Preparation of transparent flexible polysilsesquioxane monoblock aerogel and application of transparent flexible polysilsesquioxane monoblock aerogel in building glass

By mixing polyether nonionic surfactant with methyl alkoxy silane and hydrolyzing acetic acid, a double continuous framework structure is formed, which solves the problems of transparency and mechanical properties in aerogel preparation and achieves high transparency and flexible gas The preparation of gel is suitable for high light transmission applications such as architectural glass.

CN119019752APending Publication Date: 2024-11-26IBIH ADVANCED MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411335569.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-26

Smart Images

  • Figure BDA0005058147630000131
    Figure BDA0005058147630000131
  • Figure HDA0005058147650000011
    Figure HDA0005058147650000011
  • Figure HDA0005058147650000012
    Figure HDA0005058147650000012
Patent Text Reader

Abstract

The invention discloses preparation of transparent flexible polysilsesquioxane monoblock aerogel and application of the transparent flexible polysilsesquioxane monoblock aerogel to building glass. The aerogel structure is prepared by preferably selecting polyether nonionic surface active types and mixing the polyether nonionic surface active types with methyl alkoxy silane according to a proper proportion, so that the phase separation degree can be effectively regulated and controlled; acetic acid is specially selected to hydrolyze methyl alkoxy silane in a polyether nonionic surfactant system, the regulation and control capability in the aerogel phase separation process is fully exerted, a uniform and continuous double-skeleton structure is formed, the high porosity structure is guaranteed, meanwhile, the flexibility and light transmittance of the aerogel material are remarkably improved, and the preparation method is suitable for large-scale industrial production. The application in the fields of building glass and the like needing high light transmission is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aerogel preparation, and in particular relates to the preparation of a transparent flexible polysilsesquioxane monolithic aerogel and its application in architectural glass. Background Art

[0002] Aerogel is a solid material with extremely low density and high porosity. Its internal structure is composed of nano-scale solid particles, which are filled with air, so it has extremely low thermal conductivity and density. Due to these unique physical properties, aerogel has a wide range of application potential in the fields of thermal insulation, sound insulation, catalyst carrier, energy storage, etc. However, the preparation and application of aerogel still face many challenges, especially in improving its mechanical properties, transparency, and adaptability to application in specific fields.

[0003] At present, the preparation method of aerogel mainly relies on the sol-gel process to form a three-dimensional network structure by controlling the reaction conditions. However, the aerogels prepared by these methods often have the problems of large brittleness and poor hydrophobicity, which limits their use in practical applications. In order to improve these shortcomings, it is usually necessary to perform complex post-processing modification processes on the aerogel, such as surface hydrophobic treatment, cross-linking enhancement, etc. These modification steps not only increase the production cost, but may also affect other properties of the aerogel.

[0004] Polysilsesquioxane gels have been one of the hot topics of research in recent years, and have attracted attention due to their high mechanical strength and thermal stability. However, the existing polysilsesquioxane aerogel preparation process often produces white opaque products with low transparency, which is unacceptable in applications that require high light transmittance, such as architectural glass. In addition, these aerogels are difficult to prepare into large blocks, which further limits their scope of application.

[0005] In the preparation of aerogel glass, the transmittance of composite materials using granular or powdered aerogel is low, usually only about 30%, which is much lower than the 80% transmittance of a whole piece of transparent aerogel glass. The existence of intergranular gaps not only reduces the transmittance, but also increases the thermal conductivity of the material, which is contrary to the original intention of aerogel as a thermal insulation material. In addition, the existing preparation process is often cumbersome and time-consuming, making it difficult to achieve large-scale production.

[0006] It is particularly important to study aerogel materials that have both high light transmittance and flexibility. However, in current technology, the functions of flexible aerogels are relatively simple, and their pore structure is difficult to adjust according to actual application requirements. The skeleton structure of siloxane aerogels is usually composed of spherical particles. This structure leads to poor mechanical properties and is difficult to meet the requirements of applications such as architectural glass that have high requirements for strength and flexibility.

[0007] In summary, the current aerogel preparation technology has many limitations, especially in terms of improving transparency, mechanical properties and adapting to specific application requirements. Therefore, developing a new method for preparing monolithic aerogels to achieve high transparency, good flexibility and adapt to the needs of specific application fields such as architectural glass is an important direction of current research. Summary of the invention

[0008] The present invention aims at the problems in the prior art and discloses the preparation of a transparent flexible polysilsesquioxane monolithic aerogel and its application in architectural glass. The present invention prepares an aerogel structure by selecting a polyether nonionic surfactant and mixing it with methyl alkoxy silane in an appropriate ratio, and selects acetic acid to hydrolyze the methyl alkoxy silane in a polyether nonionic surfactant system, thereby significantly improving the flexibility and light transmittance of the aerogel material while ensuring a high porosity structure, which is beneficial to the application in fields requiring high light transmittance such as architectural glass.

