Anti-oxidation rubber material for printing rubber blanket and preparation method of anti-oxidation rubber material

By adding high-efficiency antioxidants and mercapto-modified boron nitride nanosheets to the printing blanket material, the problems of easy oxidation and wear of traditional printing blankets are solved, the antioxidant and mechanical properties are improved, the service life is extended, and the thermal conductivity is enhanced.

CN119019768AActive Publication Date: 2024-11-26KOMPASS TECH INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411206394.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-26
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

Traditional printing blanket materials are prone to oxidation and wear during use, which significantly shortens their service life and affects the quality of printed materials.

Method used

Antioxidant rubber materials are prepared by using natural rubber, EPDM rubber and styrene-butadiene rubber as bases, adding high-efficiency antioxidants and mercapto-modified boron nitride nanosheets, and then mixing and vulcanizing. The antioxidant and mechanical properties of the materials are improved by combining mercapto-olefin click reaction and coupling agent modification.

Benefits of technology

It significantly improves the oxidation resistance and abrasion resistance of printing blankets, extends their service life, and has excellent thermal conductivity, meeting the environmental protection requirements of the modern printing industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the field of printing rubber blankets, in particular to an anti-oxidation rubber material for printing rubber blankets and a preparation method of the anti-oxidation rubber material, which are used for solving the problems that the traditional printing rubber blanket material is easily oxidized and abraded in the use process, the service life is greatly shortened, the performance is reduced and the quality of printed matters is influenced. According to the preparation method, an efficient antioxidant is added into the rubber material, so that free radicals can be effectively captured and cleared, the oxidation resistance is remarkably improved, then sulfydryl modified boron nitride nanosheets are added, so that the rubber material keeps good flexibility, meanwhile, the strength and hardness are improved, and the requirement of the printing rubber blanket for mechanical properties is met; meanwhile, the wear resistance of the printing rubber blanket is improved, and the sulfydryl modified boron nitride nanosheets have excellent heat conduction performance, so that heat can be quickly conducted out when the printing rubber blanket is used in a thermal environment, the thermal aging oxidation performance of the printing rubber blanket is further improved, and the durability of the printing rubber blanket is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of printing rubber blankets, and in particular to an anti-oxidation rubber material for printing rubber blankets and a preparation method thereof. Background Art

[0002] As a key component of a printing press, the performance of the printing blanket directly affects the quality and production efficiency of printed products. During the printing process, the printing blanket needs to withstand greater pressure and friction, and also needs to come into contact with various inks, solvents and other chemicals in a hot environment. Therefore, traditional printing blanket materials are susceptible to oxidation and wear during use, which greatly shortens their service life and causes performance degradation, affecting the quality of printed products.

[0003] Therefore, developing an antioxidant rubber material for printing blanket and a preparation method thereof is of great significance for improving the service life and printing quality of the printing blanket. Summary of the invention

[0004] In order to overcome the above-mentioned technical problems, the purpose of the present invention is to provide an antioxidant rubber material for a printing blanket and a preparation method thereof, which solves the problem that traditional printing blanket materials are susceptible to oxidation and wear during use, greatly shortening their service life, and causing performance degradation, affecting the quality of printed products.

[0005] The purpose of the present invention can be achieved by the following technical solutions: An anti-oxidation rubber material for printing rubber blanket comprises the following components in parts by weight: 65-75 parts of natural rubber, 25-35 parts of EPDM rubber, 18-24 parts of styrene-butadiene rubber, 2.5-11.5 parts of high-efficiency antioxidant, 12-18 parts of mercapto-modified boron nitride nanosheets, 1-3 parts of sulfur and 1-3 parts of accelerator TMTD.

[0006] As a further solution of the present invention: the highly effective antioxidant is prepared by the following steps: Step A1: adding hexachlorocyclotriphosphazene, anhydrous potassium carbonate, p-phenylenediamine and anhydrous acetonitrile into a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, introducing nitrogen protection, stirring the reaction for 15-20 minutes at a temperature of 20-25° C. and a stirring rate of 300-400 r / min, then heating to reflux and continuing to stir the reaction for 15-20 hours, after the reaction is completed, cooling the reaction product to room temperature, then vacuum filtering, washing the filter cake with distilled water 2-3 times, then placing it in a vacuum drying oven, and drying it at a temperature of 60-65° C. for 2-4 hours to obtain intermediate 1; Step A2: 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid and chloroform are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a constant pressure dropping funnel, and nitrogen is introduced for protection. The mixture is stirred for reaction for 15-20 minutes at a temperature of 25-30° C. and a stirring rate of 300-400 r / min. Then, thionyl chloride is added dropwise while stirring, and the dropping rate is controlled to be 1-2 drops / s. After the addition is completed, the temperature is raised to 50-55° C. and the stirring reaction is continued for 4-5 hours. After the reaction is completed, the reaction product is cooled to room temperature, and then the solvent is removed by rotary evaporation to obtain intermediate 2; Step A3: Add intermediate 1, intermediate 2 and anhydrous acetonitrile to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a constant pressure dropping funnel, introduce nitrogen protection, stir the reaction for 15-20 minutes at a temperature of 20-25°C and a stirring rate of 300-400r / min, then add triethylamine solution dropwise while stirring until the pH is 9-10, control the dropping rate to 1-2 drops / s, and continue to stir the reaction for 10-15 hours at a temperature of 60-65°C after the dropwise addition is completed. After the reaction is completed, the reaction product is cooled to room temperature, and then the solvent is removed by rotary evaporation, and then added to dichloromethane, and then washed with sodium bicarbonate solution, hydrochloric acid solution and saturated brine for 2-3 times in sequence, and then allowed to stand for stratification, and the organic phase is dried over anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain a high-efficiency antioxidant.

