High-density polyethylene conductive composite material with isolation network and preparation method thereof

By coating graphene or edge graphene oxide on the surface of high-density polyethylene powder, a three-dimensional isolated conductive network is formed, and the problem of insufficient mechanical properties of polyethylene conductive composite materials is solved, and the combination of high conductivity and good mechanical properties is achieved. Its use in high-performance applications.

CN119019776AActive Publication Date: 2024-11-26EAST CHINA UNIV OF SCI & TECH +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411228611.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-26
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

The existing polyethylene conductive composite materials have insufficient mechanical properties under low conductivity thresholds, and the uneven distribution of conductive nanofillers leads to micro defects, limiting their application in the fields of high-performance anti-static, EMI shielding and sensing.

Method used

The mechanical shear mixed coating-high temperature pressing method is adopted to uniformly coat graphene or edge graphene oxide on the surface of high-density polyethylene powder to form a three-dimensional isolated conductive network, reducing the use of conductive fillers and improving mechanical properties.

Benefits of technology

Polyethylene materials with excellent conductivity and good mechanical properties are achieved under low conductive filler content, which significantly improves the mechanical properties of conductive composite materials and broadens their application range in the fields of antistatic, electromagnetic shielding and sensing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019776A_ABST
    Figure CN119019776A_ABST
Patent Text Reader

Abstract

The invention discloses a high-density polyethylene conductive composite material with an isolation network and a preparation method thereof, and the preparation method comprises the following steps: (1) uniformly and tightly coating the surface of high-density polyethylene powder with a conductive filler through mechanical shearing in a crushing mixer to obtain composite powder, the conductive filler is graphene or edge graphene oxide filler; and (2) carrying out hot press molding on the composite powder, and forming a three-dimensional conductive network in the material to obtain the high-density polyethylene conductive composite material with the isolation network. The negative influence of the isolation structure on the mechanical property is reduced to the greatest extent under high conductivity, the mutual contact efficiency of the conductive fillers is improved, and the insulation gap between the adjacent conductive fillers is reduced. And a stronger interface interaction is constructed between the polymer particles and the conductive filler, so that the polyethylene material with excellent conductivity and good mechanical properties is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of conductive polymers, in particular to a high-density polyethylene conductive composite material with an isolation network and a preparation method thereof. Background Art

[0002] Polyethylene has been widely used due to its advantages such as light weight, easy molding and processing, and high cost performance. However, due to its electrical insulation, static electricity easily accumulates on the surface of polyethylene products during use, causing harm. By blending conductive fillers with insulating polymers to prepare conductive polymer composites (CPC), stable and permanent antistatic properties can be obtained, which is the simplest and most effective way to eliminate static electricity hazards. For CPC prepared by traditional twin-screw extrusion and injection molding methods, conductive nanofillers are randomly distributed in the matrix, and a large amount of conductive nanofillers needs to be added to obtain sufficient conductivity, resulting in serious deterioration of the mechanical and processing properties of CPC, and no economic effect. Therefore, lowering the conductivity threshold and designing an effective conductive network is the key to preparing high-performance CPC.

[0003] Constructing a three-dimensional (3D) isolated carbon-based conductive nanofiller network in a polymer matrix is ​​an effective strategy to prepare CPCs with excellent conductivity. For isolated conductive polymer composites (s-CPCs), the carbon-based conductive nanofillers are not uniformly distributed throughout the polymer matrix, but are confined to the boundaries between polymer domains and distributed along specific pathways, forming a continuous conductive network. Compared with ordinary CPCs, this specific distribution of conductive fillers at the polymer domain interface leads to s-CPCs with efficient transport networks at extremely low conductivity thresholds, which is conducive to the development of new high-performance CPCs for wide applications in high-performance antistatic, EMI shielding, and sensing materials.

