Resin composition, prepreg and metal foil-clad laminated board

The resin composition formed by combining triallyl cyanurate with elastomer block copolymer and phosphorus-containing flame retardant has solved the poor dielectric performance and thermal oxygen aging in high-frequency and high-speed circuit boards. The problem of insufficient capability achieves halogen-free flame retardant and excellent dielectric properties.

CN119019805AActive Publication Date: 2024-11-26GUANGDONG SHENGYI SCI TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310586024.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-26
Estimated Expiration
2043-05-23

AI Technical Summary

Technical Problem

Existing electronic materials have poor dielectric performance in the field of high-frequency and high-speed circuit boards, poor thermal oxygen aging ability, and difficult to achieve halogen-free flame retardant performance.

Method used

Triallyl cyanurate is used as the main component and is combined with elastomeric block copolymer and phosphorus-containing flame retardant to form a resin composition to improve dielectric properties, thermal oxygen aging resistance and flame retardant properties.

Benefits of technology

It significantly improves dielectric properties and heat-oxygen aging resistance, achieves halogen-free flame retardant, meets the requirements of high-frequency and high-speed circuit boards, and has good processability and glue-oning process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004243361580000051
    Figure BDA0004243361580000051
  • Figure BDA0004243361580000111
    Figure BDA0004243361580000111
  • Figure BDA0004243361580000121
    Figure BDA0004243361580000121
Patent Text Reader

Abstract

The invention provides a resin composition, a prepreg and a metal foil-clad laminated board. The resin composition comprises triallyl cyanurate, an elastomer block copolymer and a phosphorus-containing flame retardant, the total mass of the resin components in the resin composition is 100%, and the content of the triallyl cyanurate is 50-70%. According to the resin composition disclosed by the invention, the triallyl cyanurate is used as a main component, and is combined with the elastomer block copolymer and the phosphorus-containing flame retardant for application, so that a plate containing the resin composition has excellent dielectric property, thermal-oxidative aging resistance, humidity and heat resistance and good flame retardance, and meets the requirements in the field of high-frequency and high-speed circuit boards.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of copper-clad laminates, and in particular relates to a resin composition, a prepreg and a metal foil-clad laminate. Background Art

[0002] In recent years, with the rapid development of electronic information technology and hardware carriers, the demand for the transmission volume of electronic components and circuit materials has also increased, making the application of electronic products enter the era of high-frequency and high-speed transmission. Therefore, the dielectric properties of related electronic materials have become a key issue of concern. With the trend of high-frequency and high-speed signal transmission and high-density circuit boards, the requirements for low dielectric constant, low dielectric loss and flame retardancy of electronic materials have become increasingly prominent.

[0003] Printed Circuit Board (PCB) is a component used for electrical connection in electronic equipment and electronic components, and is one of the important electronic materials; PCB is usually made by copper clad laminate through different processes. Therefore, the performance, quality, service life and manufacturing level of PCB largely depend on the performance of copper clad laminate.

[0004] Copper clad laminates include copper foil, reinforcement materials and resin materials. The properties of the resin materials directly affect the performance of the board and PCB. Epoxy resin is a traditional board material with good adhesion, heat resistance and processing performance, and has significant cost advantages. However, with the application of high-speed and high-frequency circuit boards, higher requirements are placed on the dielectric loss of the material, but the dielectric constant and dielectric loss Df value of epoxy resin are large, resulting in poor dielectric properties of the board, which cannot meet the use requirements.

[0005] Polyolefin materials are non-polar materials with low dielectric loss Df, which can meet the requirements of copper-clad laminates in terms of low dielectric properties, and are currently widely concerned by the industry. CN110605880A discloses a composition of a thermosetting hydrocarbon polymer, a semi-cured sheet and a thermosetting copper-clad laminate, and the preparation method includes: using a polyhydroxy polyarylether resin, a hydrogenated hydroxyl-terminated polyolefin resin, a polydiene resin, a vinyl-modified polyarylether resin, etc. as raw materials, preparing a polyarylether-polyolefin block copolymer to contain a thermosetting hydrocarbon polymer composition thereof; and then using the composition to prepare a thermosetting copper-clad laminate. Compared with epoxy resin copper-clad laminates, the above-mentioned sheet containing olefin polymers has better performance in terms of dielectric properties. However, the heat-oxidative aging resistance of olefin polymers is poor. After aging for a period of time under high temperature, oxygen and other conditions, the dielectric loss Df increases significantly, resulting in Df failing to meet the use requirements after long-term use, and the existing hydrocarbon materials are extremely flammable resins, and even after adding a large amount of halogen-free flame retardants, it is difficult to achieve halogen-free flame retardancy.