[0009] The present invention is achieved through the following technical solutions:

[0010] In a first aspect, the present invention provides a method for preparing a transparent flexible polysilsesquioxane monolithic aerogel, the preparation method comprising:

[0011] S1: a polyether nonionic surfactant and an acetic acid aqueous solution are stirred evenly, and then methyl alkoxy silane is added to prepare a silane precursor solution;

[0012] S2: adding an alkaline catalyst to the silane precursor solution described in S1, stirring evenly, and preparing a wet gel in an oven;

[0013] S3: The wet gel described in S2 is subjected to gradient replacement by a water-ethanol system, and after the replacement, it is dried to obtain a complete transparent flexible polysilsesquioxane aerogel material;

[0014] The addition amount of the polyether nonionic surfactant is 1-9%, and the silicon source is selected from silane with a mass percentage of 20-50%.

[0015] In the design scheme of the present invention, by mixing the polyether nonionic surfactant and the silicon source in an appropriate ratio to prepare the aerogel material, the degree of phase separation can be regulated, and the silane particles can be evenly diffused in the system to ensure the transparency of the aerogel structure; a double continuous skeleton structure is obtained, which helps to improve the mechanical strength and flexibility of the aerogel material; and the aerogel material is easy to fall off and not easy to crack. The present invention specifically selects acetic acid to hydrolyze silane in the system of polyether nonionic surfactant. On the one hand, the pH value of the solution can be adjusted. On the other hand, acetic acid, as a weak acid, helps to maintain the structural stability of the polyether nonionic surfactant and improve the dispersibility of the polyether nonionic surfactant in the aerogel material. On the third hand, the rate at which acetic acid promotes the hydrolysis of methyl alkoxy silane can match the rate at which the polyether nonionic surfactant forms a strong hydrogen bond with the methyl alkoxy silane, which is conducive to forming a uniform and continuous double skeleton structure and improving the transparency of its aerogel material.

[0016] As a further solution, the addition amount of the polyether nonionic surfactant is preferably 3-5%, and the methyl alkoxy silane is preferably 25-35% by mass of silane.

[0017] The addition amount of polyether nonionic surfactant and the ratio of silicon source within the optimized range can ensure that the aerogel material has excellent mechanical properties and flexibility while maintaining high transparency, ensure the uniform pore structure of the aerogel, and effectively combine with the EOPOEO chain of the polyether nonionic surfactant to form a strong hydrogen bond, thereby improving its transparency and thermal insulation performance. Give full play to the role of polyether nonionic surfactant in regulating the pore structure of aerogels, and form a uniform and unobstructed double continuous network skeleton structure.

[0018] As a further scheme, the type of the polyether nonionic surfactant is selected from one or more of propylene glycol block polyether, polyoxyethylene ether nonionic surfactant, polyol ester nonionic surfactant, HSH polyether polyol, polyoxyethylene polyoxypropylene ether block copolymer or other commercially available specific types of polyether nonionic surfactants; as some specific examples: propylene glycol block polyether may include one or more of models L31, L35, F38, L42, L43, L44, L61, L62, L63, L64, P65, F68; polyoxyethylene polyoxypropylene ether block copolymer may include one or more of PE6200, PE6100, F127; other commercially available specific types of polyether nonionic surfactants include one or more of polyether F-6, polyether NPE-108, polyether NPE-105, and PEP type block copolymer.

[0019] Furthermore, the type of the polyether nonionic surfactant is preferably selected from polyoxyethylene polyoxypropylene ether block copolymers.

[0020] As a further solution, the methylalkoxy silane is selected from one or more of methyltrimethoxysilane, methyltriethoxysilane, and polydimethylsiloxane.

[0021] As a further embodiment, the alkaline catalyst includes one or more of ammonia water, urea, triethylamine, tetramethylammonium hydroxide, and tetraethylammonium hydroxide.

[0022] As a further solution, the content of the alkaline catalyst is 2-4%; alkaline catalysts within a suitable range can accelerate the reaction process of hydrolysis and polycondensation, and cooperate with polyether nonionic surfactants to promote the uniform distribution and orderly arrangement of precursor molecules, thereby forming a uniform and controllable pore structure in the gel network.

[0023] Furthermore, the content of the alkaline catalyst is preferably 2.5-3%.

[0024] As a further solution, the mass fraction of acetic acid in S1 is selected from 0.01-0.3%.

[0025] As a further solution, the oven temperature in S2 is selected from 50-80°C.

[0026] As a further solution, in S3, the drying method is selected from CO 2 One of the following methods: supercritical drying, vacuum drying or freeze drying. A suitable drying method is essential for obtaining high-quality aerogel materials. 2 Supercritical drying can be achieved by using CO 2 The dissolution and diffusion effect of the liquid-gas interface tension avoids the damage to the bicontinuous skeleton structure of the aerogel, thereby obtaining an aerogel material with high transparency and low density.

[0027] In a second aspect, the present invention provides an application of a transparent flexible polysilsesquioxane monolithic aerogel on architectural glass, wherein the architectural glass field includes windows, curtain walls, skylights and other architectural structures in airports, libraries, office buildings, residential buildings, schools, hospitals and other places. By applying the transparent flexible polysilsesquioxane monolithic aerogel material to architectural glass, the thermal insulation performance and light transmittance of the architectural glass can be significantly improved.

