the shipment volume of foldable screen mobile phones continues to increase, and the cover plates used in the products are mostly UTG and CPI. Among them, UTG refers to ultra-thin glass material; CPI refers to transparent polyimide.
[0003] However, both transparent polyimide CPI and ultra-thin glass UTG have obvious disadvantages when used as flexible display cover materials. Although transparent polyimide has excellent flexibility and folding performance, is not easy to break, has high safety, and can adapt to the needs of large-screen folding and screen curling, its surface hardness is lower than 1H, and the screen is easily scratched. Although ultra-thin glass has a high surface hardness and the screen is scratch-resistant, its impact resistance is still insufficient, so a protective film needs to be attached. Moreover, after the protective film is attached, UTG is very prone to creases during use, and it is difficult to produce large screens and special forms of folding screens due to the relatively fixed bending point. Summary of the invention
[0004] The purpose of the present invention is to provide a scratch-resistant transparent polyimide film, which has good flexibility and foldability and hardness sufficient to resist scratches and can be used as a flexible display cover.
[0005] The present invention adopts the following technical scheme: a scratch-resistant transparent polyimide film, which has a three-layer structure, namely a lower layer, a middle layer and an upper layer stacked in sequence, wherein the upper layer and the lower layer are both transparent polyimide films containing nano-silicon dioxide, and the middle layer is a transparent polyimide film body.
[0006] Furthermore, the transparent polyimide film containing nano-silicon dioxide has a thickness of 1 to 10 μm, preferably 4 to 6 μm.
[0007] Furthermore, the transparent polyimide film body is prepared by imidization of transparent polyamic acid glue.
[0008] Furthermore, the thickness of the transparent polyimide film body is 10-50 μm.
[0009] Furthermore, the thickness of the transparent polyimide film body is 35-45 μm.
[0010] Furthermore, the surface of the nano-silicon dioxide is modified to have amino groups or hydroxyl groups, with the number of groups being 1 to 10 per nm. 2 .
[0011] Furthermore, the number of the groups is 3 to 5 / nm 2.
[0012] Furthermore, in the transparent polyimide film containing nano-silicon dioxide, the specific surface area of the nano-silicon dioxide is not less than 150 m 2 / g, particle size is 1 ~ 100nm.
[0013] The present invention also discloses a method for preparing the above-mentioned scratch-resistant transparent polyimide film, comprising the following steps:
[0014] Step 1: Preparation of nano-silicon dioxide slurry:
[0015] Adding nano-silicon dioxide into an organic solvent and dispersing it by ultrasonic wave to obtain a nano-silicon dioxide dispersion liquid; the mass percentage of nano-silicon dioxide in the dispersion liquid is 30%;
[0016] Adding transparent polyamic acid glue into nano-silicon dioxide dispersion to obtain nano-silicon dioxide slurry; in the nano-silicon dioxide slurry, the mass ratio of nano-silicon dioxide to polyamic acid is 20:80 to 25:75;
[0017] Step 2: Prepare transparent polyimide film body:
[0018] The transparent polyamic acid glue solution is coated on a glass plate, imidized once, and cooled to room temperature after the imidization to obtain a transparent polyimide film body;
[0019] Step 3: Preparation of scratch-resistant transparent polyimide film:
[0020] The upper and lower surfaces of the transparent polyimide film in step 2 are coated with the nano-silicon dioxide slurry prepared in step 1, and secondary imidization is performed. After the secondary imidization is completed, the temperature is cooled to room temperature, and transparent polyimide films containing nano-silicon dioxide are formed on the upper and lower surfaces to obtain a scratch-resistant transparent polyimide film.
[0021] Furthermore, the primary imidization process in step 2 and the secondary imidization process in step 3 are both as follows: 80°C / 5min→120°C / 5min→150°C / 5min→180°C / 5min→200°C / 5min→250°C / 5min→300°C / 4min→350°C / 4min→400°C / 3min.