[0007] As a further scheme of the present invention: the usage ratio of the hexachlorocyclotriphosphazene, anhydrous potassium carbonate, p-phenylenediamine and anhydrous acetonitrile in step A1 is 10 mmol: 65-75 mmol: 60 mmol: 80-100 mL.

[0008] As a further embodiment of the present invention: the usage ratio of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, chloroform and thionyl chloride in step A2 is 10 mmol:40-50 mL:8-12 mL.

[0009] As a further scheme of the present invention: the usage ratio of the intermediate 1, intermediate 2 and anhydrous acetonitrile in step A3 is 10 mmol: 65-75 mmol: 60-80 mL.

[0010] As a further solution of the present invention: the triethylamine solution in step A3 is a solution with a molar concentration of 0.3-0.5 mol / L formed by dissolving triethylamine in anhydrous acetonitrile.

[0011] As a further solution of the present invention: the mass fraction of the sodium bicarbonate solution in step A3 is 5-7%, and the mass fraction of the hydrochloric acid solution is 8-10%.

[0012] As a further solution of the present invention: the thiol-modified boron nitride nanosheets are prepared by the following steps: Step B1: adding hexagonal boron nitride and anhydrous glucose into a ball mill, milling for 12-16 hours at a ball-to-material ratio of 8-10:1 and a ball milling speed of 300-400 r / min, then adding into deionized water and standing for 15-25 minutes, then centrifuging, placing the precipitate in a vacuum drying oven, and drying at a temperature of 40-45° C. for 3-5 hours to obtain boron nitride nanosheets; Step B2: Add coupling agent KH-590, anhydrous ethanol and deionized water into a three-necked flask equipped with a stirrer, a thermometer and an air duct, introduce nitrogen protection, stir and react for 30-40 minutes at a temperature of 20-25°C and a stirring rate of 300-400r / min, then add boron nitride nanosheets and continue stirring and reacting for 8-10 hours at a temperature of 75-80°C. After the reaction is completed, the reaction product is cooled to room temperature and then centrifuged. The precipitate is placed in a vacuum drying oven and dried at a temperature of 60-65°C for 6-8 hours to obtain thiol-modified boron nitride nanosheets.

[0013] As a further solution of the present invention: the usage ratio of the hexagonal boron nitride and anhydrous glucose in step B1 is 1g:8-10g.

[0014] As a further solution of the present invention: the usage ratio of the coupling agent KH-590, anhydrous ethanol, deionized water and boron nitride nanosheets in step B2 is 1.5-8.5 g: 80-85 mL: 10-15 mL: 5 g.

[0015] As a further solution of the present invention: a method for preparing an oxidation-resistant rubber material for a printing blanket comprises the following steps: Step 1: weigh 65-75 parts of natural rubber, 25-35 parts of EPDM rubber, 18-24 parts of styrene-butadiene rubber, 2.5-11.5 parts of high-efficiency antioxidant, 12-18 parts of mercapto-modified boron nitride nanosheets, 1-3 parts of sulfur and 1-3 parts of accelerator TMTD according to weight parts, and set aside; Step 2: Put natural rubber, EPDM rubber and styrene-butadiene rubber into an internal mixer, mix them at a temperature of 140-160° C. for 10-20 minutes, then add a high-efficiency antioxidant, mercapto-modified boron nitride nanosheets, sulfur and accelerator TMTD and continue mixing for 10-20 minutes to obtain an internal mixer rubber compound; Step 3: Put the mixed rubber material into an open mill and thin-pass it 3-5 times, then put it into a vulcanizer, and vulcanize it at a temperature of 160-180° C. for 10-20 minutes to obtain an antioxidant rubber material for printing rubber blanket.