[0028] The characteristics and beneficial effects of the present invention are:

[0029] (1) The present invention prepares an aerogel structure by selecting polyether nonionic surfactant species and mixing them with methyl alkoxy silane in an appropriate ratio, which can effectively control the degree of phase separation. The EOPOEO chain of the polyether nonionic surfactant entangles the network structure of silane, so that a strong hydrogen bond is formed between the silanol and the ether oxygen on the EO group, which is conducive to obtaining a bicontinuous skeleton structure, and further improving the light transmittance and flexibility of the aerogel material while maintaining the high porosity structure of the aerogel; the generated aerogel material is easy to fall off and not easy to crack.

[0030] (2) The present invention particularly selects acetic acid to hydrolyze methyl alkoxy silane in the system of polyether nonionic surfactant, which can not only adjust the pH value of the solution, thereby controlling the hydrolysis rate of the silicon source; it can also help maintain the structural stability of the polyether nonionic surfactant, so that it can fully exert its regulatory ability in the aerogel phase separation process; in addition, the rate at which acetic acid promotes the hydrolysis of methyl alkoxy silane can match the rate at which the polyether nonionic surfactant forms a strong hydrogen bond with the methyl alkoxy silane, which is conducive to forming a uniform and continuous double-skeleton structure and improving the transparency of its aerogel material.

[0031] (3) The present invention uses water as a solvent, which is not only environmentally friendly but also low in cost. Using water as a solvent in the process of preparing aerogels can effectively reduce production costs and reduce environmental pollution. In addition, the use of water helps to improve the uniformity of the reaction system, thereby making the pore structure of the aerogel material more uniform, further improving its flexibility and light transmittance. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0033] Figure 1 This is the SEM image of the transparent flexible polysilsesquioxane monolithic aerogel material of Example 4

[0034] Figure 2 This is a sample picture of the transparent flexible polysilsesquioxane monolithic aerogel material of Example 4. Figure 2 A is a sample of wet gel material of Example 4, and 2B is a sample of aerogel material of Example 4.

[0035] Figure 3 The aerogel material sample diagrams of Comparative Example 2 and Comparative Example 3 are shown in FIG. Figure 3 A is a sample of aerogel material in comparative example 2. Figure 3B is a picture of the aerogel material sample of Example 3.

[0036] Figure 4 This is the SEM image of the aerogel material of Comparative Example 1

[0037] Figure 5 This is a sample of the aerogel material of Example 1

[0038] Figure 6 The aerogel material sample diagrams of Comparative Examples 4 and 5 are shown in FIG. Figure 6 A is a sample diagram of the wet gel material of Example 4, Figure 6 B is a picture of the wet gel material sample of Comparative Example 5. DETAILED DESCRIPTION

[0039] In order to facilitate the understanding of the present invention, the present invention will be described in more detail below, and embodiments of the present invention are given, but the scope of the present invention is not limited thereby.

[0040] It has been found that in the process of preparing aerogels, there are significant differences in the interactions between different types of surfactants and aerogel precursors; these differences will further affect the formation of the pore structure of the aerogel. In the prior art, the types of surfactants are mostly ionic surfactants and non-ionic surfactants; the present invention has found through research that non-ionic surfactants have a better effect on improving the light transmittance and flexibility of aerogel materials. Therefore, the types and contents of non-ionic surfactants in the present invention are studied and explored, hoping to prepare a polysilsesquioxane monolithic aerogel with high transparency and good flexibility.

[0041] In a first aspect, the present invention provides a method for preparing a transparent flexible polysilsesquioxane monolithic aerogel, the preparation method comprising:

[0042] S1: a polyether nonionic surfactant and an acetic acid aqueous solution are stirred evenly, and then methyl alkoxy silane is added to prepare a silane precursor solution;

[0043] S2: adding an alkaline catalyst to the silane precursor solution described in S1, stirring evenly, and preparing a wet gel in an oven;

[0044] S3: The wet gel described in S2 is subjected to gradient replacement by a water-ethanol system, and after the replacement, it is dried to obtain a complete transparent flexible polysilsesquioxane aerogel material;

[0045] The addition amount of the polyether nonionic surfactant is 1-9%, and the silicon source is selected from silane with a mass percentage of 20-50%.

[0046] In the design scheme of the present invention, the degree of phase separation can be adjusted by mixing a polyether nonionic surfactant with a silicon source in an appropriate ratio to prepare an aerogel material. On the one hand, the EOPOEO chain of the polyether nonionic surfactant entangles the network structure of silane, so that a strong hydrogen bond is formed between silanol and the ether oxygen on the EO group, which is conducive to obtaining a bicontinuous skeleton structure, thereby helping to improve the mechanical strength and flexibility of the aerogel material; its stronger hydrogen bonding force allows the aerogel material to continue to react during the aging process, causing the gel to shrink slightly and form a film, which is easy to fall off and not easy to crack; further improving the transparency and flexibility of the aerogel. On the other hand, the appropriate silane ratio helps to maintain a good aerogel network structure, improve the uniformity of the gel network, avoid the formation of short chains or cyclic groups due to the presence of methyl groups in the polycondensation process, and cause precipitation. The silane particles can be evenly diffused in the system to ensure the transparency of the aerogel structure.