[0022] The beneficial effects of the present invention are as follows: 1. Nano-silicon dioxide with active reaction groups is introduced, and the active reaction groups can react with the groups in polyimide, so that the silicon dioxide and polyimide are firmly combined, thereby improving the surface hardness, scratch resistance and light transmittance of the transparent polyimide film. 2. The three-layer sandwich structure transparent polyimide film is adopted, which not only improves the surface hardness and scratch resistance of the transparent polyimide film, but also avoids the shortcomings of the single-layer structure transparent polyimide film that the surface hardness is too low and easy to be scratched or too high and poor toughness. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a structural diagram of scratch-resistant transparent polyimide film.
[0024] Wherein: 1. a transparent polyimide film containing nano silicon dioxide; 2. a transparent polyimide film body. DETAILED DESCRIPTION
[0025] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0026] The present invention provides a scratch-resistant transparent polyimide film, such as Figure 1 As shown, it is a three-layer structure, which is a lower layer, a middle layer and an upper layer stacked in sequence, wherein the upper layer and the lower layer are both transparent polyimide films 1 containing nano-silicon dioxide, and the middle layer is a transparent polyimide film body 2, and the transparent polyimide film body 2 does not contain nano-silicon dioxide.
[0027] The transparent polyimide film 1 containing nano-silicon dioxide has a thickness of 1 to 10 μm, preferably 4 to 6 μm.
[0028] The transparent polyimide film body 2 is made by imidization of transparent polyamic acid glue, and has a thickness of 10 to 50 μm, preferably 35 to 45 μm.
[0029] In the above-mentioned transparent polyimide film 1 containing nano-silicon dioxide, the surface of the nano-silicon dioxide is modified to have amino groups or hydroxyl groups, and the number of groups is 1 to 10 / nm. 2 , preferably, the number of groups is 3 to 5 / nm 2 The active reactive groups can react with the groups in polyimide to firmly combine silicon dioxide and polyimide, thereby improving the surface hardness, scratch resistance and light transmittance of the transparent polyimide film.
[0030] In the above-mentioned transparent polyimide film 1 containing nano-silicon dioxide, the specific surface area of the nano-silicon dioxide is not less than 150 m 2 / g, and the particle size is 1 to 100 nm, preferably, the particle size is 10 to 30 nm.
[0031] The present invention also discloses a method for preparing the scratch-resistant transparent polyimide film, comprising the following steps:
[0032] Step 1: Preparation of nano-silicon dioxide slurry:
[0033] At room temperature, add nano-silicon dioxide into a glass container containing an organic solvent and disperse it by ultrasonic for 30 minutes to obtain a nano-silicon dioxide dispersion. The mass percentage of nano-silicon dioxide in the dispersion is 30%. Room temperature refers to the temperature of the laboratory during the experiment, generally 25°C.
[0034] At room temperature, transparent polyamic acid glue is added into a high-speed disperser containing nano-silicon dioxide dispersion, and dispersed at a speed of 2000 rpm for 30 minutes to obtain nano-silicon dioxide slurry; in the nano-silicon dioxide slurry, the mass ratio of nano-silicon dioxide to polyamic acid is 20:80-25:75.
[0035] Step 2: Prepare transparent polyimide film body 2:
[0036] The transparent polyamic acid glue is evenly coated on a clean and flat glass plate, and imidization is carried out according to the following procedure: 80℃ / 5min→120℃ / 5min→150℃ / 5min→180℃ / 5min→200℃ / 5min→250℃ / 5min→300℃ / 4min→350℃ / 4min→400℃ / 3min. After the imidization is completed, the temperature is cooled to room temperature to obtain a transparent polyimide film body 2. The amount of the transparent polyamic acid glue is determined according to the thickness of the transparent polyimide film obtained after imidization.
[0037] Step 3: Preparation of scratch-resistant transparent polyimide film:
[0038] The upper and lower surfaces of the transparent polyimide film in step 2 are evenly coated with the nano-silicon dioxide slurry prepared in step 1 using a double coating head. Imidization is carried out according to the following procedure: 80℃ / 5min→120℃ / 5min→150℃ / 5min→180℃ / 5min→200℃ / 5min→250℃ / 5min→300℃ / 4min→350℃ / 4min→400℃ / 3min. After the imidization is completed, the temperature is lowered to room temperature, and a transparent polyimide film 1 containing nano-silicon dioxide is formed on the upper and lower surfaces to obtain a scratch-resistant transparent polyimide film. The amount of nano-silicon dioxide slurry is determined according to the thickness of the transparent polyimide containing silicon dioxide obtained after imidization.