[0004] However, s-CPC still faces many challenges. Although a good isolation structure can be constructed by hot pressing polymer mixed particles coated with carbon-based conductive nanofillers, the selective distribution of nanofillers often leads to poor interfacial interaction between nanofillers and polymer matrix, and the nanofillers are severely aggregated on the isolation path to form abundant micro-defects. The mechanical properties of s-CPC are much lower than those of ordinary CPC composites with randomly distributed fillers, especially the elongation at break, which seriously hinders its application in many fields. Summary of the invention

[0005] The object of the present invention is to provide a high-density polyethylene conductive composite material with an isolation network and a preparation method thereof, which can prepare a polyethylene material with excellent conductive properties and good mechanical properties.

[0006] In one aspect of the present invention, the present invention proposes a method for preparing a high-density polyethylene conductive composite material with an isolation network, by constructing a three-dimensional conductive network with an isolation structure, achieving high conductivity of the material at a low filler content, and the preparation adopts a "mechanical shearing, mixing, coating-high temperature pressing" method. According to an embodiment of the present invention, the method comprises the following steps:

[0007] (1) in a pulverizing mixer, a conductive filler is uniformly and tightly coated on the surface of a high-density polyethylene powder (HDPE) by mechanical shearing to obtain a composite powder, wherein the conductive filler is a graphene (GNP) or an edge-oxidized graphene filler;

[0008] (2) hot pressing the composite powder to form a three-dimensional conductive network inside the material, thereby obtaining the high-density polyethylene conductive composite material with an isolation network.

[0009] In addition, the method for preparing the high-density polyethylene conductive composite material with an isolation network according to the above embodiment of the present invention may also have the following additional technical features:

[0010] In some embodiments of the present invention, in the step (1), the edge oxide graphene filler is prepared as follows: graphene is subjected to edge oxidation modification using nitric acid and potassium permanganate to obtain edge oxide graphene, and then a conductive polymer polyaniline is polymerized in situ on the surface of the edge oxide graphene to obtain an edge oxide graphene filler. In order to further improve the mechanical properties of polyethylene conductive composite materials with an isolation network under high conductivity, the present invention prepares an edge oxide graphene filler (PANI-EOG) of in-situ polymerized polyaniline. The coating effect of the conductive filler on the surface of the polymer particles is improved, the efficiency of the conductive filler contacting each other is increased, and the insulation gap between adjacent conductive fillers is reduced. In addition, a stronger interface interaction is constructed between the polymer particles and the carbon-based nanofiller, and while maintaining a highly conductive isolation network, the mechanical properties of s-CPC are significantly improved.

[0011] In some embodiments of the present invention, the method for preparing the edge oxidized graphene is as follows: adding graphene to a KMnO4 / HNO3 solution for chemical oxidation, and then centrifuging, washing, filtering, and drying to obtain the edge oxidized graphene.

[0012] In some embodiments of the present invention, the concentration of KMnO4 in the KMnO4 / HNO3 solution is 2.0-4.0 mg / ml;

[0013] The mass ratio of KMnO4 to graphene is 0.20-0.25; the temperature of the chemical oxidation is 50-55°C, the stirring speed is 800-1000rpm, and the reaction time is 24-36h; the centrifugal speed is 5000-8000rpm, and the centrifugal time is 8-10min; the washing is carried out with distilled water; the drying temperature is 55-60°C, and the drying time is 24-36h.

[0014] In some embodiments of the present invention, the specific steps of in situ polymerization of conductive polymer polyaniline on the surface of edge graphene oxide are as follows: edge graphene oxide is added to a hydrochloric acid solution and dispersed to obtain a uniform EOG dispersion, aniline monomer is added to the EOG dispersion and mixed evenly, and then APS solution is added dropwise. After the reaction is completed, the mixture is filtered, washed, and dried to obtain an edge graphene oxide filler.

[0015] In some embodiments of the present invention, the concentration of the hydrochloric acid solution is 1-1.1 mol / L; the mass ratio of the edge graphene oxide to the aniline monomer is 0.3-1; the reaction temperature is 20-25°C, the reaction time is 6-9h, the drying temperature is 55-60°C, and the drying time is 24-36h.