[0016] Beneficial effects of the present invention: The invention discloses an antioxidant rubber material for printing rubber blanket and a preparation method thereof. The method comprises the following steps: mixing natural rubber, EPDM rubber and styrene-butadiene rubber in an internal mixer, then adding a high-efficiency antioxidant, mercapto-modified boron nitride nanosheets, sulfur and accelerator TMTD and continuing mixing to obtain an internal mixing rubber compound. The internal mixing rubber compound is placed in an open mixer for thin-passing, and then placed in a vulcanizer for vulcanization to obtain the antioxidant rubber material for printing rubber blanket. In the preparation method, the high-efficiency antioxidant is added to the rubber material to effectively capture and remove free radicals, thereby preventing the rubber material from being oxidized during use. Chemical degradation can significantly improve the antioxidant performance. Then, the addition of mercapto-modified boron nitride nanosheets allows the rubber material to maintain good flexibility while improving its strength and hardness, meeting the requirements of the printing rubber blanket for mechanical properties, while improving the wear resistance of the printing rubber blanket and extending its service life. In addition, the mercapto-modified boron nitride nanosheets have excellent thermal conductivity, which allows the printing rubber blanket to quickly conduct heat when used in a hot environment, further improving its thermal aging and oxidation performance, and improving the durability of the printing rubber blanket, which meets the environmental protection requirements of the modern printing industry and has broad market application prospects.

[0017] In the process of preparing an antioxidant rubber material for printing rubber blanket, a high-efficiency antioxidant is firstly prepared. Firstly, hexachlorocyclotriphosphazene and p-phenylenediamine are reacted, and the chlorine atom on the hexachlorocyclotriphosphazene reacts with an amino group on the p-phenylenediamine to obtain intermediate 1. Then, 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid and dithionyl chloride are reacted, and the carboxyl group on the 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid is converted into an acyl chloride group by dithionyl chloride to obtain intermediate 2. Finally, intermediate 1 and intermediate 2 are reacted, and the amino group on intermediate 1 reacts with the acyl chloride group on intermediate 2, and a large number of hindered phenol structures are introduced to obtain a high-efficiency antioxidant. The molecular structure of the high-efficiency antioxidant contains a large number of hindered phenol structures, which can effectively capture and remove free radicals, and can give it excellent antioxidant performance under the synergistic effect of a large number of hindered phenol structures. Therefore, adding the high-efficiency antioxidant to the rubber material can significantly improve the antioxidant performance of the rubber material and extend the service life of the printing rubber blanket.

[0018] In the process of preparing the antioxidant rubber material for printing rubber blanket, a thiol-modified boron nitride nanosheet was also prepared. First, glucose was used as a ball milling aid. The impact between the grinding ball and the material and the temperature rise of the material caused by the impact friction during the ball milling process were used to achieve the exfoliation modification of the hexagonal boron nitride sheet. Glucose was grafted and a large number of hydroxyl groups were introduced to obtain boron nitride nanosheets. Then, the boron nitride nanosheets were modified using the coupling agent KH-590. The siloxane on the coupling agent KH-590 was hydrolyzed to form silanol, which could undergo dehydration condensation with the hydroxyl groups on the boron nitride nanosheets. Organosilicon and a large number of mercapto groups are introduced to obtain mercapto-modified boron nitride nanosheets; the boron nitride nanosheets have excellent mechanical properties and thermal conductivity, and the modified boron nitride nanosheets have excellent dispersion properties, so that they can be evenly distributed in the rubber material, and can also participate in the cross-linking reaction of the rubber through the mercapto-ene click reaction, increase the interface interaction, form a boron nitride nanosheet particle network, and improve the consistency of the thermal conductivity and mechanical properties of the rubber material, which can greatly improve the mechanical properties and thermal conductivity of the rubber material, and further extend the service life of the printing rubber blanket. DETAILED DESCRIPTION