[0006] Therefore, in the art, it is desired to develop a circuit material that can have excellent aging resistance, dielectric properties, bonding strength and halogen-free flame retardant properties to meet the requirements of the high-frequency and high-speed circuit board field. Summary of the invention

[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide a resin composition, a prepreg and a metal foil-clad laminate. The resin composition of the present invention uses triallyl cyanurate as a main component, which is combined with an elastomeric block copolymer and a phosphorus-containing flame retardant for use, so that the plate containing it has excellent dielectric properties, resistance to heat and oxygen aging, resistance to moisture and heat (stability of electrical properties under long-term moisture and heat conditions, i.e., wet bleaching performance often mentioned in the industry) and good flame retardant properties, meeting the requirements of the field of high-frequency and high-speed circuit boards.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In one aspect, the present invention provides a resin composition comprising triallyl cyanurate (TAC), an elastomeric block copolymer, and a phosphorus-containing flame retardant;

[0010] Based on the total mass of the resin components in the resin composition being 100%, the content of the triallyl cyanurate is 50-70%.

[0011] In the resin composition provided by the present invention, the triallyl cyanurate (TAC) as the main component has excellent heat oxygen aging resistance and dielectric properties, excellent wetting, good bonding force, good fluidity, and high nitrogen content. It can form N, P synergistic flame retardant with phosphorus-containing flame retardant, and can achieve halogen-free flame retardant. The elastomer block copolymer and TAC are compounded to help improve and regulate the viscosity of the glue, which is conducive to glue hanging, optimizes the processability and gluing processability, and plays a role in enhancing the toughness of the finished tree board. The resin composition has a low dielectric constant and dielectric loss and excellent dielectric properties through the synergistic effect of TAC and the elastomer block copolymer, which significantly improves the heat oxygen aging resistance of the resin composition, the semi-cured sheet and the metal foil-clad laminate, the high stability of the dielectric properties, the good reliability of the board, etc., and has good processability and gluing processability, which fully meets the dielectric reliability requirements of the resin composition and the board in the high-frequency and high-speed field. The resin composition of the present invention, with the cooperation of triallyl cyanurate (TAC), elastomeric block copolymer and phosphorus-containing flame retardant, enables the board to have excellent dielectric properties, heat oxygen aging resistance, moisture heat resistance and good flame retardant properties, and has excellent comprehensive performance.

[0012] In the present invention, based on the total mass of the resin components in the resin composition as 100%, the content of triallyl cyanurate is 50-70%, for example, it can be 50%, 55%, 58%, 60%, 63%, 65%, 68% or 70%. If the content of triallyl cyanurate is lower than 50%, it will lead to insufficient resistance to thermal oxygen aging; if the content of triallyl cyanurate is higher than 70%, the board is too brittle and has poor mechanical properties.

[0013] In the present invention, the elastomeric block copolymer includes any one of styrene-butadiene copolymer, styrene-butadiene-styrene triblock copolymer, styrene-isoprene copolymer or styrene-isoprene-styrene triblock copolymer or a combination of at least two thereof.

[0014] Preferably, the number average molecular weight of the elastomeric block copolymer is ≥50,000, for example, it may be 50,000, 60,000, 70,000, 80,000, 100,000, 120,000, 150,000, 180,000, 200,000, 250,000 or 300,000.

[0015] In the present invention, the molecular weight (weight average molecular weight, number average molecular weight, etc.) is measured according to GB / T21863-2008 and is obtained by gel permeation chromatography (GPC) based on polystyrene calibration.

