High-temperature-resistant steam rubber for sanitary valve diaphragm

Through improved rubber formula and added materials, the high temperature and dynamic fatigue resistance of the sanitary valve diaphragm is improved, and the problems of lax sealing and insufficient performance in the existing technology under high-temperature steam environment are solved, and the stability of complying with FDA certification is achieved performance.

CN119019787APending Publication Date: 2024-11-26翌中流体技术(江苏)有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411285242.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing sanitary valve diaphragms are prone to problems such as lax sealing, cracks and damage in high-temperature steam environments, and the rubber diaphragms have insufficient water vapor resistance and dynamic fatigue performance.

Method used

Use bio-based EPDM rubber with the third monomer content in Gomoney's high elasticity as the main material, and combine it with liquid rubber, active agent, reinforcement, filler, softener, antioxidant, dispersant, Oxides and aided crosslinking agents form a high-temperature resistant steam rubber. By improving the rubber formula and adding materials such as nanokaolin, carbon nanotubes and different types of antioxidants, it improves its high-temperature, low-compression permanent deformation and dynamics. Fatigue performance.

Benefits of technology

It achieves stable performance in high-temperature and low-compression environments, has excellent dynamic fatigue performance, and avoids precipitate problems through a multi-layer protection system, and complies with FDA certification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005042940890000021
    Figure BDA0005042940890000021
  • Figure BDA0005042940890000041
    Figure BDA0005042940890000041
  • Figure FDA0005042940880000011
    Figure FDA0005042940880000011
Patent Text Reader

Abstract

The invention relates to high-temperature steam resistant rubber for a sanitary valve diaphragm. The ethylene propylene diene monomer comprises the following components in parts by weight: 100 parts of ethylene propylene diene monomer, 0-8 parts of liquid rubber, 3-6 parts of an active agent, 55-60 parts of a reinforcing agent, 5-10 parts of a filling agent, 0-5 parts of a softening agent, 1-3 parts of an antioxidant, 1-2 parts of a dispersing agent, 2-7 parts of peroxide and 1-5 parts of an assistant crosslinking agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention relates to high temperature steam resistant rubber for sanitary valve diaphragm. Background technology:

[0002] Due to its special use, the sanitary valve diaphragm is required to have high temperature resistance, low compression permanent deformation, water vapor resistance, excellent dynamic fatigue performance, and good impact resistance. However, the current sanitary valve rubber diaphragm has many shortcomings due to the unreasonable formulation: for example, when the sanitary valve diaphragm is opened and closed in a cyclic movement under high-temperature steam for many times, the rubber diaphragm will soon show poor sealing, cracks, or even damage. Summary of the invention:

[0003] The present invention is aimed at the above problems and provides a high temperature steam resistant rubber for sanitary valve diaphragm.

[0004] In order to achieve the above object, the present invention adopts the following technical scheme, the composition and weight parts of which are: 100 parts of EPDM rubber, 0-8 parts of liquid rubber, 3-6 parts of active agent, 55-60 parts of reinforcing agent, 5-10 parts of filler, 0-5 parts of softener, 1-3 parts of antioxidant, 1-2 parts of dispersant, 2-7 parts of peroxide, and 1-5 parts of cross-linking agent;

[0005] The EPDM rubber is a bio-based raw rubber with high Mooney and high elasticity and a third monomer content, and its structural formula is

[0006]

[0007] It is copolymerized by ethylene, propylene and ethylidene norbornene (ENB), with the contents of the three monomers being 55.0%, 39.5% and 5.5% respectively. The ethylene comes from sugar cane.

[0008] The active agent is zinc oxide, which has the function of improving the temperature resistance of the product;

[0009] The filler is activated and modified nano-kaolin, which is PF81 from Shanzhen Industrial Co., Ltd.

[0010] The reinforcing agents are fast extrusion carbon black N550, semi-reinforcing carbon black N774 and carbon nanotube GT-300 (Shandong Dazhan Nano New Materials), and are added in a ratio of 7-8:2-3:0-1;

[0011] The softener is Sunpar 2280, an environmentally friendly paraffin oil with a high flash point and very low volatility, which is mainly composed of 80% to 95% straight-chain alkanes and contains a small amount of alkanes with individual branches and monocyclic cycloalkanes with long side chains;

[0012] The dispersant is Struktol, a processing aid for EPDM rubber that improves carbon black dispersion and fluidity. @ WB42, whose main component is zinc soap of unsaturated fatty acids;

[0013] The antioxidant is food grade BASF IRGANOXL57 (octylbutyl diphenylamine), ZMTI (2-thiol methylbenzimidazole zinc salt) or TMQ (2,2,4-trimethyl-1,2-dihydroquinoline polymer);

[0014] Luperox @ 101XL45-SP2 is a powder of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane with calcium carbonate and silicon dioxide as carriers and an active ingredient content of 45%;

[0015] The auxiliary cross-linking agent Sovlink TAIC-70P is a powder of TAIC (triallyl 1,3,5-cyanurate) with calcium carbonate and silicon dioxide as carriers and an active ingredient content of 70%.