[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] Embodiment 1: This embodiment is a method for preparing an oxidation-resistant rubber material for a printing blanket, comprising the following steps: Step S1: 10 mmol hexachlorocyclotriphosphazene, 65 mmol anhydrous potassium carbonate, 60 mmol p-phenylenediamine and 80 mL anhydrous acetonitrile were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred for reaction at a temperature of 20° C. and a stirring rate of 300 r / min for 15 min, and then the temperature was raised to reflux and the stirring reaction was continued for 15 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered. The filter cake was washed twice with distilled water, and then placed in a vacuum drying oven and dried at a temperature of 60° C. for 2 h to obtain intermediate 1; Step S2: 10 mmol 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid and 40 mL chloroform were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a constant pressure dropping funnel, and nitrogen was introduced for protection. The mixture was stirred for reaction at a temperature of 25° C. and a stirring rate of 300 r / min for 15 min, and then 8 mL thionyl chloride was added dropwise while stirring, and the dropping rate was controlled to be 1 drop / s. After the addition was completed, the temperature was raised to 50° C. and the stirring reaction was continued for 4 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain intermediate 2; Step S3: 10 mmol of intermediate 1, 65 mmol of intermediate 2 and 60 mL of anhydrous acetonitrile are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a constant pressure dropping funnel, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 20° C. and a stirring rate of 300 r / min for 15 min, and then a triethylamine solution with a molar concentration of 0.3 mol / L formed by dissolving triethylamine in anhydrous acetonitrile is added dropwise while stirring until the pH is 9, and the dropping rate is controlled to be 1 drop / s. After the dropwise addition is completed, the temperature is raised to 60° C. and the stirring reaction is continued for 10 h. After the reaction is completed, the reaction product is cooled to room temperature, and then the solvent is removed by rotary evaporation, and then added to dichloromethane, and then washed twice with a sodium bicarbonate solution with a mass fraction of 5%, a hydrochloric acid solution with a mass fraction of 8%, and a saturated brine, and then allowed to stand for stratification, and the organic phase is dried over anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain a high-efficiency antioxidant; Step S4: adding 1 g of hexagonal boron nitride and 8 g of anhydrous glucose into a ball mill, milling for 12 h at a ball-to-material ratio of 8:1 and a ball milling speed of 300 r / min, then adding it into deionized water and letting it stand for 15 min, then centrifuging it, placing the precipitate in a vacuum drying oven, and drying it at a temperature of 40° C. for 3 h to obtain boron nitride nanosheets; Step S5: 1.5 g of coupling agent KH-590, 80 mL of anhydrous ethanol and 10 mL of deionized water were added to a three-necked flask equipped with a stirrer, a thermometer and an air guide tube, and nitrogen was introduced for protection. The mixture was stirred at 20° C. and a stirring rate of 300 r / min for 30 min. Then, 5 g of boron nitride nanosheets were added and the mixture was heated to 75° C. and stirred for 8 h. After the reaction, the reaction product was cooled to room temperature and then centrifuged. The precipitate was placed in a vacuum drying oven and dried at 60° C. for 6 h to obtain thiol-modified boron nitride nanosheets. Step S6: weigh 65 parts of natural rubber, 25 parts of EPDM rubber, 18 parts of styrene-butadiene rubber, 2.5 parts of high-efficiency antioxidant, 12 parts of mercapto-modified boron nitride nanosheets, 1 part of sulfur and 1 part of accelerator TMTD according to weight parts, and set aside; Step S7: natural rubber, EPDM rubber and styrene-butadiene rubber are put into an internal mixer, and mixed at a temperature of 140° C. for 10 minutes, and then a high-efficiency antioxidant, mercapto-modified boron nitride nanosheets, sulfur and accelerator TMTD are added and mixed for another 10 minutes to obtain an internal mixer rubber material; Step S8: Put the mixed rubber material into an open mixer and thin-pass it three times, then put it into a vulcanizer and vulcanize it at a temperature of 160° C. for 10 minutes to obtain an antioxidant rubber material for a printing blanket.