[0016] In the present invention, the total mass of the resin components in the resin composition is 100%, and the content of the elastomeric block copolymer is 10-30%, for example, 10%, 13%, 15%, 18%, 20%, 23%, 25%, 28% or 30%. If the amount of the elastomeric block copolymer added is too much, the viscosity of the glue is too high, and the wettability of the reinforcing materials such as glass fiber cloth is insufficient, resulting in more voids in the plate, increased water absorption, poor processability, etc.; if the amount of the elastomeric block copolymer added is too little, the viscosity of the glue is too low, and the semi-cured sheet has poor formability.

[0017] Preferably, the phosphorus-containing flame retardant may be a reactive or additive flame retardant. The reactive phosphorus-containing flame retardant refers to one containing reactive groups that can react with the resin component in the resin composition, and the additive phosphorus-containing flame retardant refers to one not containing reactive groups that can react with the resin component in the resin composition.

[0018] Preferably, the phosphorus-containing flame retardant is selected from any one of tris(2,6-dimethylphenyl)phosphine, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 2,6-bis(2,6-dimethylphenyl)phosphinobenzene, p-xylylenebisdiphenylphosphine oxide, phenoxyphosphazene compounds, phosphates, polyphosphates, phosphonates, polyphosphonates, phosphonate-carbonate copolymers or phosphinates containing organic phosphorus, or a mixture of at least two thereof, such as SPB-100 manufactured by Otsuka Chemical Co., Ltd. of Japan, OP-930 and OP-935 manufactured by Clariant of Germany, SP-703H manufactured by Shikoku Chemical Co., Ltd., PQ-60 of Shinichi Chemical, DE-295 of Jiangsu Yake, etc. Further preferred phosphinate flame retardants containing organic phosphorus can obtain better heat resistance and electrical properties.

[0019] Preferably, based on the total mass of the resin components in the resin composition as 100%, the content of the phosphorus-containing flame retardant is 10-35%, for example, 10%, 15%, 18%, 20%, 23%, 25%, 28%, 30% or 35%.

[0020] It should be noted that in the resin composition provided by the present invention, the combination of triallyl cyanurate and elastomeric block copolymer reacts when used in a prepreg or a metal foil-clad laminate, and the reaction may proceed spontaneously at an appropriate temperature, or may be initiated (or promoted) by adding an optional initiator (or accelerator).

[0021] Preferably, the resin composition further comprises an initiator.

[0022] Preferably, the initiator is an organic peroxide.

[0023] Preferably, the initiator includes any one of dicumyl peroxide, di-tert-butyl dicumyl peroxide, tert-butyl perbenzoate or 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne, or a combination of at least two thereof.

[0024] Preferably, based on the total mass of the resin components in the resin composition as 100%, the content of the initiator is 0.1-8%, for example 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7% or 8%.

[0025] Preferably, the resin composition further comprises polyphenylene ether resin.

[0026] Preferably, the polyphenylene ether resin is a polyphenylene ether resin containing an unsaturated group.

[0027] Preferably, the unsaturated group-containing polyphenylene ether resin is an unsaturated group-terminated polyphenylene ether resin.

[0028] As a preferred technical solution of the present invention, the resin composition also includes a polyphenylene ether resin containing an unsaturated group, which is compounded with TAC and an elastomeric block copolymer to improve the rigidity of the resin composition, the prepreg and the metal foil-clad laminate and prevent the board from warping.

[0029] Preferably, the unsaturated group includes any one of vinyl, vinylphenyl, vinylbenzyl or acrylate groups, or a combination of at least two of them.

[0030] Preferably, the polyphenylene ether resin containing unsaturated groups includes a structural unit as shown in Formula I:

[0031]

[0032] In Formula I, the wavy line represents the attachment site of the group.

[0033] In Formula I, R1, R2, R1', R2' are each independently selected from any one of hydrogen, halogen, substituted or unsubstituted C1-C7 (C1, C2, C3, C4, C5, C6 or C7) straight chain or branched alkyl, C1-C7 (C1, C2, C3, C4, C5, C6 or C7) aminoalkyl, C1-C7 (C1, C2, C3, C4, C5, C6 or C7) straight chain or branched alkoxy, C2-C7 (C2, C3, C4, C5, C6 or C7) straight chain or branched alkenyl, substituted or unsubstituted C6-C12 (C6, C9, C10 or C12, etc.) aryl, C6-C1 (C6, C9, C10 or C12, etc.) aryloxy.