[0047] The present invention particularly selects acetic acid to hydrolyze silane in the system of polyether nonionic surfactant. Firstly, the pH value of the solution can be adjusted, thereby controlling the hydrolysis rate of the silicon source and ensuring the uniformity of the aerogel pore structure. Secondly, acetic acid, as a weak acid, helps to maintain the structural stability of the polyether nonionic surfactant, so that it can fully exert its control ability in the aerogel phase separation process, improve the dispersibility of the polyether nonionic surfactant in the aerogel material, avoid the aggregation behavior of the polyether nonionic surfactant affecting the transparency and uniformity of the aerogel, and acetic acid can gently further optimize the pore structure of the aerogel. Thirdly, the rate at which acetic acid promotes the hydrolysis of methyl alkoxy silane can match the rate at which the polyether nonionic surfactant forms a strong hydrogen bond with the methyl alkoxy silane, which is conducive to forming a uniform and continuous double skeleton structure and improving the transparency of the aerogel material.

[0048] As a further solution, the addition amount of the polyether nonionic surfactant is preferably 3-5%, and the methyl alkoxy silane is preferably 25-35% by mass of silane.

[0049] The addition amount of polyether nonionic surfactant and the ratio of silicon source within the optimized range can ensure that the aerogel material has excellent mechanical properties and flexibility while maintaining high transparency. The appropriate ratio of methyl alkoxy silane can effectively avoid the uneven distribution of silane particles during the acetic acid hydrolysis process, thereby ensuring the uniform pore structure of the aerogel, effectively combining with the EOPOEO chain of the polyether nonionic surfactant to form a strong hydrogen bond, and improving its transparency and thermal insulation performance. When the addition amount of polyether nonionic surfactant is too much, it may cause the pore structure of the aerogel material to be too tight, which is not conducive to the full expansion of its EOPOEO chain in the system and the full entanglement of the MSQ network of methyl alkoxy silane, reducing the binding ability of hydrogen bonds, greatly prolonging the gel time, and may cause structural collapse during the aging process, making the aerogel material crack and difficult to demold; thereby reducing its transparency and mechanical properties; while if the addition amount is too little, the role of polyether nonionic surfactant in regulating the pore structure of the aerogel may not be fully exerted, which is not conducive to the formation of a uniform and unobstructed network structure, and affects the formation of a stable porous structure of the aerogel.

[0050] As a further scheme, the type of the polyether nonionic surfactant is selected from one or more of propylene glycol block polyether, polyoxyethylene ether nonionic surfactant, polyol ester nonionic surfactant, HSH polyether polyol, polyoxyethylene polyoxypropylene ether block copolymer or other commercially available specific types of polyether nonionic surfactants; as some specific examples: propylene glycol block polyether may include one or more of models L31, L35, F38, L42, L43, L44, L61, L62, L63, L64, P65, F68; polyoxyethylene polyoxypropylene ether block copolymer may include one or more of PE6200, PE6100, F127; other commercially available specific types of polyether nonionic surfactants include one or more of polyether F-6, polyether NPE-108, polyether NPE-105, and PEP type block copolymer.

[0051] This type of surfactant generally has a polyether chemical structure and can construct stable EOPOEO segments. These segments can form stronger hydrogen bonding forces with methyl alkoxy silanes. Maintaining the stability of the porous skeleton structure, it is easy to remove the film during the aging process, which is beneficial to maintaining the integrity of the aerogel structure and forming a double continuous skeleton network structure with high transmittance.

[0052] Furthermore, the type of the polyether nonionic surfactant is preferably selected from polyoxyethylene polyoxypropylene ether block copolymers.

[0053] As a further solution, the methylalkoxy silane is selected from one or more of methyltrimethoxysilane, methyltriethoxysilane, and polydimethylsiloxane.

[0054] Methyl alkoxy silanes can form a continuous three-dimensional network structure in the process of preparing aerogel structures, which provides a good skeleton support for aerogels. It is beneficial to prepare polysilsesquioxane monolithic aerogels with high transparency and good flexibility. These silanes are beneficial to combine with polyether surfactants during the hydrolysis process to form a uniform network porous structure.

[0055] As a further embodiment, the alkaline catalyst includes one or more of ammonia water, urea, triethylamine, tetramethylammonium hydroxide, and tetraethylammonium hydroxide.

[0056] As a further solution, the content of the alkaline catalyst is 2-4%; alkaline catalysts within a suitable range can accelerate the reaction process of hydrolysis and polycondensation, and cooperate with polyether nonionic surfactants to promote the uniform distribution and orderly arrangement of precursor molecules, thereby forming a uniform and controllable pore structure in the gel network.

[0057] Furthermore, the content of the alkaline catalyst is preferably 2.5-3%.

[0058] As a further solution, the mass fraction of acetic acid in S1 is selected from 0.01-0.3%.

[0059] On the one hand, the acetic acid concentration within the appropriate range can promote the rapid hydrolysis of methylalkoxy silane, so that its hydrolysis rate can match the rate of strong hydrogen bond formation between the polyether nonionic surfactant and the methylalkoxy silane, forming a uniform pore structure; on the other hand, it can play a synergistic protective role on the polyether nonionic surfactant, avoiding the breakage of its EOPOEO chain during the preparation of aerogel, and protecting the structural stability of the polyether nonionic surfactant so as to form a double continuous network skeleton structure in the subsequent preparation process.

