Anti-discoloration flame-retardant water-resistant polypropylene composite material as well as preparation method and application thereof

By using Si-ZnO particles and cetyltrimethoxysilane modification in polypropylene materials, the flammability and color change problems of polypropylene materials are solved, the flame retardant performance and water resistance are improved, and the color resistance is achieved is achieved. Variable and mechanical properties, suitable for a variety of application fields.

CN119019784AInactive Publication Date: 2024-11-26GUANGDONG ALDEX NEW MATERIAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411171799.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Polypropylene materials are flammable and prone to color change and agglomeration in high temperature and high humidity environments, resulting in reduced flame retardant performance. The existing flame retardant is poorly compatible with the matrix, affecting the mechanical properties and water resistance of the composite material.

Method used

Using Si-ZnO particles as synergistic agents, the interaction force between the flame retardant and the matrix is ​​improved by grafting cetyltrimethoxysilane on the surface of ZnO, the flame retardant performance and water resistance are enhanced, and the formulation and process are optimized. , prepare chromotropic flame-retardant and water-resistant polypropylene composite materials.

Benefits of technology

It significantly improves the flame retardant properties, color degeneration and mechanical properties of composite materials, enhances high temperature and high humidity resistance, reduces agglomeration, improves the compatibility and water resistance of the materials, and is suitable for home appliances, automotive parts and electronics. and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019784A_ABST
    Figure CN119019784A_ABST
Patent Text Reader

Abstract

The invention discloses an anti-discoloration flame-retardant water-resistant polypropylene composite material as well as a preparation method and application thereof, and belongs to the technical field of modified high polymer materials. The preparation method comprises the following steps: adding zinc acetate and lithium hydroxide into ethanol, placing in a water bath, carrying out a stirring reaction, and after the reaction is finished, carrying out filtering, washing and vacuum drying to obtain ZnO; the preparation method comprises the following steps: ultrasonically mixing ZnO and ethanol, heating, adding hexadecyl trimethoxysilane, stirring for reaction, carrying out suction filtration and washing to obtain a filter cake, and drying the filter cake to obtain a product Si-ZnO; the preparation method comprises the following steps: mixing 74-81% by mass of polypropylene, 15-22% by mass of a bromine-antimony flame retardant, 2-6% by mass of Si-ZnO, 0.1-1% by mass of an antioxidant, 0.5-1.2% by mass of a weather-resistant agent, 0.1-1% by mass of a lubricant and 1-4% by mass of toner, and carrying out melt extrusion and granulation to prepare the polypropylene composite material. The polypropylene composite material prepared by the invention has excellent color change resistance, flame retardance, high-temperature and high-humidity resistance and mechanical properties, and can be widely applied to the fields of household appliances, automobile parts, electronic appliances and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of modified polymer materials, and in particular to a color change resistant, flame retardant and water resistant polypropylene composite material, a preparation method and application thereof. Background Art

[0002] Polypropylene is one of the most widely used general-purpose plastics. It has the advantages of heat resistance, chemical resistance, good mechanical properties and processing properties, and is widely used in various industries. However, PP is extremely flammable, which greatly limits the use of PP. Adding flame retardants is the simplest and most effective way to solve the flammability of PP. Octabromo flame retardant is the most widely used halogen flame retardant system in PP. It has the advantages of good stability, good compatibility, environmental protection, and significant flame retardant effect. While the addition of octabromo flame retardant improves the flame retardancy of PP, the product may turn yellow due to the instability of octabromo flame retardant under certain conditions. For example, it may decompose or lose its flame retardant effect in high temperature or high humidity environments. It poses a great threat to people's lives and property. In addition, octabromo flame retardant may have poor compatibility with other materials, easily agglomerate in the matrix, and reduce the physical and mechanical properties of the composite material.

[0003] Hexadecyltrimethoxysilane is a silane coupling agent containing a long-chain alkyl structure. It can be dehydrated and condensed to form polysiloxane after hydrolysis. After being coated on the surface of the flame retardant, it effectively reduces the surface polarity of the flame retardant and enhances the interaction between the flame retardant and the matrix, thereby increasing the water resistance and mechanical properties of the composite material. However, flame-retardant polypropylene products are prone to agglomeration and yellowing in the substrate after absorbing water, especially in bathrooms used in high temperature and high humidity environments. Therefore, in order to solve the above technical problems, it is urgent to develop a flame-retardant and water-resistant polypropylene composite material with excellent anti-color change performance. Summary of the invention

[0004] Based on the technical problems existing in the background technology, the present invention proposes a color change resistant, flame retardant and water resistant polypropylene composite material, a preparation method and application thereof.