[0034] The substituents in R1, R2, R1' and R2' are each independently selected from at least one of halogen, C1-C6 (C1, C2, C3, C4, C5 or C6) straight chain or branched alkyl.

[0035] The halogen includes fluorine, chlorine, bromine or iodine, and chlorine or bromine is more preferred.

[0036] Preferably, R1 and R2 are each independently selected from any one of unsubstituted or halogenated C1-C7 (C1, C2, C3, C4, C5, C6 or C7) straight chain or branched alkyl, C2-C5 (C2, C3, C4 or C5) straight chain or branched alkenyl, phenyl or tolyl.

[0037] Preferably, R1' and R2' are each independently hydrogen or methyl.

[0038] Preferably, the polyphenylene ether in the polyphenylene ether resin containing unsaturated groups includes poly(2,6-dimethyl-1,4-phenylene) ether, poly(2,3,6-trimethyl-1,4-phenylene) ether, poly(2,6-diethyl-1,4-phenylene) ether, poly(2,6-dipropyl-1,4-phenylene) ether, poly(2-methyl-6-allyl-1,4-phenylene) ether, poly(di-tert-butyl-dimethoxy-1,4-phenylene) ether, poly(2,6-dichloromethyl-1,4-phenylene) ether, Any one or a combination of at least two of poly(2,5-dimethyl-1,4-phenylene) ether, poly(2,6-dibromomethyl-1,4-phenylene) ether, poly(2,6-bis(2-chloroethyl)-1,4-phenylene) ether, poly(2,6-xylyl-1,4-phenylene) ether, poly(2,6-dichloro-1,4-phenylene) ether, poly(2,6-diphenyl-1,4-phenylene) ether or poly(2,5-dimethyl-1,4-phenylene) ether, and poly(2,6-dimethyl-1,4-phenylene) ether is further preferred.

[0039] The types exemplified above are types of main structures of polyphenylene ether, which further contain unsaturated groups, preferably their end groups contain unsaturated groups, and the unsaturated groups include any one or a combination of at least two of vinyl, vinylphenyl, vinylbenzyl, acrylate or methacrylate.

[0040] In the present invention, the polyphenylene ether containing unsaturated groups can be purchased from the market, and illustratively includes but is not limited to: polyphenylene ether MX9000 containing methacrylate groups (SABIC) and polyphenylene ether OPE-2ST containing vinylbenzyl groups (Mitsubishi Chemical Corporation).

[0041] Preferably, based on the total mass of the resin components in the resin composition as 100%, the content of the polyphenylene ether resin is 1-30%, for example, 1%, 3%, 5%, 10%, 13%, 15%, 18%, 20%, 25%, 28% or 30%.

[0042] Preferably, the resin composition further comprises a filler; the filler has the functions of preventing adhesion, improving the mechanical properties of the board, and improving the coefficient of thermal expansion CTE.

[0043] Preferably, the filler is an inorganic filler and / or an organic filler.

[0044] Preferably, the filler is a powder filler, including any one or a combination of at least two of crystalline silica, amorphous silica, spherical silica, angular silica, chemical silica, silicon powder, hollow glass microspheres, titanium dioxide, strontium titanate, barium titanate, boron nitride, aluminum nitride, silicon nitride, silicon carbide, aluminum oxide, polytetrafluoroethylene, polyphenylene sulfide or polyether sulfone.

[0045] Preferably, based on the total mass of the resin composition and the filler as 100%, the content of the filler is 50-70%, for example, 50%, 55%, 60%, 65% or 70%.

[0046] On the other hand, the present invention provides a resin adhesive solution, which is obtained by dissolving or dispersing the above-mentioned resin composition in a solvent.

[0047] The amount of solvent added is selected by those skilled in the art based on experience and process requirements to make the resin composition reach a suitable viscosity for use, so as to facilitate impregnation, coating, etc. of the resin composition. In the subsequent drying, semi-curing or full curing stage, the solvent in the resin composition will partially or completely evaporate.