[0039] The specifications of the prepared transparent polyimide film body are as follows: hardness ≧1B; transmittance ≧90%; yellowing index ≦10; glass transition temperature ≧200°C; thermal decomposition temperature Td1% ≧300°C; thermal expansion coefficient at 50-200°C ≦20ppm; tensile strength ≧200MPa; tensile modulus ≧2GPa; elongation at break ≧20%.
[0040] To further explain the method of the present invention, the following examples are given:
[0041] The amounts of the components used in Examples E1 to E4 are shown in Table 1. The test methods and data for the properties of the scratch-resistant transparent polyimide films prepared in Examples E1 to E4 are shown in Table 2.
[0042] Table 1 Examples E1 to E4
[0043]
[0044]
[0045] Example E1
[0046] Step 1: Preparation of nano-silicon dioxide slurry:
[0047] At room temperature, 3 g of amino-modified nano-silica was added to a glass container containing 7 g of organic solvent N,N-dimethylacetamide, and dispersed by ultrasonic for 30 minutes to obtain a nano-silica dispersion liquid, in which the mass percentage of nano-silica was 30%.
[0048] At room temperature, add 60g of transparent polyamic acid glue into a high-speed disperser containing the nano-silicon dioxide dispersion prepared in step 1, and disperse at 2000 rpm for 30min to obtain nano-silicon dioxide slurry. The density of nano-silicon dioxide is 2.43g / cm 3 , the specific gravity of nano-silica slurry is 1.026.
[0049] Step 2: Prepare transparent polyimide film body:
[0050] Take a certain amount of transparent polyamide acid and evenly coat it on a clean and flat glass plate. Follow the following procedure for imidization: 80℃ / 5min→120℃ / 5min→150℃ / 5min→180℃ / 5min→200℃ / 5min→250℃ / 5min→300℃ / 4min→350℃ / 4min→400℃ / 3min. After imidization, cool to room temperature to obtain a transparent polyimide film. The density of the transparent polyimide film is 1.4g / cm 3 , 40μm thick, 20cm long and 15cm wide.
[0051] Step 3: Preparation of scratch-resistant transparent polyimide film:
[0052] The nano-silicon dioxide slurry prepared in step 1 is evenly coated on the upper and lower surfaces of the transparent polyimide film body prepared in step 2. Imidization is carried out according to the following procedure: 80℃ / 5min→120℃ / 5min→150℃ / 5min→180℃ / 5min→200℃ / 5min→250℃ / 5min→300℃ / 4min→350℃ / 4min→400℃ / 3min. After the imidization is completed, the temperature is cooled to room temperature, and a transparent polyimide film containing nano-silicon dioxide is formed on the upper and lower surfaces to obtain a scratch-resistant transparent polyimide film E1. The performance test data of the scratch-resistant transparent polyimide film E1 are shown in Table 2.
[0053] Example E2
[0054] The steps are the same as those in Example E1, except that:
[0055] In step 1, 3 g of hydroxyl-modified nano-silica is used;
[0056] In step 2,
[0057] Example E3
[0058] In step 1, 45 g of transparent polyamic acid glue is used;
[0059] In step three, 2.16 g of nano-silicon dioxide slurry was obtained.
[0060] Example E4
[0061] In step 1, 3g of hydroxyl-modified nano-silica and 45g of transparent polyamic acid glue are used;
[0062] Comparison sample
[0063] The preparation method of transparent polyimide film is as follows:
[0064] Take 10.5g of transparent polyamic acid glue and evenly apply it on a clean and flat glass plate with a length x width of 20cm x 15cm. Imidization is carried out according to the following procedure: 80℃ / 5min→120℃ / 5min→150℃ / 5min→180℃ / 5min→200℃ / 5min→250℃ / 5min→300℃ / 4min→350℃ / 4min→400℃ / 3min. After the imidization is completed, cool to room temperature to obtain a comparative transparent polyimide film with a thickness of 50μm.