[0005] A method for preparing a color-discoloration-resistant, flame-retardant and water-resistant polypropylene composite material comprises the following steps:

[0006] (1) adding zinc acetate and lithium hydroxide to ethanol, placing in a water bath, stirring for reaction, filtering after the reaction, washing, and vacuum drying to obtain ZnO;

[0007] (2) mixing ZnO and ethanol by ultrasonication, then heating, adding hexadecyltrimethoxysilane, stirring and reacting, filtering and washing to obtain a filter cake, and drying the filter cake to obtain a product Si-ZnO;

[0008] (3) 74-81% by mass of polypropylene, 15-22% by mass of bromine antimony flame retardant, 2-6% by mass of Si-ZnO, 0.1-1% by mass of antioxidant, 0.5-1.2% by mass of weathering agent, 0.1-1% by mass of lubricant and 1-4% by mass of color powder are mixed, melt-extruded and granulated to obtain a polypropylene composite material.

[0009] Preferably, the mass ratio of ZnO to hexadecyltrimethoxysilane is (20-50):(1-2).

[0010] Preferably, the weathering agent includes one or more of a hindered amine light stabilizer and a benzoate light stabilizer.

[0011] Preferably, the antioxidant includes one or more of hindered phenol antioxidants and phosphite antioxidants.

[0012] Preferably, the lubricant includes one or more of stearate, white oil, TAF and EBS; and the toner includes titanium dioxide masterbatch.

[0013] Preferably, the bromine antimony flame retardant includes one or more of octabromoether, octabromotriphenylether and antimony powder.

[0014] Preferably, the polypropylene has a melt index of 1 to 100 g / 10 min at 230° C. and 2.16 kg; and the polypropylene includes one or more of copolymer polypropylene and homopolymer polypropylene.

[0015] Preferably, the reaction temperature of step (1) and step (2) is 60-80°C.

[0016] A color change resistant, flame retardant and water resistant polypropylene composite material, comprising the following raw materials in percentage by mass:

[0017] Polypropylene 74-81%, bromine antimony flame retardant 15-22%, Si-ZnO 2-6%, antioxidant 0.1-1%, weathering agent 0.5-1.2%, lubricant 0.1-1% and color powder 1-4%;

[0018] Si-ZnO includes the following raw materials: zinc acetate, lithium hydroxide, ethanol and hexadecyltrimethoxysilane.

[0019] The anti-color change, flame retardant and water-resistant polypropylene composite material prepared by the above preparation method or the application of the above anti-color change, flame retardant and water-resistant polypropylene composite material in the production of household appliances, automobile parts and electronic appliances.

[0020] The beneficial effects of the present invention are as follows:

[0021] The present invention adds Si-ZnO particles as a synergist to the polypropylene material, and the long-chain alkyl on its surface can effectively improve the interaction force between the matrix, improve compatibility, inhibit migration and precipitation, reduce the agglomeration phenomenon in the matrix, thereby reducing the defects in the composite material and enhancing the mechanical properties; at the same time, Si-ZnO can effectively increase the water resistance of the flame-retardant polypropylene composite material and promote the cross-linking of the matrix and the flame retardant to form carbon at high temperature. In summary, the polypropylene composite material prepared by the present invention can not only meet the requirements of high-efficiency flame retardant performance, but also has excellent color change resistance and excellent water resistance, the process is simple, and the molded product has good color change resistance, high mechanical strength, and good high temperature and high humidity resistance, and can be widely used in the fields of home appliances, automotive parts, and electronic appliances. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0023] Figure 1 This is a SEM image of Si-ZnO particles prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] In the following examples and comparative examples:

[0026] The copolymer polypropylene is Guangzhou Petrochemical PP K8009, with a melt index of 8-11g / cm 3 ;

[0027] Homopolymer polypropylene is Beihai Refining PP Z30S, with a melt index of 20-26g / cm 3 ;

[0028] Bromine antimony flame retardant is octabromo-S ether and antimony powder;

[0029] The antioxidant is composed of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1;

[0030] The lubricant is ethylene bis stearamide;

[0031] The weathering agent is light stabilizer 944;

[0032] The color powder is titanium dioxide masterbatch;

[0033] The preparation method of ZnO particles is as follows:

[0034] Zinc acetate and lithium hydroxide in a molar ratio of 1:2 were added to ethanol, placed in a 0°C water bath, stirred for reaction for 1.5 hours, then transferred to a 60°C water bath, stirred for reaction for 5 hours, and after the reaction was completed, filtered, washed, and vacuum dried to obtain ZnO particles with a particle size of 2 to 50 μm.