[0048] The solvent of the present invention is not particularly limited, and generally, ketones such as acetone, butanone, and cyclohexanone, aromatic hydrocarbons such as toluene and xylene, esters such as ethyl acetate and butyl acetate, alcohols such as methanol, ethanol, or butanol, alcohols such as ethyl cellosolve, butyl cellosolve, ethylene glycol monomethyl ether, carbitol, or butyl carbitol, and nitrogen-containing solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, or N-methyl-2-pyrrolidone can be selected; the solvent can be used alone or in combination of two or more. Ketones such as acetone, butanone, and cyclohexanone, and aromatic hydrocarbons such as toluene and xylene are preferred.

[0049] In another aspect, the present invention provides a resin film, wherein the material of the resin film comprises the resin composition as described above.

[0050] Preferably, the resin film is obtained by coating the resin composition on a release material and then drying and / or semi-curing the resin composition.

[0051] In another aspect, the present invention provides a prepreg, comprising a reinforcing material and the above-mentioned resin composition attached to the reinforcing material.

[0052] Preferably, the resin composition is attached to the reinforcing material by impregnation and then drying.

[0053] Preferably, the reinforcing material includes any one of natural fibers, organic synthetic fibers, organic fabrics, and inorganic fibers, or a combination of at least two thereof; for example, glass fiber cloth, quartz glass fiber blended cloth, non-woven fabric, quartz cloth, and the like.

[0054] Exemplarily, the method for preparing the prepreg is: using the resin glue of the resin composition to infiltrate a reinforcing material, and then drying to obtain the prepreg.

[0055] Preferably, the drying temperature is 100-160°C, for example, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C or 155°C, etc.

[0056] In another aspect, the present invention provides a metal foil-clad laminate, comprising a metal foil and at least one of the resin film as described above or the prepreg as described in the third aspect.

[0057] Preferably, the metal foil is copper foil, and the metal foil-clad laminate is a copper-clad laminate.

[0058] Exemplarily, the method for preparing the metal-clad laminate comprises: laminating metal foil on one side or both sides of a semi-cured sheet and curing to obtain the metal-clad laminate; or, stacking at least two semi-cured sheets into a laminate, and then laminating metal foil on one side or both sides of the laminate and curing to obtain the metal-clad laminate.

[0059] Preferably, the curing is carried out in a press.

[0060] Preferably, the curing temperature is 170-280°C, for example, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C or 270°C.

[0061] Preferably, the curing pressure is 1-10 MPa, for example, 1.5 MPa, 2 MPa, 3 MPa, 4 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa or 9 MPa.

[0062] Preferably, the curing time is 30-150 min, for example, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min or 145 min, etc.

[0063] In another aspect, the present invention provides a printed circuit board, comprising at least one of the resin film as described above, the prepreg as described above, or the metal foil-clad laminate as described above.

[0064] Compared with the prior art, the present invention has the following beneficial effects:

[0065] The resin composition of the invention uses triallyl cyanurate as a main component, and is matched with an elastomer block copolymer and a phosphorus-containing flame retardant to significantly improve the heat-oxidation aging resistance, dielectric properties, moisture-heat resistance and flame retardancy of the resin composition, the prepreg and the metal foil-clad laminate, so that the dielectric loss of the plate at 10GHz is 0.0036-0.0045; after high-temperature heat-oxidation aging for 4 weeks, the dielectric loss is 0.0050-0.0058, the dielectric loss change value is ≤0.0020, the Df change rate is ≤52.94%, the flame retardancy reaches V-0 level, the resin composition has good dielectric properties and reliability, good processability and gluing processability, high peel strength, low warping degree, and fully meets various performance requirements for the resin composition and the plate in the high-frequency and high-speed field. DETAILED DESCRIPTION

[0066] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0067] The materials involved in the following embodiments and comparative examples of the present invention include:

[0068] (1) Main components

[0069] Triallyl cyanurate, TAC;

[0070] Triallyl isocyanurate, TAIC;