[0016] In some embodiments of the present invention, the step (1) is specifically as follows: using a pulverizer mixer, at a rotation speed of 34000-40000 rpm, shear mixing 1wt%-3wt% of a conductive filler and 50-400 μm of a high-density polyethylene powder, the shear mixing time is 2-3 min, and electrostatic adsorption is used to coat the GNP on the surface of the HDPE powder to obtain a composite powder.

[0017] In some embodiments of the present invention, in step (2), the hot pressing molding temperature is 132-147°C, the hot pressing pressure is 2-12 MPa, the hot pressing time is 8-10 min, and after the hot pressing is completed, the pressure is removed to allow the mold to cool naturally to room temperature.

[0018] In another aspect of the present invention, the present invention provides a high-density polyethylene conductive composite material with an isolation network prepared according to the method for preparing the high-density polyethylene conductive composite material with an isolation network.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1) The coating effect of the conductive coating on the surface of the polymer particles, the sufficient dispersion level of the conductive filler in the isolation network, the continuity and density of the isolated conductive path, and the interfacial adhesion strength between the conductive filler and the polymer particles are the key factors affecting the conductive properties and mechanical properties of s-CPC. In order to obtain the best comprehensive performance, the present invention minimizes the adverse effects of the isolation structure on the mechanical properties under high conductivity, optimizes the processing variables (for example, molding temperature, molding pressure, polymer particle size, etc.), and avoids the serious migration of carbon-based nanofillers to the internal matrix while building a tight isolation network, thereby achieving the preparation of polyethylene conductive composite materials with good conductivity and mechanical properties at a low content of conductive fillers.

[0021] 2) The present invention prepares PANI-EOG by simply modifying the conductive filler, which significantly improves the mechanical properties of the conductive composite material under high conductivity. This method is applicable to different isolated conductive polymer composite materials, and broadens the application of isolated conductive polymer composite materials in the fields of antistatic, electromagnetic shielding, and sensing.

[0022] 3) This patent is easy to implement, the equipment maintenance and cleaning are simple, and there are no stringent requirements on environmental conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a process flow chart for preparing a polyethylene conductive composite material with an isolation structure in Examples 1 to 18 of the present invention;

[0024] Figure 2 This is a SEM image of PANI-EOG prepared in Example 21 of the present invention;

[0025] Figure 3 a is a SEM image of the surface of the GNP@HDPE composite powder prepared in Example 17 of the present invention, Figure 3 b is a SEM image of the surface of the PANI-EOG@HDPE composite powder prepared in Example 21 of the present invention;

[0026] Figure 4 These are optical microscope photos of high-density polyethylene conductive composite materials with an isolation network prepared in the examples of the present invention, a is the GNP / HDPE prepared in Example 17, and b is the PANI-EOG / HDPE prepared in Example 21;

[0027] Figure 5 These are cross-sectional SEM images of high-density polyethylene conductive composite materials with isolation networks prepared in accordance with the embodiments of the present invention; a is the GNP / HDPE prepared in Example 17, and b is the PANI-EOG / HDPE prepared in Example 21. DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] The raw materials used in the embodiment of the present invention are as follows: conductive graphene (vertical size 2-10 μm, Sinopec (Beijing) Chemical Research Institute Co., Ltd.), aniline (≥99%, Aladdin), potassium permanganate (≥99.5%, Yonghua Chemical Technology), concentrated nitric acid (68%, Kunshan Jingke), concentrated hydrochloric acid (38%, Kunshan Jincheng), high-density polyethylene powder (melting point 132°C, density 0.952 g / cm 3 , melt index 0.25g / 10min, Dongguan Zhangmutou Taihe Plastic), ammonium persulfate (≥98%, Shanghai Lingfeng).

[0030] The performance tests of the standard samples of polyethylene conductive composite materials obtained in Examples 1 to 21 were carried out according to the following standards: tensile test was carried out according to GB / T1040.3-2006; surface resistivity test was carried out using Trek152-1 surface resistivity meter according to ANSI / ESD Association standard; all samples were kept at a constant temperature of 23°C for 24 hours before testing, and the test temperature was 23°C.