[0016] Beneficial effects of the present invention:

[0017] In order to obtain ideal comprehensive performance, high-Mooney and high-elastic EPDM rubber is used as the main material in the formula. At the same time, liquid EPDM rubber and softener paraffin oil are added to improve processability, thereby ensuring both functional performance and processability.

[0018] Fast-extrusion carbon black N550 and semi-reinforced carbon black N774 are added to the formula, which can not only improve the elasticity and low compression permanent deformation performance of the product, but also ensure the smoothness of the product appearance and processing performance. In addition, the addition of carbon nanotube material GT-300 improves the tear strength and tensile strength of the product.

[0019] The activated and modified nano-kaolin, whose porous structure and high adsorption activity help absorb small molecular substances in the formula, thereby further reducing the precipitates on the product surface.

[0020] The protection system uses three different types of antioxidants in combination to provide better protection and prevent precipitation due to increased solubility of a single type of antioxidant in EPDM rubber.

[0021] The vulcanization system uses peroxide 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane and co-crosslinking agent TAIC. Through high temperature, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane is decomposed into free radicals to attack the unsaturated double bonds in EPDM rubber, causing chain growth reaction and crosslinking reaction inside the rubber to form more stable CC crosslinking bonds, so that the product has better high temperature resistance and high temperature low compression permanent deformation.

[0022] The invention is resistant to high temperature and low compression permanent deformation, resistant to high temperature water vapor, has excellent dynamic fatigue performance, and complies with FDA certification. Specific implementation method:

[0023] Example 1

[0024] The specific composition and specific addition amount are shown in Table 1 below.

[0025] Table 1

[0026] Raw material name Mass Weight(kg) EPDM 100.0 24 Liquid EPDM 5.0 1.2 Activator ZnO 5.0 1.2 Carbon Black N550 41.0 9.84 Carbon Black N774 14.0 3.36 Carbon Nanotube GT-300 2.0 0.48 Nano Kaolin PF-81 8.0 1.92 Paraffin oil 2280 4.0 0.96 Dispersant WB42 1.5 0.36 L57 0.5 0.12 ZM 1.0 0.24 TMQ 1.0 0.24 101XL45-SP2 6.5 1.56 TAIC-70P 1.5 0.36

[0027] After the finished product of Example 1 was applied to the rubber for sanitary valve diaphragm, the performance test results are shown in Table 2.

[0028] Table 2

[0029]

Claims

1. A high temperature steam resistant rubber for sanitary valve diaphragm, It is characterized in that Its composition and weight parts are: 100 parts of EPDM rubber, 0-8 parts of liquid rubber, 3-6 parts of active agent, 55-60 parts of reinforcing agent, 5-10 parts of filler, 0-5 parts of softener, 1-3 parts of antioxidant, 1-2 parts of dispersant, 2-7 parts of peroxide, and 1-5 parts of cross-linking agent; The EPDM rubber is a bio-based raw rubber with high Mooney and high elasticity and a third monomer content, and its structural formula is The active agent is zinc oxide; The filler is activated and modified nano-kaolin; The reinforcing agents are fast extrusion carbon black N550, semi-reinforcing carbon black N774 and carbon nanotube GT-300, and are added in a weight ratio of 7-8:2-3:0-1; The softener is Sunpar 2280, an environmentally friendly paraffin oil with a high flash point and extremely low volatility; The dispersant is WB42, a processing aid specially used for EPDM rubber to improve the dispersion and fluidity of carbon black; The antioxidant is food grade octylbutyl diphenylamine), 2-mercaptomethylbenzimidazole zinc salt or 2,2,4-trimethyl-1,2-dihydroquinoline polymer; Peroxide 101XL45-SP2 is a powder of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane with calcium carbonate and silicon dioxide as carriers, and the active ingredient content is 45%; The auxiliary cross-linking agent Sovlink TAIC-70D is a powder of 1,3,5-triacyl cyanurate with calcium carbonate and silicon dioxide as carriers and an active ingredient content of 70%.

Citation Information

Patent Citations

  • Rubber composition capable of resisting expansibility of synthetic brake fluid of motor vehicle

    CN102516670A

  • High-strength high-temperature-resistant ethylene propylene diene monomer

    CN112724541A

  • Rubber composition for aerator diaphragm, vulcanized rubber as well as preparation method and application of vulcanized rubber

    CN116265521A

  • Ultralow-temperature-resistant ethylene-butadiene rubber compound and application thereof in rubber tube

    CN118388889A