[0060] As a further solution, the oven temperature in S2 is selected from 50-80°C. Selecting a suitable oven temperature can ensure that the gelation process can proceed smoothly, form a stable and uniform porous structure, promote the polyether nonionic surfactant to maintain the stable structure of the EOPOEO chain under the synergistic effect of acetic acid and fully react with methyl alkoxy silane to form a strong hydrogen bonding ability, promote the formation of aerogel bicontinuous skeleton structure, and improve the transparency and flexibility of aerogel. If the oven temperature is too low during the gelation process, the gelation process may be slow, or even a stable porous structure may not be formed; while if the temperature is too high, it may cause thermal shrinkage of the aerogel material, resulting in deformation of the pore structure, which is not conducive to the formation of a stable bicontinuous skeleton structure and affects the transparency and flexibility of the aerogel material.

[0061] As a further solution, in S3, the drying method is selected from CO 2One of the following methods: supercritical drying, vacuum drying or freeze drying. A suitable drying method is essential for obtaining high-quality aerogel materials. 2 Supercritical drying can be achieved by using CO 2 The dissolution and diffusion effect of the liquid-gas interface tension avoids the damage to the bicontinuous skeleton structure of the aerogel, thereby obtaining an aerogel material with high transparency and low density.

[0062] In a second aspect, the present invention provides an application of a transparent flexible polysilsesquioxane monolithic aerogel on architectural glass, wherein the architectural glass field includes windows, curtain walls, skylights and other architectural structures in airports, libraries, office buildings, residential buildings, schools, hospitals and other places. By applying the transparent flexible polysilsesquioxane monolithic aerogel material to architectural glass, the thermal insulation performance and light transmittance of the architectural glass can be significantly improved.

[0063] As a specific example of the implementation of the present invention, the detailed case is provided as follows:

[0064] The methyl alkoxy silane of the present invention forms a siloxane-based sesqui-system under the influence of acetic acid, a polyether nonionic surfactant and base catalysis.

[0065] Example 1

[0066] (1) 4% of a polyether nonionic surfactant PE6200 and 0.12% of an acetic acid aqueous solution were mixed uniformly, and 29% of methyltriethoxysilane was added and stirred uniformly at a speed of 1000 r / min, a stirring time of 100 min, and a temperature of 40° C. to prepare a silane precursor solution;

[0067] (2) adding 2.88% ammonia water, stirring evenly for 1 min, pouring the mixture into a mold, sealing it, and drying it in an oven at 50-80°C for gelation;

[0068] (3) The prepared wet gel block was subjected to water-ethanol gradient replacement for 8 h to ensure the integrity of the wet gel block;

[0069] (4) The wet gel after replacement is subjected to supercritical CO 2 Drying can obtain a complete aerogel material.

[0070] Example 2

[0071] Same as Example 1, except that the polyether nonionic surfactant is PE6100.

[0072] Example 3

[0073] Same as Example 1, except that the polyether nonionic surfactant is L62.

[0074] Example 4

[0075] Same as Example 1, except that the polyether nonionic surfactant is F127.

[0076] Example 5

[0077] (1) 4% of a polyether nonionic surfactant PE6100 and 0.05% of an acetic acid aqueous solution were mixed uniformly, and 20% of methyltriethoxysilane was added and stirred uniformly at a speed of 1000 r / min, a stirring time of 100 min, and a temperature of 40° C. to prepare a silane precursor solution;

[0078] (2) adding 2.95% ammonia water, stirring evenly for 1 min, pouring the mixture into a mold, sealing it, and drying it in an oven at 50-80°C for gelation;

[0079] (3) The prepared wet gel block was subjected to water-ethanol gradient replacement for 8 h to ensure the integrity of the wet gel block;

[0080] (4) The wet gel after replacement is subjected to supercritical CO 2 Drying can obtain a complete aerogel material.

[0081] Example 6

[0082] (1) 4% polyether nonionic surfactant F127 and 0.1% acetic acid aqueous solution were mixed uniformly, and 40% methyltriethoxysilane was added and stirred uniformly at a speed of 1000 r / min, a stirring time of 100 min, and a temperature of 40° C. to prepare a silane precursor solution;

[0083] (2) adding 3.9% ammonia water, stirring evenly for 1 min, pouring the mixture into a mold, sealing it, and drying it in an oven at 50-80°C for gelation;

[0084] (3) The prepared wet gel block was subjected to water-ethanol gradient replacement for 8 h to ensure the integrity of the wet gel block;

[0085] (4) The wet gel after replacement is subjected to supercritical CO 2 Drying can obtain a complete aerogel material.

[0086] Example 7

[0087] (1) 8% polyether nonionic surfactant F127 and 0.25% acetic acid aqueous solution were mixed uniformly, and 42% methyltriethoxysilane was added and stirred uniformly at a speed of 1000 r / min, a stirring time of 100 min, and a temperature of 40° C. to prepare a silane precursor solution;

[0088] (2) adding 3.2% ammonia water, stirring evenly for 1 min, pouring the mixture into a mold, sealing it, and drying it in an oven at 50-80°C for gelation;

[0089] (3) The prepared wet gel block was subjected to water-ethanol gradient replacement for 8 h to ensure the integrity of the wet gel block;

[0090] (4) The wet gel after replacement is subjected to supercritical CO 2 Drying can obtain a complete aerogel material.