[0021] Embodiment 2: This embodiment is a method for preparing an oxidation-resistant rubber material for a printing blanket, comprising the following steps: Step S1: 10 mmol hexachlorocyclotriphosphazene, 70 mmol anhydrous potassium carbonate, 60 mmol p-phenylenediamine and 90 mL anhydrous acetonitrile were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred for reaction at a temperature of 22° C. and a stirring rate of 350 r / min for 18 min, and then the mixture was heated to reflux and continued to stir for 18 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered. The filter cake was washed twice with distilled water, and then placed in a vacuum drying oven and dried at a temperature of 62° C. for 3 h to obtain intermediate 1; Step S2: 10 mmol 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid and 45 mL chloroform were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a constant pressure dropping funnel, and nitrogen was introduced for protection. The mixture was stirred for reaction at 28° C. and a stirring rate of 350 r / min for 18 min, and then 10 mL thionyl chloride was added dropwise while stirring, and the dropping rate was controlled to be 1 drop / s. After the addition was completed, the temperature was raised to 52° C. and the stirring reaction was continued for 4.5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain intermediate 2; Step S3: 10 mmol of intermediate 1, 70 mmol of intermediate 2 and 70 mL of anhydrous acetonitrile are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a constant pressure dropping funnel, and nitrogen is introduced for protection. The reaction is stirred for 18 min at a temperature of 22 ° C and a stirring rate of 350 r / min, and then a triethylamine solution with a molar concentration of 0.4 mol / L formed by dissolving triethylamine in anhydrous acetonitrile is added dropwise while stirring until the pH is 9.5, and the dropping rate is controlled to 1 drop / s. After the dropwise addition is completed, the temperature is raised to 62 ° C and the stirring reaction is continued for 12 h. After the reaction is completed, the reaction product is cooled to room temperature, and then the solvent is removed by rotary evaporation, and then added to dichloromethane, and then washed twice with a sodium bicarbonate solution with a mass fraction of 6%, a hydrochloric acid solution with a mass fraction of 9%, and a saturated brine, and then allowed to stand for stratification, and the organic phase is dried over anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain a high-efficiency antioxidant; Step S4: adding 1 g of hexagonal boron nitride and 9 g of anhydrous glucose into a ball mill, milling for 14 h at a ball-to-material ratio of 9:1 and a ball milling speed of 350 r / min, then adding the mixture into deionized water and letting it stand for 20 min, then centrifuging, placing the precipitate in a vacuum drying oven, and drying it at 42° C. for 4 h to obtain boron nitride nanosheets; Step S5: 5 g of coupling agent KH-590, 82 mL of anhydrous ethanol and 12 mL of deionized water were added to a three-necked flask equipped with a stirrer, a thermometer and an air guide tube, and nitrogen was introduced for protection. The mixture was stirred at 22° C. and a stirring rate of 350 r / min for 35 min. Then, 5 g of boron nitride nanosheets were added and the mixture was heated to 78° C. and stirred for 9 h. After the reaction, the reaction product was cooled to room temperature and then centrifuged. The precipitate was placed in a vacuum drying oven and dried at 62° C. for 7 h to obtain thiol-modified boron nitride nanosheets. Step S6: weigh 70 parts of natural rubber, 30 parts of EPDM rubber, 21 parts of styrene-butadiene rubber, 7 parts of high-efficiency antioxidant, 15 parts of mercapto-modified boron nitride nanosheets, 2 parts of sulfur and 2 parts of accelerator TMTD according to weight parts, and set aside; Step S7: natural rubber, EPDM rubber and styrene-butadiene rubber are put into an internal mixer, and mixed at a temperature of 150° C. for 15 minutes, and then a high-efficiency antioxidant, mercapto-modified boron nitride nanosheets, sulfur and accelerator TMTD are added and mixed for another 15 minutes to obtain an internal mixer rubber compound; Step S8: Put the mixed rubber material into an open mixer and thin-pass it 4 times, then put it into a vulcanizer and vulcanize it at a temperature of 170° C. for 15 minutes to obtain an antioxidant rubber material for a printing blanket.

[0022] Embodiment 3: This embodiment is a method for preparing an oxidation-resistant rubber material for a printing blanket, comprising the following steps: Step S1: 10 mmol hexachlorocyclotriphosphazene, 75 mmol anhydrous potassium carbonate, 60 mmol p-phenylenediamine and 100 mL anhydrous acetonitrile were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred for reaction at a temperature of 25° C. and a stirring rate of 400 r / min for 20 min, and then the temperature was raised to reflux and the stirring reaction was continued for 20 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered. The filter cake was washed with distilled water 3 times, and then placed in a vacuum drying oven and dried at a temperature of 65° C. for 4 h to obtain intermediate 1; Step S2: 10 mmol 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid and 50 mL chloroform were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a constant pressure dropping funnel, and nitrogen was introduced for protection. The mixture was stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 20 min. Then, 12 mL thionyl chloride was added dropwise while stirring, and the dropping rate was controlled to be 2 drops / s. After the addition was completed, the temperature was raised to 55° C. and the stirring reaction was continued for 5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain intermediate 2; Step S3: 10 mmol of intermediate 1, 75 mmol of intermediate 2 and 80 mL of anhydrous acetonitrile are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a constant pressure dropping funnel, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 25° C. and a stirring rate of 400 r / min for 20 min, and then a triethylamine solution with a molar concentration of 0.5 mol / L formed by dissolving triethylamine in anhydrous acetonitrile is added dropwise while stirring until the pH is 10, and the dropping rate is controlled to be 2 drops / s. After the dropwise addition is completed, the temperature is raised to 65° C. and the stirring reaction is continued for 15 h. After the reaction is completed, the reaction product is cooled to room temperature, and then the solvent is removed by rotary evaporation, and then added to dichloromethane, and then washed three times with a sodium bicarbonate solution with a mass fraction of 7%, a hydrochloric acid solution with a mass fraction of 10%, and a saturated brine, and then allowed to stand for stratification, and the organic phase is dried over anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain a high-efficiency antioxidant; Step S4: adding 1 g of hexagonal boron nitride and 10 g of anhydrous glucose into a ball mill, milling for 16 h at a ball-to-material ratio of 10:1 and a ball mill speed of 400 r / min, then adding the mixture into deionized water and letting it stand for 25 min, then centrifuging, placing the precipitate in a vacuum drying oven, and drying it at 45° C. for 5 h to obtain boron nitride nanosheets; Step S5: 8.5 g of coupling agent KH-590, 85 mL of anhydrous ethanol and 15 mL of deionized water are added to a three-necked flask equipped with a stirrer, a thermometer and an air guide tube, and nitrogen is introduced for protection. The mixture is stirred at 25° C. and a stirring rate of 400 r / min for 40 min, and then 5 g of boron nitride nanosheets are added and the mixture is heated to 80° C. and stirred for 10 h. After the reaction is completed, the reaction product is cooled to room temperature and then centrifuged. The precipitate is placed in a vacuum drying oven and dried at 65° C. for 8 h to obtain thiol-modified boron nitride nanosheets; Step S6: weigh 75 parts of natural rubber, 35 parts of EPDM rubber, 24 parts of styrene-butadiene rubber, 11.5 parts of high-efficiency antioxidant, 18 parts of mercapto-modified boron nitride nanosheets, 3 parts of sulfur and 3 parts of accelerator TMTD according to weight parts, and set aside; Step S7: putting natural rubber, EPDM rubber and styrene-butadiene rubber into an internal mixer, mixing at a temperature of 160° C. for 20 min, then adding a high-efficiency antioxidant, mercapto-modified boron nitride nanosheets, sulfur and accelerator TMTD and continuing to mix for 20 min to obtain an internal mixer rubber compound; Step S8: putting the mixed rubber material into an open mixer and thinning it for 5 times, then putting it into a vulcanizer and vulcanizing it at a temperature of 180° C. for 20 minutes to obtain an antioxidant rubber material for a printing blanket.