[0031] Example 1

[0032] A method for preparing a high-density polyethylene conductive composite material having an isolation network, such as Figure 1 As shown, the following steps are included:

[0033] (1) Preparation of GNP@HDPE particles

[0034] Polyethylene powder with a particle size of 200 μm and graphene nanosheets were placed in a pulverizer, the mass fraction of graphene was controlled to be 1%, and the shear mixing time was 3 min at a rotation speed of 34,000 rpm to obtain polyethylene powder GNP@HDPE coated with 1% conductive filler.

[0035] (2) Preparation of GNP / HDPE with isolation structure by hot pressing

[0036] The GNP@HDPE composite powder was hot-pressed at a temperature of 132°C and a pressure of 8 MPa for 8 min, after which the pressure was removed and the mold was allowed to cool naturally to room temperature to prepare GNP / HDPE with an isolation network.

[0037] Example 2

[0038] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 1 only in that in the step (1), the mass fraction of graphene is controlled to be 2%, and polyethylene powder GNP@HDPE coated with 1% conductive filler is obtained.

[0039] Example 3

[0040] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 1 only in that: in the step (1), the mass fraction of graphene is controlled to be 3%, and polyethylene powder GNP@HDPE coated with 3% conductive filler is obtained.

[0041] Example 4

[0042] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 3 only in that in the step (2), the pressure of the hot pressing process is 4 MPa.

[0043] Example 5

[0044] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 3 only in that in the step (2), the pressure of the hot pressing process is 6 MPa.

[0045] Example 6

[0046] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 3 only in that in the step (2), the pressure of the hot pressing process is 10 MPa.

[0047] Example 7

[0048] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 3 only in that in the step (2), the pressure of the hot pressing process is 12 MPa.

[0049] Example 8

[0050] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 3 only in that in the step (2), the temperature of the hot pressing process is 137°C.

[0051] Example 9

[0052] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 3 only in that in the step (2), the temperature of the hot pressing process is 142°C.

[0053] Example 10

[0054] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 3 only in that in the step (2), the temperature of the hot pressing process is 147°C.

[0055] Embodiment 11

[0056] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 8 only in that in the step (2), the pressure of the hot pressing process is 6 MPa.

[0057] Example 12

[0058] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 8 only in that in the step (2), the pressure of the hot pressing process is 4 MPa.

[0059] Embodiment 13

[0060] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 8 only in that in the step (2), the pressure of the hot pressing process is 2 MPa.

[0061] Embodiment 14

[0062] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 9 only in that in the step (2), the pressure of the hot pressing process is 6 MPa.

[0063] Embodiment 15

[0064] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 9 only in that in the step (2), the pressure of the hot pressing process is 4 MPa.

[0065] Example 16

[0066] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 9 only in that in the step (2), the pressure of the hot pressing process is 2 MPa.

[0067] Embodiment 17

[0068] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 15 only in that in the step (1), the particle size of the polyethylene powder is 50 μm.

[0069] like Figure 3 As shown in a, GNPs are coated on the surface of HDPE, and there are gaps between the GNP fillers.

[0070] like Figure 4 As shown in (a), the HDPE particles are isolated by GNPs, and the GNPs are evenly distributed between the HDPE particles, forming a GNP / HEDPE with an isolated three-dimensional conductive network, and some of the isolated paths have conductive filler agglomerations.

[0071] like Figure 5 As shown in (a), the rough and uneven cross-section presents a typical isolation structure. GNPs are selectively distributed at the interface of HDPE particles to form a conductive path. Some holes and cracks appear at the interface between adjacent particles, indicating that the interface interaction is relatively poor, resulting in relatively poor mechanical properties of the composite material.