[0035] The preparation method of the synergist Si-ZnO particles is as follows:

[0036] Add 10kg ZnO and 100mL ethanol into a beaker and mix them evenly by ultrasonic for 30min. After mixing evenly, heat the system to 70℃, drop 0kg, 0.2kg, 0.5kg, 0.8kg, 1.1kg, 1.4kg of hexadecyltrimethoxysilane (0%, 2%, 5%, 8%, 11%, 14% of the mass of ZnO, respectively) into the flask, stir and react for 5h, filter and wash to obtain a filter cake, dry the filter cake in an oven at 80℃ for 12h, and obtain products of 0%Si-ZnO, 2%Si-ZnO, 5%Si-ZnO, 8%Si-ZnO, 11%Si-ZnO and 14%Si-ZnO, respectively.

[0037] The component formulas of Examples 1 to 11 and Comparative Examples are shown in Tables 1 and 2:

[0038] Table 1

[0039]

[0040] Table 2

[0041]

[0042]

[0043] According to the formulas in Table 1 and Table 2, the raw materials were weighed and put into a high-speed mixer for mixing at a mixing speed of 450 rpm / min for a mixing time of 2 to 3 minutes. Then, the raw materials were transferred to the main feeding hopper of a twin-screw extruder and melt-extruded and granulated at a temperature of 170-210° C. to obtain pellets.

[0044] The pellets prepared in the above-mentioned comparative examples were injection molded and tested for performance under the same conditions according to the following standards:

[0045] (1) Flame retardant properties: PP and flame retardant modified PP samples were injection molded into a size of 100×13×1.6 mm 3The specimens were subjected to a vertical burning test (UL-94) according to ISO 9773-1998 standard using a vertical burning tester. The burning grade was evaluated five times and the burning behavior was recorded.

[0046] (2) Tensile strength: tested according to GB / T 1040-2006 standard, with a tensile rate of 50 mm / min.

[0047] (3) Water resistance test: The flame-retardant and water-resistant polypropylene composite material was dried in an oven to constant weight to remove moisture and the weight was recorded. It was then immersed in deionized water at 85°C for 168 h and the weight was recorded. The immersed composite material was dried in an oven to constant weight and the dried specimens were then subjected to vertical burning and tensile strength tests. The water resistance of the material was determined by the change rate of tensile strength before and after immersion and the vertical burning grade.

[0048] (4) Anti-color change property: 1.5 kg of the polypropylene composite materials obtained in the embodiment and the comparative example were respectively taken and injection molded into standard color plates using an injection molding machine. Then, the color plates prepared as above were subjected to room temperature test and aging resistance test (at 60°C). After 120 h, 240 h and 720 h of the experiment, the color difference values ​​(△E) of the color plates after the room temperature test and the aging resistance test were obtained using a spectrometer.

[0049] The test results are shown in Table 3:

[0050] Table 3

[0051]

[0052]

[0053] It can be seen from the data in Table 3 that the color difference at room temperature and the color difference at aging of the flame-retardant and water-resistant polypropylene composite material provided by the present invention are both small, indicating that the color change phenomenon of the flame-retardant and water-resistant polypropylene material obtained by the present invention after room temperature and aging treatment is significantly improved through the optimal formula design, and the flame retardant performance can also be relatively stable.

[0054] ZnO can significantly improve the flame retardant properties of composite materials, but its dispersibility is poor and its interaction with the matrix is ​​weak, which will reduce the water resistance of the composite material. From Example 1 and Comparative Example 2, it can be seen that the flame retardant properties and tensile strength of adding Si-ZnO are better than those of adding ZnO, and the change rate of tensile strength before and after soaking in water in Example 1 is 5.2%, and that in Comparative Example 2 is 12.6%, indicating that the surface hydrophilicity and hydrophobicity of modified ZnO can improve the water resistance of the material. Therefore, the interfacial interaction is changed by the surface grafting method, and hexadecyltrimethoxysilane is grafted on the surface of ZnO to further improve the flame retardancy, water resistance and mechanical properties of the flame retardant system.