[0091] Example 8

[0092] (1) 2.5% of a polyether nonionic surfactant F127 and 0.12% of an acetic acid aqueous solution were mixed uniformly, and 37% of methyltriethoxysilane was added and stirred uniformly at a speed of 1000 r / min, a stirring time of 100 min, and a temperature of 40° C. to prepare a silane precursor solution;

[0093] (2) adding 2.68% ammonia water, stirring evenly for 1 min, pouring the mixture into a mold, sealing it, and drying it in an oven at 50-80°C for gelation;

[0094] (3) The prepared wet gel block was subjected to water-ethanol gradient replacement for 8 h to ensure the integrity of the wet gel block;

[0095] (4) The wet gel after replacement is subjected to supercritical CO 2 Drying can obtain a complete aerogel material.

[0096] Example 9

[0097] (1) 2% of a polyether nonionic surfactant PE6100 and 0.09% of an acetic acid aqueous solution were mixed uniformly, and 22% of methyltriethoxysilane was added and stirred uniformly at a speed of 1000 r / min, a stirring time of 100 min, and a temperature of 40° C. to prepare a silane precursor solution;

[0098] (2) adding 2.2% ammonia water, stirring evenly for 1 min, pouring the mixture into a mold, sealing it, and drying it in an oven at 50-80°C for gelation;

[0099] (3) The prepared wet gel block was subjected to water-ethanol gradient replacement for 8 h to ensure the integrity of the wet gel block;

[0100] (4) The wet gel after replacement is subjected to supercritical CO 2 Drying can obtain a complete aerogel material.

[0101] Example 10

[0102] (1) 7.5% of a polyether nonionic surfactant PE6100 and 0.28% of an acetic acid aqueous solution were mixed uniformly, and 40% of methyltriethoxysilane was added and stirred uniformly at a speed of 1000 r / min, a stirring time of 100 min, and a temperature of 40° C. to prepare a silane precursor solution;

[0103] (2) adding 3.25% ammonia water, stirring evenly for 1 min, pouring the mixture into a mold, sealing it, and drying it in an oven at 50-80°C for gelation;

[0104] (3) The prepared wet gel block was subjected to water-ethanol gradient replacement for 8 h to ensure the integrity of the wet gel block;

[0105] (4) The wet gel after replacement is subjected to supercritical CO 2 Drying can obtain a complete aerogel material.

[0106] Comparative Example 1

[0107] Same as Example 4, except for the type of surfactant and the added amount of 4% cationic surfactant cetyltrimethylammonium bromide (CTAB).

[0108] Comparative Example 2

[0109] Same as Example 4, except that the content of the polyether nonionic surfactant F127 is 0.5%.

[0110] Comparative Example 3

[0111] Same as Example 4, except that the content of the polyether nonionic surfactant F127 is 10%.

[0112] Comparative Example 4

[0113] Same as Example 4, except that the mass fraction of methyltriethoxysilane is 10%.

[0114] Comparative Example 5

[0115] Same as Example 4, except that the mass fraction of methyltriethoxysilane is 60%.

[0116] Comparative Example 6

[0117] Same as Example 4, except that the 0.12% by mass acetic acid aqueous solution is replaced by 0.12% by mass hydrofluoric acid aqueous solution.

[0118] Comparative Example 7

[0119] Same as Example 4, except that the polyether nonionic surfactant F127 is not added.

[0120] Comparative Example 8

[0121] Same as Example 4, except that the 0.12% by mass citric acid aqueous solution is replaced by 0.12% by mass hydrofluoric acid aqueous solution.

[0122] Comparative Example 9

[0123] Same as Example 4, except that the 0.12% by mass oxalic acid aqueous solution is replaced by the 0.12% by mass hydrofluoric acid aqueous solution.

[0124] Specific test methods and conditions:

[0125] 1. Visible light transmittance

[0126] The photometer used was a T6 series UV-visible spectrophotometer, manufactured by Nanjing Filler Instrument Co., Ltd.

[0127] ① Place the sample to be tested on the sample holder and adjust the position of the sample to ensure that the light passes through the center of the sample.

[0128] ② Use a light source to generate stable light and ensure that the light hits the sample vertically.

[0129] ③ Use a photometer to measure the intensity of transmitted light.

[0130] ④Record the transmitted light intensity and incident light intensity, and calculate the visible light transmittance.

[0131] 2. Young's modulus

[0132] Compression test is used to measure Young's modulus. The equipment used is universal testing machine CTS-E100, and the brand is Quanli Testing. In the compression test, the sample is placed on the universal material testing machine, and its size is reduced under the action of an external force. The corresponding stress and strain are measured, and the Young's modulus can be obtained by dividing the stress value by the corresponding strain value.

[0133] 3. Thermal conductivity

[0134] The thermal conductivity is measured by the plate method. The instrument model is DRPL-111 high-precision thermal conductivity tester, and the manufacturer is Xiangtan Xiangyi Instrument Co., Ltd. In the plate method experiment, two parallel plates are usually used, one of which is heated and the other is cooled, and the material to be tested is sandwiched between the two plates. By measuring the temperature of the heating plate and the cooling plate, as well as the heat flux density of the material to be tested, the thermal conductivity of the material to be tested can be obtained.