[0072] Embodiment 18

[0073] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 15 only in that: in the step (1), the particle size of the polyethylene powder is 400 μm,

[0074] The relevant processing parameters of the high-density polyethylene conductive composite material with isolation network in Examples 1 to 18 are shown in Table 1:

[0075] Table 1 Relevant processing parameters of high-density polyethylene conductive composite materials with isolation network in Examples 1 to 18

[0076]

[0077]

[0078] The conductive properties and mechanical properties of the high-density polyethylene conductive composite materials with isolation networks prepared in Examples 1 to 18 were tested. The test results are shown in Table 2.

[0079] Table 2 Conductive properties and mechanical properties of isolated conductive polyethylene in Examples 1 to 18

[0080]

[0081]

[0082] The results in Tables 1 and 2 show that Examples 1 to 3 reveal the effect of different GNP conductive filler contents on the conductive properties and mechanical properties of isolated conductive polyethylene. As the mass percentage of the conductive filler increases from 1wt% to 3wt%, the conductivity of the conductive polyethylene is improved and the mechanical properties decrease. Examples 4 to 7 reveal the effect of different hot pressing pressures on the conductive properties and mechanical properties of isolated conductive polyethylene. High pressure can reduce the amount of micro-gaps between the conductive particles, produce a tight isolation network, and appropriately improve the mechanical properties and conductive properties. However, too high a pressure may cause the main polymer melt to rupture, reduce the aspect ratio of the conductive filler, and decompose the separated conductive network into separate conductive channels, thereby reducing the conductivity of the conductive polyethylene; Examples 8 to 10 reveal the effects of different hot pressing temperatures on the conductive properties and mechanical properties of isolated conductive polyethylene. Excessive processing temperature reduces the melt viscosity of the main polymer, and significant mutual mixing occurs between the conductive filler and the polymer, which hinders the formation of the separated network, thereby reducing the conductivity of the conductive polyethylene; Examples 11 to 16 reveal that with reference to the above-mentioned temperature and pressure effects, the pressure applied when increasing the processing temperature should be kept reasonable to ensure that the conductive filler and polymer particles are tightly stacked without damaging their geometric dimensions, and the best comprehensive properties of the conductive polyethylene are obtained by adjusting different hot pressing temperatures and pressures; Examples 17 to 18 reveal the effects of HDPE powders of different particle sizes on the mechanical properties and conductive properties of isolated conductive polyethylene. By reducing the particle size of the HDPE powder, the isolated conductive path can be refined, the aggregation of a large amount of conductive fillers can be avoided, and the density of the isolated conductive path can be increased, thereby improving the mechanical properties and conductivity of the conductive polyethylene.

[0083] Embodiment 19

[0084] A method for preparing a high-density polyethylene conductive composite material with an isolation network comprises the following steps:

[0085] (1) Preparation of PANI-EOG@HDPE particles

[0086] a. Preparation of EOG

[0087] 4.0 g of GNP was added to 200 mL of KMnO4 / HNO3 solution (68% nitric acid solution: H2O=1:3) containing 0.8 g of KMnO4, and chemically oxidized at 50°C with continuous stirring at 800 rpm for 24 h to obtain edge oxide graphene EOG. The reaction product was centrifuged at 5000 rpm for 10 min, and then repeatedly washed with distilled water to remove residual acid. The product was filtered, dried in an oven at 60°C for 24 h, and ground into powder in a mortar to obtain EOG for later use.

[0088] b. Preparation of PANI-EOG

[0089] Dissolve 20ml of 38% hydrochloric acid in 220ml of deionized water to prepare a 1mol / L hydrochloric acid solution. Next, add 0.7464g of EOG to 120ml of 1mol / L hydrochloric acid solution and ultrasonically disperse for 30min to obtain a uniform EOG dispersion. Then, add 0.024mol of aniline (An) and 2.2ml of monomer to the EOG dispersion (EOG: An monomer mass ratio = 1:3), and continue ultrasonic treatment for 30min to ensure that they are completely mixed. At the same time, add 5.4768g of ammonium persulfate (APS) to the remaining 120ml of hydrochloric acid solution, stir magnetically for 30min, and obtain an APS solution (monomer: initiator = 1:1). Under water bath conditions, add the prepared APS solution dropwise to the An / EOG mixture, and the water bath temperature is maintained at 25°C. After reacting for 9h, filter and wash the product solution until the filtrate becomes colorless. The filtered product is dried in an oven at 60°C for 24h and ground with a mortar to obtain PANI-EOG.