[0071] Polybutadiene resin, B-3000, Japan Soda, number average molecular weight 4500;

[0072] (2) Elastomer block copolymer

[0073] Styrene-butadiene-styrene triblock copolymer (SBS), KRATON D-1118, weight average molecular weight 80,000, Kraton, USA;

[0074] Styrene-butadiene diblock copolymer (SB), weight average molecular weight 40000, T171E, Dushanzi Petrochemical;

[0075] Styrene-isoprene-styrene triblock copolymer, weight average molecular weight 100000, KRATON D-1114, Kraton, USA;

[0076] Non-block copolymer: butadiene-styrene copolymer, number average molecular weight 4500, R100, Sartomer Company;

[0077] (3) Polyphenylene ether containing unsaturated groups

[0078] Polyphenylene ether MX9000, methacrylate-terminated, SABIC;

[0079] Polyphenylene ether OPE-2ST, vinyl benzyl ether modified polyphenylene ether, Mitsubishi Chemical Corporation;

[0080] (4) Initiator

[0081] Dicumyl peroxide, DCP;

[0082] Diisopropylbenzene (di-tert-butylperoxide), BIPB;

[0083] (5) Filling

[0084] Filler F1, silicon dioxide, brand Megasil525, Sibelco;

[0085] (6) Flame retardant

[0086] Phosphorus-containing flame retardant 1: P1, aluminum diethylphosphinate, brand OP935, Clariant Company.

[0087] Phosphorus-containing flame retardant 2: P2, Di-DOPO, brand DE-295, Jiangsu Yak Technology Co., Ltd.

[0088] Phosphorus-containing flame retardant 3: P3, phenoxyphosphazene, brand name SPB-100, Otsuka Chemical Co., Ltd.

[0089] Example 1

[0090] A resin composition comprises the following components by mass: 50 parts of triallyl cyanurate TAC, 30 parts of elastomeric block copolymer KRATON D-1118, 20 parts of polyphenylene ether MX9000, 4 parts of initiator DCP, 200 parts of filler F1, and 10 parts of phosphorus-containing flame retardant.

[0091] A prepreg and a copper-clad laminate comprising the resin composition, the preparation method of which is as follows:

[0092] (1) mixing the resin composition with toluene according to the formula to prepare a glue solution with a solid content of 60%; impregnating a glass fiber cloth with the glue solution and then baking and drying at 120° C. for 3 minutes to obtain a prepreg;

[0093] (2) 6 prepregs are stacked, and copper foils are covered on the upper and lower sides thereof. The prepregs are cured in a press at 240° C. and 5 MPa for 2 h to obtain the copper clad laminate.

[0094] The components of the resin composition and their mass fractions are shown in Table 1 and Table 2; the mass unit of each component in Table 1 and Table 2 is "part".

[0095] Table 1 Example

[0096]

[0097]

[0098] Table 2 Comparative Examples

[0099]

[0100]

[0101] The above resin composition was made into a copper clad laminate according to the method in Example 1, and the following performance tests were performed on it:

[0102] (1) Dielectric constant Dk and dielectric loss factor Df: measured using the resonant cavity method (SPDR) at a frequency of 10 GHz; the receiving state is the original state, and the state after thermal oxygen aging after aging at 153°C for 4 weeks is the state after thermal oxygen aging; Df change rate = (Df after thermal oxygen aging - Df in the original state) / Df in the original state;

[0103] (2) Warp height: Cut the laminate into 300 mm × 300 mm, etch the copper foil on one side, place it on a horizontal table, and measure the vertical distance between the edge of the board and the table. This distance is the warp height.

[0104] (3) Flame retardancy: UL94. For detailed test methods, please refer to UL Flame Retardancy Test Method, UL Chapter 8.

[0105] (4) Gluing processability: Based on the appearance of the semi-cured sheet during the gluing process, observe with the naked eye whether there is obvious sag or stickiness. If the semi-cured sheet has no sag or stickiness at all, the gluing processability is excellent; if the semi-cured sheet has slight sag, the gluing processability is good; if the semi-cured sheet has severe sag or stickiness, the gluing processability is poor.