[0023] Comparative Example 1: This comparative example is a method for preparing an oxidation-resistant rubber material for a printing blanket, comprising the following steps: Step S1: weigh 75 parts of natural rubber, 35 parts of EPDM rubber, 24 parts of styrene-butadiene rubber, 3 parts of sulfur and 3 parts of accelerator TMTD according to weight parts and set aside; Step S2: putting natural rubber, EPDM rubber and styrene-butadiene rubber into an internal mixer, mixing them at a temperature of 160° C. for 20 minutes, then adding sulfur and accelerator TMTD and continuing to mix for 20 minutes to obtain an internal mixer rubber material; Step S3: putting the mixed rubber material into an open mixer and thinning it for 5 times, then putting it into a vulcanizer and vulcanizing it at a temperature of 180° C. for 20 minutes to obtain an antioxidant rubber material for a printing blanket.

[0024] Comparative Example 2: This comparative example is a method for preparing an oxidation-resistant rubber material for a printing blanket, comprising the following steps: Step S1: weigh 75 parts of natural rubber, 35 parts of EPDM rubber, 24 parts of styrene-butadiene rubber, 11.5 parts of antioxidant BHT, 3 parts of sulfur and 3 parts of accelerator TMTD according to weight parts, and set aside; Step S2: natural rubber, EPDM rubber and styrene-butadiene rubber are put into an internal mixer, and mixed at a temperature of 160° C. for 20 minutes, and then antioxidant BHT, sulfur and accelerator TMTD are added and mixed for another 20 minutes to obtain an internal mixer rubber material; Step S3: putting the mixed rubber material into an open mixer and thinning it for 5 times, then putting it into a vulcanizer and vulcanizing it at a temperature of 180° C. for 20 minutes to obtain an antioxidant rubber material for a printing blanket.

[0025] Comparative Example 3: This comparative example is a method for preparing an oxidation-resistant rubber material for a printing blanket, comprising the following steps: Step S1: 10 mmol hexachlorocyclotriphosphazene, 75 mmol anhydrous potassium carbonate, 60 mmol p-phenylenediamine and 100 mL anhydrous acetonitrile were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred for reaction at a temperature of 25° C. and a stirring rate of 400 r / min for 20 min, and then the temperature was raised to reflux and the stirring reaction was continued for 20 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered. The filter cake was washed with distilled water 3 times, and then placed in a vacuum drying oven and dried at a temperature of 65° C. for 4 h to obtain intermediate 1; Step S2: 10 mmol 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid and 50 mL chloroform were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a constant pressure dropping funnel, and nitrogen was introduced for protection. The mixture was stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 20 min. Then, 12 mL thionyl chloride was added dropwise while stirring, and the dropping rate was controlled to be 2 drops / s. After the addition was completed, the temperature was raised to 55° C. and the stirring reaction was continued for 5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain intermediate 2; Step S3: 10 mmol of intermediate 1, 75 mmol of intermediate 2 and 80 mL of anhydrous acetonitrile are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a constant pressure dropping funnel, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 25° C. and a stirring rate of 400 r / min for 20 min, and then a triethylamine solution with a molar concentration of 0.5 mol / L formed by dissolving triethylamine in anhydrous acetonitrile is added dropwise while stirring until the pH is 10, and the dropping rate is controlled to be 2 drops / s. After the dropwise addition is completed, the temperature is raised to 65° C. and the stirring reaction is continued for 15 h. After the reaction is completed, the reaction product is cooled to room temperature, and then the solvent is removed by rotary evaporation, and then added to dichloromethane, and then washed three times with a sodium bicarbonate solution with a mass fraction of 7%, a hydrochloric acid solution with a mass fraction of 10%, and a saturated brine, and then allowed to stand for stratification, and the organic phase is dried over anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain a high-efficiency antioxidant; Step S4: weigh 75 parts of natural rubber, 35 parts of EPDM rubber, 24 parts of styrene-butadiene rubber, 11.5 parts of high-efficiency antioxidant, 3 parts of sulfur and 3 parts of accelerator TMTD according to weight parts, and set aside; Step S5: putting natural rubber, EPDM rubber and styrene-butadiene rubber into an internal mixer, mixing at a temperature of 160° C. for 20 min, then adding a high-efficiency antioxidant, sulfur and accelerator TMTD and continuing to mix for 20 min to obtain an internal mixer rubber material; Step S6: Put the mixed rubber material into an open mixer and thin-pass it for 5 times, then put it into a vulcanizer and vulcanize it at a temperature of 180° C. for 20 minutes to obtain an antioxidant rubber material for a printing blanket.