[0090] c. Place polyethylene powder with a particle size of 50 μm and PANI-EOG with a mass fraction of 3% in a pulverizer, shear and mix at a speed of 34,000 rpm for 3 minutes to obtain polyethylene powder PANI-EOG@HDPE coated with 3% conductive filler.

[0091] (2) Preparation of PANI-EOG / HDPE with isolation structure by hot pressing:

[0092] The PANI-EOG@HDPE particles were hot-pressed at a temperature of 142°C and a pressure of 4 MPa for 8 min. The pressure was then removed and the mold was allowed to cool naturally to room temperature to prepare PANI-EOG / HDPE with an isolation network.

[0093] Embodiment 20

[0094] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 19 only in that in the step (1) b, the mass ratio of EOG:An monomers is 1:2.

[0095] Embodiment 21

[0096] The method for preparing a high-density polyethylene conductive composite material with an isolation network is different from that of Example 19 only in that in the step (1) b, the mass ratio of EOG:An monomers is 1:1.

[0097] like Figure 2 As shown in the figure, the rod-shaped PANI is uniformly polymerized on the surface of EOG through π-π conjugation and electrostatic adsorption.

[0098] like Figure 3As shown in b, PANI-EOG is tightly coated on the surface of HDPE, and adjacent EOGs overlap each other.

[0099] like Figure 4 As shown in (b), the HDPE particles are isolated by PANI-EOG, and PANI-EOG is evenly distributed between the HDPE particles, forming a PANI-EOG / HDPE with an isolated three-dimensional conductive network.

[0100] like Figure 5 As shown in Figure b, the flat cross section shows an improved isolation structure. PANI-EOG is selectively distributed at the interface of HDPE particles to form a conductive path. There are no holes and cracks at the interface between adjacent particles, indicating that the interface interaction is strong, resulting in relatively good mechanical properties of the composite material.

[0101] The relevant processing parameters for preparing high-density polyethylene conductive composite materials with isolation networks in Examples 19 to 21 are shown in Table 3.

[0102] Table 3 Relevant processing parameters of high-density polyethylene conductive composite materials with isolation network in Examples 19 to 21

[0103]

[0104] The conductive properties and mechanical properties of the high-density polyethylene conductive composite materials with isolation networks prepared in Examples 19 to 21 were tested. The test results are shown in Table 4.

[0105] Table 4 Conductive properties and mechanical properties of high-density polyethylene conductive composite materials prepared in Examples 19 to 21

[0106] sample Surface resistivity(Ω) Tensile strength(MPa) Elongation at break (%) Embodiment 19 <![CDATA[5.22×10 5 ]]> 22.9 97.0 Embodiment 20 <![CDATA[8.43×10 4 ]]> 22.7 116.7 Embodiment 21 <![CDATA[6.56×10 3 ]]> 23.1 235.4

[0107] The results in Tables 3 and 4 show that Examples 19 to 21 reveal the effects of PANI-EOG with different EOG:An ratios on the conductive properties and mechanical properties of isolated conductive polyethylene. PANI, as an intrinsic conductive polymer, can be used as an adhesive and conductive bridge to enhance the coating of EOG on the surface of HDPE powder, and promote the contact between EOG and the formation of conductive bridges (i.e., PANI phase) between EOG to improve the conductive network. At the same time, PANI can also enhance the interaction between the conductive filler and the HDPE interface to improve the mechanical properties. The mechanical and conductive properties of the conductive polyethylene prepared in Example 21 with PANI-EOG as the conductive filler are significantly improved compared to those prepared in Example 17 with GNP as the conductive filler.