[0135] 4. Porosity

[0136] The porosity of the samples was tested using a BSD-PS2 porosity meter manufactured by Best Instrument Technology (Beijing) Co., Ltd.

[0137] Table 1

[0138] Surfactants acid Silicon source ammonia Example 1 4% PE6200 0.12% 29% 2.88% Example 2 4% PE6100 0.12% 29% 2.88% Example 3 4%L62 0.12% 29% 2.88% Example 4 4%F127 0.12% 29% 2.88% Example 5 4% PE6100 0.05% 20% 2.95% Example 6 4%F127 0.1% 40% 3.9% Example 7 8%F127 0.25% 42% 3.2% Example 8 2.5%F127 0.12% 37% 2.68% Example 9 2% PE6100 0.09% 22% 2.2% Example 10 7.5% PE6100 0.28% 40% 3.25% Comparative Example 1 4% CTAB 0.12% 29% 2.88% Comparative Example 2 0.5%F127 0.12% 29% 2.88% Comparative Example 3 10%F127 0.12% 29% 2.88% Comparative Example 4 4%F127 0.12% 10% 2.88% Comparative Example 5 4%F127 0.12% 60% 2.88% Comparative Example 6 4%F127 0.12% 29% 2.88% Comparative Example 7 0 0.12% 29% 2.88% Comparative Example 8 4%F127 0.12% 29% 2.88% Comparative Example 9 4%F127 0.12% 29% 2.88%

[0139] Table 2

[0140]

[0141]

[0142] It can be seen from the data in Table 1 that the embodiments have higher visible light transmittance, porosity, and lower thermal conductivity and Young's modulus than the comparative examples, which indicates that the preferred type and composition ratio of the polyether nonionic surfactant can form a bicontinuous skeleton structure with methyl alkoxy silane under the synergistic effect of acetic acid, which is conducive to forming a dense and stable porous structure, thereby maintaining the overall aerogel structure with good flexibility and transmittance.

[0143] By combining Examples 1-10 with Comparative Example 1 Figure 4 , Figure 5 It can be seen that the use of CTAB cationic surfactant cannot form a good bicontinuous network skeleton structure, and its transmittance and Young's modulus cannot be effectively improved; the flexibility and transmittance are poor. This is because the EOPOEO chain unique to the polyether nonionic surfactant is entangled with the MSQ network, and a strong hydrogen bond is formed between the silanol and the ether oxygen on the EO group, making the system more viscous and easier to maintain a bicontinuous structure. The bicontinuous network structure has high flexibility while ensuring a good stable structure, which is beneficial to improving the transmittance and flexibility of the aerogel material.

[0144] Combination Figure 3 A. Figure 3 B and through Examples 1-10 and Comparative Examples 2-3, it can be seen that when the addition amount of the polyether nonionic surfactant is too high or too low, the light transmittance of the aerogel material will be poor, because the addition amount of the polyether nonionic surfactant directly affects the pore size distribution and pore structure of the aerogel material. When the addition amount is too high, the polyether nonionic surfactant is too dense in the system, which increases the difficulty of binding between silanes, greatly prolongs the gel time, causes poor gel structure, and reduces light transmittance. On the contrary, when the addition amount is too low, the polyether nonionic surfactant cannot effectively form a stable network structure, is not conducive to fully combining with methyl alkoxy silanes, reduces the stability and integrity of the aerogel material, and the double skeleton network structure is unevenly formed, resulting in an uneven pore structure, which will reduce the light transmittance of the aerogel material.

[0145] pass Figure 6 A. Figure 6 B and Examples 1-6 and Comparative Examples 4-5 show that when the content of methyl alkoxy silane is too high or too low, the light transmittance, thermal conductivity and Young's modulus of the aerogel material will also be affected, and a good aerogel structure cannot be formed. Appropriate content of methyl alkoxy silane can ensure that the aerogel material has a high light transmittance, a low thermal conductivity and a Young's modulus while maintaining a high porosity, so that while maintaining good light transmittance, it also has excellent thermal insulation performance and flexibility. This is because when the content of methyl alkoxy silane is appropriate, it can form a uniform and dense pore network structure with polyether nonionic surfactants, thereby improving the light transmittance and flexibility of the aerogel; when the content of methyl alkoxy silane is too low, it will lead to insufficient formation of the siloxane network, and a stable dual continuous network skeleton structure cannot be formed, thereby reducing the light transmittance and flexibility of the aerogel. On the contrary, too high a content of methyl alkoxy silane may cause the siloxane network to be too dense, the gel network to be poorly uniform, and the aerogel density to increase, while the flexibility to decrease. At the same time, due to the presence of a large number of methyl groups, the polymerization of silanols will be hindered to form short chains or cyclic groups, causing precipitation and affecting the light transmittance and flexibility of the aerogel.

[0146] It can be seen from Examples 1-10 and Comparative Example 6 that, compared with hydrofluoric acid with a higher acid strength, acetic acid has a better hydrolysis effect on the aerogel material formed by polyether surfactants and methyl alkoxy silanes, and can also synergistically protect the structure of the polyether surfactant from damage, so that it can better play its role and form a stable and continuous double skeleton structure. Thus, a whole aerogel material with higher porosity, light transmittance, lower thermal conductivity and Young's modulus is obtained.