[0026] Comparative Example 4: This comparative example is a method for preparing an oxidation-resistant rubber material for a printing blanket, comprising the following steps: Step S1: 1 g of hexagonal boron nitride and 10 g of anhydrous glucose were added to a ball mill, and the mixture was ball milled for 16 h at a ball-to-material ratio of 10:1 and a ball milling speed of 400 r / min. The mixture was then added to deionized water and allowed to stand for 25 min, followed by centrifugation. The precipitate was placed in a vacuum drying oven and dried at 45° C. for 5 h to obtain boron nitride nanosheets. Step S2: 8.5 g of coupling agent KH-590, 85 mL of anhydrous ethanol and 15 mL of deionized water were added to a three-necked flask equipped with a stirrer, a thermometer and an air guide tube, and nitrogen was introduced for protection. The mixture was stirred at 25° C. and a stirring rate of 400 r / min for 40 min. Then, 5 g of boron nitride nanosheets were added and the mixture was heated to 80° C. and the stirring reaction was continued for 10 h. After the reaction was completed, the reaction product was cooled to room temperature and then centrifuged. The precipitate was placed in a vacuum drying oven and dried at 65° C. for 8 h to obtain thiol-modified boron nitride nanosheets. Step S3: weigh 75 parts of natural rubber, 35 parts of EPDM rubber, 24 parts of styrene-butadiene rubber, 18 parts of mercapto-modified boron nitride nanosheets, 3 parts of sulfur and 3 parts of accelerator TMTD according to weight parts, and set aside; Step S4: putting natural rubber, EPDM rubber and styrene-butadiene rubber into an internal mixer, mixing them at a temperature of 160° C. for 20 min, then adding mercapto-modified boron nitride nanosheets, sulfur and accelerator TMTD and continuing to mix for 20 min to obtain an internal mixer rubber compound; Step S5: putting the mixed rubber material into an open mixer and thinning it for 5 times, then putting it into a vulcanizer and vulcanizing it at a temperature of 180° C. for 20 minutes to obtain an antioxidant rubber material for a printing blanket.

[0027] The performance of the anti-oxidation rubber materials for printing blankets in Examples 1-3 and Comparative Examples 1-4 was tested, and the test results are shown in the following table:

[0028] Referring to the data in the above table, it can be seen that adding a high-efficiency antioxidant can effectively improve the antioxidant properties of rubber materials, and adding mercapto-modified boron nitride nanosheets can effectively improve the mechanical properties of rubber materials. Under the synergistic effect of the high-efficiency antioxidant and mercapto-modified boron nitride nanosheets, the obtained rubber material has excellent antioxidant and mechanical properties.

[0029] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0030] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. An anti-oxidation rubber material for a printing blanket, characterized in that: It includes the following components by weight: 65-75 parts of natural rubber, 25-35 parts of EPDM rubber, 18-24 parts of styrene-butadiene rubber, 2.5-11.5 parts of high-efficiency antioxidant, 12-18 parts of mercapto-modified boron nitride nanosheets, 1-3 parts of sulfur and 1-3 parts of accelerator TMTD; Wherein, the high-efficiency antioxidant is prepared by the following steps: Step A1: stirring hexachlorocyclotriphosphazene, anhydrous potassium carbonate, p-phenylenediamine and anhydrous acetonitrile for reaction, cooling the reaction product after the reaction is completed, and then vacuum filtering, washing and drying the filter cake to obtain intermediate 1; Step A2: 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid and chloroform are stirred for reaction, and then thionyl chloride is added dropwise while stirring. After the addition is completed, the stirring reaction is continued. After the reaction is completed, the reaction product is cooled and then rotary evaporated to obtain intermediate 2; Step A3: Stir the intermediate 1, intermediate 2 and anhydrous acetonitrile for reaction, then add triethylamine solution dropwise while stirring, continue stirring the reaction after the addition is complete, cool the reaction product after the reaction is complete, then rotary evaporate, then add it to dichloromethane, then wash it with sodium bicarbonate solution, hydrochloric acid solution and saturated brine in sequence, then stand and separate, dry the organic phase, then vacuum filter, and rotary evaporate the filtrate to obtain a high-efficiency antioxidant.