[0108] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the present invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a high-density polyethylene conductive composite material with an isolation network, characterized in that: The following steps are involved: (1) in a pulverizing mixer, a conductive filler is uniformly and tightly coated on the surface of a high-density polyethylene powder by mechanical shearing to obtain a composite powder, wherein the conductive filler is a graphene or an edge-oxidized graphene filler; (2) hot pressing the composite powder to form a three-dimensional conductive network inside the material, thereby obtaining the high-density polyethylene conductive composite material with an isolation network.

2. The method for preparing a high-density polyethylene conductive composite material with an isolation network according to claim 1, characterized in that: In the step (1), the edge oxidized graphene filler is prepared by using nitric acid and potassium permanganate to perform edge oxidation modification on graphene to obtain edge oxidized graphene, and then in-situ polymerizing the conductive polymer polyaniline on the surface of the edge oxidized graphene to obtain the edge oxidized graphene filler.

3. The method for preparing a high-density polyethylene conductive composite material with an isolation network according to claim 2, characterized in that: The preparation method of the edge oxidized graphene is as follows: adding graphene to a KMnO4 / HNO3 solution for chemical oxidation, and then centrifuging, washing, filtering, and drying to obtain the edge oxidized graphene.

4. The method for preparing a high-density polyethylene conductive composite material with an isolation network according to claim 3, characterized in that: The concentration of KMnO4 in the KMnO4 / HNO3 solution is 2.0-4.0 mg / ml; The mass ratio of KMnO4 to graphene is 0.20-0.25; The temperature of the chemical oxidation is 50-55°C, the stirring speed is 800-1000rpm, and the reaction time is 24-36h; The centrifugal speed is 5000-8000 rpm, and the centrifugal time is 8-10 min; The washing is carried out using distilled water; The drying temperature is 55-60° C., and the drying time is 24-36 hours.

5. The method for preparing a high-density polyethylene conductive composite material with an isolation network according to claim 2, characterized in that: The specific steps of in-situ polymerization of conductive polymer polyaniline on the surface of edge graphene oxide are as follows: edge graphene oxide is added to a hydrochloric acid solution and dispersed to obtain a uniform EOG dispersion, aniline monomer is added to the EOG dispersion and mixed evenly, and then APS solution is added dropwise. After the reaction is completed, the solution is filtered, washed, and dried to obtain an edge graphene oxide filler.

6. The method for preparing a high-density polyethylene conductive composite material with an isolation network according to claim 5, characterized in that: The concentration of the hydrochloric acid solution is 1-1.1 mol / L; The mass ratio of the edge graphene oxide to the aniline monomer is 0.3 to 1; The reaction temperature is 20-25° C., the reaction time is 6-9 hours, the drying temperature is 55-60° C., and the drying time is 24-36 hours.

7. The method for preparing a high-density polyethylene conductive composite material with an isolation network according to claim 1, characterized in that: The step (1) is specifically as follows: using a pulverizer mixer, at a rotation speed of 34000-40000 rpm, shear mixing 1wt%-3wt% of conductive filler and 50-400 μm high-density polyethylene powder, the shear mixing time is 2-3 minutes, and using electrostatic adsorption to coat the GNP on the surface of the HDPE powder to obtain a composite powder.

8. The method for preparing a high-density polyethylene conductive composite material with an isolation network according to claim 1, characterized in that: In the step (2), the temperature of the hot pressing molding is 132-147° C., the hot pressing pressure is 2-12 MPa, and the hot pressing time is 8-10 min. After the hot pressing is completed, the pressure is removed to allow the mold to cool naturally to room temperature.

9. A high-density polyethylene conductive composite material with an isolation network prepared according to the method for preparing a high-density polyethylene conductive composite material with an isolation network according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Preparation method of antistatic ultra-high molecular weight polyethylene (UHMWPE) / graphene composite material

    CN103450537A

  • High-density polyethylene / graphene / polyaniline composite material and synthetic method thereof

    CN104194131A