[0065] Table 2 Main performance data and performance test methods of scratch-resistant transparent polyimide film
[0066]
[0067]
[0068] It can be seen from Table 2 that the hardness of the transparent polyimide film prepared in Examples E1 to E4 is significantly higher than that of the comparative film, and has good scratch resistance. At the same time, other properties of the film do not show obvious deterioration, and the glass transition temperature, thermal decomposition temperature, thermal expansion performance, tensile strength, tensile modulus and other properties are improved. This shows that the method of the present invention is effective, and the scratch-resistant transparent polyimide film of the present invention can be used as a flexible display cover and other polyimide material application fields that require scratch resistance, good light transmittance, good thermal properties, and good mechanical properties.
Claims
1. A scratch-resistant transparent polyimide film, It is characterized in that It has a three-layer structure, which comprises a lower layer, a middle layer and an upper layer stacked in sequence, wherein the upper layer and the lower layer are both transparent polyimide films (1) containing nano silicon dioxide, and the middle layer is a transparent polyimide film body (2).
2. A scratch-resistant transparent polyimide film as claimed in claim 1, It is characterized in that The transparent polyimide film (1) containing nano-silicon dioxide has a thickness of 1 to 10 μm, preferably 4 to 6 μm.
3. The scratch-resistant transparent polyimide film according to claim 1, It is characterized in that The transparent polyimide film body (2) is prepared by imidization of transparent polyamic acid glue.
4. The scratch-resistant transparent polyimide film according to claim 1, It is characterized in that The transparent polyimide film body (2) has a thickness of 10 to 50 μm.
5. A scratch-resistant transparent polyimide film as claimed in claim 4, It is characterized in that The thickness of the transparent polyimide film body (2) is 35-45 μm.
6. A scratch-resistant transparent polyimide film as claimed in claim 5, It is characterized in that The surface of the nano-silicon dioxide is modified to have amino groups or hydroxyl groups, and the number of the groups is 1 to 10 / nm 2 .
7. A scratch-resistant transparent polyimide film as claimed in claim 6, It is characterized in that The number of groups is 3 to 5 / nm 2 .
8. The scratch-resistant transparent polyimide film according to claim 7, It is characterized in that In the transparent polyimide film containing nano-silicon dioxide, the specific surface area of the nano-silicon dioxide is not less than 150 m 2 / g, particle size is 1 ~ 100nm.
9. A method for preparing a scratch-resistant transparent polyimide film according to any one of claims 1 to 8, It is characterized in that The steps include: Step 1: Preparation of nano-silicon dioxide slurry: Adding nano-silicon dioxide into an organic solvent and dispersing it by ultrasonic wave to obtain a nano-silicon dioxide dispersion liquid; the mass percentage of nano-silicon dioxide in the dispersion liquid is 30%; Adding transparent polyamic acid glue into nano-silicon dioxide dispersion to obtain nano-silicon dioxide slurry; in the nano-silicon dioxide slurry, the mass ratio of nano-silicon dioxide to polyamic acid is 20:80 to 25:75; Step 2: Prepare a transparent polyimide film body (2): The transparent polyamic acid glue solution is coated on a glass plate, imidized once, and cooled to room temperature after the imidization to obtain a transparent polyimide film body; Step 3: Preparation of scratch-resistant transparent polyimide film: The upper and lower surfaces of the transparent polyimide film in step 2 are coated with the nano-silicon dioxide slurry prepared in step 1, and secondary imidization is performed. After the secondary imidization is completed, the temperature is cooled to room temperature, and transparent polyimide films (1) containing nano-silicon dioxide are formed on the upper and lower surfaces to obtain a scratch-resistant transparent polyimide film.
10. The method for preparing a scratch-resistant transparent polyimide film according to claim 7, It is characterized in that The primary imidization process in step 2 and the secondary imidization process in step 3 are both as follows: 80°C / 5min→120°C / 5min→150°C / 5min→180°C / 5min→200°C / 5min→250°C / 5min→300°C / 4min→350°C / 4min→400°C / 3min.