[0147] It can be seen from Examples 1-10 and Comparative Example 7 that the aerogel structure cannot be formed without the addition of polyether nonionic surfactants, which indicates that polyether nonionic surfactants play a vital role in the formation of aerogel structures. The addition of polyether nonionic surfactants not only helps to form a bicontinuous skeleton structure, but also can fully combine with methyl alkoxy silane under the synergistic effect of acetic acid to form a stable porous structure. This structure not only improves the porosity and light transmittance of the aerogel material, but also reduces the thermal conductivity and Young's modulus, so that it has excellent thermal insulation performance and flexibility.

[0148] By comparing Example 4 with Examples 1, 2, 3, 5, 6, 7, 8, 9, and 10 and combining Figure 1 , Figure 2It can be seen that Example 4 has higher visible light transmittance, porosity, and lower thermal conductivity and Young's modulus. This shows that when the polyether nonionic surfactant within the preferred range is combined with the appropriate proportion of methyl alkoxy silane under the synergistic effect of acetic acid, it can form a better bicontinuous skeleton structure with stronger hydrogen bonding to maintain the integrity of the aerogel structure. At the same time, due to the ethoxy content of nearly 70% and the high relative molecular mass in the EOPOEO segment of F127, this special structure can self-assemble to form a large number of repeating units in the form of a "zipper". The EO and PO units are arranged in an alternating manner to form an interlocking network structure, which is more conducive to the construction of the gel network, forming a uniform pore structure, and further improving the light transmittance and flexibility of the aerogel.

[0149] It can be seen from Example 4 and Comparative Examples 8 and 9 that acetic acid as a catalyst for the hydrolysis of siloxane is more conducive to improving the light transmittance of the aerogel material; this is because the rate at which acetic acid promotes the hydrolysis of methyl alkoxy silane can better adapt to the rate at which the polyether nonionic surfactant combines with the methyl alkoxy silane to form a strong hydrogen bond, which is conducive to the formation of a uniform and continuous double-skeleton network structure; thereby, the aerogel material has better light transmittance.

[0150] It should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a transparent flexible polysilsesquioxane monolithic aerogel, the preparation method comprising: S1: a polyether nonionic surfactant and an acetic acid aqueous solution are stirred evenly, and then methyl alkoxy silane is added to prepare a silane precursor solution; S2: adding an alkaline catalyst to the silane precursor solution described in S1, stirring evenly, and preparing a wet gel in an oven; S3: The wet gel described in S2 is subjected to gradient replacement by a water-ethanol system, and after the replacement, it is dried to obtain a complete transparent flexible polysilsesquioxane aerogel material; The addition amount of the polyether nonionic surfactant is 1-9%, and the silicon source is selected from silane with a mass percentage of 20-50%.

2. The method for preparing a transparent flexible polysilsesquioxane monolithic aerogel according to claim 1, characterized in that: The addition amount of the polyether nonionic surfactant is preferably 3-5%, and the methyl alkoxy silane is preferably 25-35% by mass of silane.

3. The method for preparing a transparent flexible polysilsesquioxane monolithic aerogel according to claim 1, characterized in that: The type of the polyether nonionic surfactant is selected from one or more of propylene glycol block polyether, polyoxyethylene ether nonionic surfactant, polyol ester nonionic surfactant, HSH polyether polyol, polyoxyethylene polyoxypropylene ether block copolymer or other commercially available specific types of polyether nonionic surfactants; Furthermore, the type of the polyether nonionic surfactant is preferably selected from polyoxyethylene polyoxypropylene ether block copolymers.

4. The method for preparing a transparent flexible polysilsesquioxane monolithic aerogel according to claim 1, characterized in that: The methylalkoxy silane is selected from one or more of methyltrimethoxysilane, methyltriethoxysilane and polydimethylsiloxane.

5. The method for preparing a transparent flexible polysilsesquioxane monolithic aerogel according to claim 1, characterized in that: The alkaline catalyst includes one or more of ammonia water, urea, triethylamine, tetramethylammonium hydroxide, and tetraethylammonium hydroxide.

6. The method for preparing a transparent flexible polysilsesquioxane monolithic aerogel according to claim 1, characterized in that: The content of the alkaline catalyst is 2-4%; Furthermore, the content of the alkaline catalyst is preferably 2.5-3%.

7. The method for preparing a transparent flexible polysilsesquioxane monolithic aerogel according to claim 1, characterized in that: The mass fraction of acetic acid in S1 is selected from 0.01-0.3%.

8. The method for preparing a transparent flexible polysilsesquioxane monolithic aerogel according to claim 1, characterized in that: The oven temperature in S2 is selected from 50-80°C.

9. The method for preparing a transparent flexible polysilsesquioxane monolithic aerogel according to claim 1, characterized in that: In S3, the drying method is selected from one of CO2 supercritical drying, vacuum drying or freeze drying.

10. Application of a transparent flexible polysilsesquioxane monolithic aerogel in architectural glass, wherein the architectural glass field includes windows, curtain walls, and skylights in one or more places such as airports, libraries, office buildings, residential buildings, schools, and hospitals.