2. The anti-oxidation rubber material for printing blanket according to claim 1, characterized in that: The usage ratio of the hexachlorocyclotriphosphazene, anhydrous potassium carbonate, p-phenylenediamine and anhydrous acetonitrile in step A1 is 10 mmol: 65-75 mmol: 60 mmol: 80-100 mL.

3. The anti-oxidation rubber material for printing blanket according to claim 1, characterized in that: The usage ratio of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, chloroform and thionyl chloride in step A2 is 10 mmol: 40-50 mL: 8-12 mL.

4. The anti-oxidation rubber material for printing blanket according to claim 1, characterized in that: The usage ratio of the intermediate 1, intermediate 2 and anhydrous acetonitrile in step A3 is 10 mmol: 65-75 mmol: 60-80 mL.

5. The anti-oxidation rubber material for printing blanket according to claim 1, characterized in that: The triethylamine solution in step A3 is a solution with a molar concentration of 0.3-0.5 mol / L formed by dissolving triethylamine in anhydrous acetonitrile.

6. The anti-oxidation rubber material for printing blanket according to claim 1, characterized in that: The mass fraction of the sodium bicarbonate solution in step A3 is 5-7%, and the mass fraction of the hydrochloric acid solution is 8-10%.

7. The anti-oxidation rubber material for printing blanket according to claim 1, characterized in that: The thiol-modified boron nitride nanosheets are prepared by the following steps: Step B1: adding hexagonal boron nitride and anhydrous glucose into a ball mill for ball milling, then adding them into deionized water for standing, then centrifuging, and drying the precipitate to obtain boron nitride nanosheets; Step B2: The coupling agent KH-590, anhydrous ethanol and deionized water are stirred for reaction, and then the boron nitride nanosheets are added and the stirring reaction is continued. After the reaction is completed, the reaction product is cooled, centrifuged, and the precipitate is dried to obtain thiol-modified boron nitride nanosheets.

8. The anti-oxidation rubber material for printing blanket according to claim 7, characterized in that: The usage ratio of the hexagonal boron nitride and anhydrous glucose in step B1 is 1g:8-10g.

9. The anti-oxidation rubber material for printing blanket according to claim 7, characterized in that: The usage ratio of the coupling agent KH-590, anhydrous ethanol, deionized water and boron nitride nanosheets in step B2 is 1.5-8.5 g: 80-85 mL: 10-15 mL: 5 g.

10. A method for preparing an anti-oxidation rubber material for a printing blanket, characterized in that: The following steps are involved: Step 1: weigh 65-75 parts of natural rubber, 25-35 parts of EPDM rubber, 18-24 parts of styrene-butadiene rubber, 2.5-11.5 parts of high-efficiency antioxidant, 12-18 parts of mercapto-modified boron nitride nanosheets, 1-3 parts of sulfur and 1-3 parts of accelerator TMTD according to weight parts, and set aside; Step 2: Put natural rubber, EPDM rubber and styrene-butadiene rubber into an internal mixer, mix them at a temperature of 140-160° C. for 10-20 minutes, then add a high-efficiency antioxidant, mercapto-modified boron nitride nanosheets, sulfur and accelerator TMTD and continue mixing for 10-20 minutes to obtain an internal mixer rubber compound; Step 3: Put the mixed rubber material into an open mixer and thin-pass it 3-5 times, then put it into a vulcanizer, and vulcanize it at a temperature of 160-180° C. for 10-20 minutes to obtain an antioxidant rubber material for printing rubber blanket.

Citation Information

Patent Citations

  • High-temperature-resistant rubber guide wheel for centerless grinding machine

    CN105602119A

  • Special rubber material for tyre and preparation method thereof

    CN106243427A

  • High-dispersion amorphous carbon coated hexagonal boron nitride nanosheet and preparation method thereof

    CN112662449A

  • Preparation method, material and application of flexible neutron protection composite material with ordered arrangement of functionalized boron nitride nanosheets

    CN117866340A

  • Antistatic composite rubber plate and preparation method thereof

    CN118325207A