[0055] Specifically, from the data comparison of Examples 1 to 5, it can be seen that the addition of Si-ZnO significantly improves the flame retardant properties and mechanical properties of the composite material, and the tensile strength is significantly improved. At the same time, the comparison of the flame retardant immersion before and after the high-temperature combustion process shows that Si-ZnO in the material plays a role in promoting carbonization, because methoxysilane effectively enhances the interaction between the substrate and ZnO. Moreover, from Examples 1-13 and Comparative Examples 1-7, it can be seen that the addition of Si-ZnO is superior to the addition of ZnO in flame retardant properties, water resistance and tensile strength before and after the flame retardant and water-resistant polypropylene composite material is immersed under certain conditions (168h in deionized water at 85°C). With the increase in the amount of hexadecyltrimethoxysilane added, the room temperature color change resistance and aging color change resistance of the flame retardant and water-resistant polypropylene composite material will be improved; at the same time, the tensile strength of the flame retardant and water-resistant polypropylene composite material is also improved, indicating that the mechanical properties of the material are good. The reason for the above phenomenon is that the modification of hexadecyltrimethoxysilane can effectively enhance the interaction between ZnO and the matrix and improve the compatibility. Therefore, after adding the synergist Si-ZnO, the polypropylene material has excellent anti-color change, flame retardant properties, high temperature and high humidity resistance and mechanical properties.

[0056] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0057] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A method for preparing a color-discoloration-resistant, flame-retardant and water-resistant polypropylene composite material, characterized in that: The following steps are involved: (1) adding zinc acetate and lithium hydroxide to ethanol, placing in a water bath, stirring for reaction, filtering after the reaction, washing, and vacuum drying to obtain ZnO; (2) mixing ZnO and ethanol by ultrasonication, then heating, adding hexadecyltrimethoxysilane, stirring and reacting, filtering and washing to obtain a filter cake, and drying the filter cake to obtain a product Si-ZnO; (3) 74-81% by mass of polypropylene, 15-22% by mass of bromine antimony flame retardant, 2-6% by mass of Si-ZnO, 0.1-1% by mass of antioxidant, 0.5-1.2% by mass of weathering agent, 0.1-1% by mass of lubricant and 1-4% by mass of color powder are mixed, melt-extruded and granulated to obtain a polypropylene composite material.

2. The method for preparing the anti-color change flame retardant and water-resistant polypropylene composite material according to claim 1, characterized in that: The mass ratio of ZnO to hexadecyltrimethoxysilane is (20-50): (1-2).

3. The method for preparing the anti-color change flame retardant and water-resistant polypropylene composite material according to claim 1, characterized in that: The weathering agent includes one or more of a hindered amine light stabilizer and a benzoate light stabilizer.

4. The method for preparing the anti-color change flame retardant and water-resistant polypropylene composite material according to claim 1, characterized in that: The antioxidant includes one or more of a hindered phenol antioxidant and a phosphite antioxidant.

5. The method for preparing the anti-color change flame retardant and water-resistant polypropylene composite material according to claim 1, characterized in that: The lubricant includes one or more of stearate, white oil, TAF and EBS; the toner includes titanium dioxide masterbatch.

6. The method for preparing the anti-color change flame retardant and water-resistant polypropylene composite material according to claim 1, characterized in that: The bromine antimony flame retardant includes one or more of octabromoether, octabromotriphenylether and antimony powder.

7. The method for preparing the anti-color change flame retardant and water-resistant polypropylene composite material according to claim 1, characterized in that: The polypropylene has a melting index of 1 to 100 g / 10 min at 230° C. and 2.16 kg; the polypropylene includes one or more of copolymer polypropylene and homopolymer polypropylene.

8. The method for preparing the anti-color change flame retardant and water-resistant polypropylene composite material according to claim 1, characterized in that: The reaction temperature of step (1) and step (2) is 60-80°C.

9. A color-discoloration-resistant, flame-retardant and water-resistant polypropylene composite material, characterized in that: The invention comprises the following raw materials in percentage by weight: Polypropylene 74-81%, bromine antimony flame retardant 15-22%, Si-ZnO 2-6%, antioxidant 0.1-1%, weathering agent 0.5-1.2%, lubricant 0.1-1% and color powder 1-4%; Si-ZnO includes the following raw materials: zinc acetate, lithium hydroxide, ethanol and hexadecyltrimethoxysilane.

10. Use of the anti-color change, flame retardant and water-resistant polypropylene composite material obtained by the preparation method of any one of claims 1 to 8 or the anti-color change, flame retardant and water-resistant polypropylene composite material according to claim 9 in the production of household appliances, automobile parts and electronic appliances.

Citation Information

Patent Citations

  • Thermal aging resistant PP-ZnO nano composite insulating material and preparation method thereof

    CN118185185A