[0106] (5) Sheet formability: If the sheet is too brittle and forms granular fragments after slightly bending the sheet, it is considered that the sheet has poor formability. If the sheet cracks or breaks when bent but there are no obvious granular fragments, it is considered that the sheet has good formability. If the sheet does not have any of the above conditions, it has excellent formability.

[0107] Table 3 Changes in Df after 153℃ thermal oxidation aging

[0108]

[0109]

[0110] Table 4 Warpage / flame retardancy / processability / formability

[0111]

[0112] From the data in Table 3 and Table 4, the present invention uses TAC as the main component, and through compounding it with components such as elastomeric block copolymers, and adding 50-70% by mass of fillers and 10-35% by mass of halogen-free flame retardants, a high-frequency copper clad laminate with halogen-free V-0 flame retardancy can be prepared, and the dielectric loss (SPDR@10GHz) is low, at 0.0036-0.0045, and the heat-oxidation aging resistance is also good. After 4 weeks of heat-oxidation treatment at 153°C, the change rate of Df is 22.22%-52.94%.

[0113] Specifically, the initial state dielectric loss of Example 4 is relatively low. After using OPE-2ST, it is beneficial to reduce the dielectric loss in the initial state, which is 0.0034. After using MX9000, the dielectric loss in the initial state is slightly higher, which is 0.0036. The thermal oxygen aging resistance of Examples 3, 5 and 6 is relatively strong. After 4 weeks of thermal oxygen aging treatment at 153°C, the dielectric loss change rate is only 28.21%, 22.22% and 25.00%. The TAC content corresponding to these examples is relatively high, at 65%-70%. The high TAC content is beneficial to improve the thermal oxygen aging resistance. It can be seen that the flame retardancy of the embodiments improved by the present invention is relatively good. Examples 1-7 can all achieve V-0 halogen-free flame retardancy. After TAC is the main resin, it forms a certain degree of N and P synergistic flame retardancy with the halogen-free phosphorus-containing flame retardant. In Example 5, the MX9000 polyphenylene ether content is relatively low, which is 5%, resulting in a large warping height of 3.0 cm, which is not very conducive to PCB processing. In Example 1, Example 4 and Example 6, when the polyphenylene ether content is 20%, the warping height is relatively low, ranging from 1.1 to 1.3 cm.

[0114] Compared with Example 1, Comparative Example 1 uses an equal amount of B3000 to replace TAC. It can be seen that the initial state Df of Comparative Example 1 is greatly optimized, from 0.0036 of Example 1 to 0.0032 of Comparative Example 1. However, the shortcomings are also very obvious. The flame-retardant spline of Comparative Example 1 burns to the fixture and has no flame retardancy. In addition, the thermal oxygen aging resistance is also poor. After thermal oxygen aging treatment, the Df change rate of Comparative Example 1 is 112.50%, while that of Example 1 is only 47.22%.

[0115] Compared with Example 1, Comparative Example 2 uses an equal amount of R100 styrene-butadiene copolymer to replace the elastic block copolymer. Although V-0 halogen-free flame retardancy and good thermal oxidation aging resistance can be achieved after the replacement, there are serious process problems such as the adhesive sheet being sticky and unable to be rolled up, the sheet being too brittle and extremely easy to break, and it cannot be produced and used normally.

[0116] Compared with Example 1, Comparative Example 3 uses a lower content of 40 parts of TAC to replace 50 parts of TAC in Example 1. The thermal oxidative aging ability of Comparative Example 3 deteriorates, and the Df change rate reaches 66.67%, while that of Example 1 is 47.22%. The most serious impact is the flame retardant performance, which is downgraded from V-0 flame retardant grade to V-1 flame retardant.

[0117] Compared with Example 6, Comparative Example 4 uses a higher content of 80 parts of TAC to replace 70 parts of TAC in Example 6. The high content of TAC causes the glue viscosity to be very low, and the glue on the bonding sheet seriously sags and cannot be formed, resulting in the inability to produce and use normally, and the inability to test the dielectric properties.

[0118] Compared with Example 1, Comparative Example 5 removes the phosphorus-containing flame retardant, and the corresponding flame retardancy test result is V-2, which cannot reach V-0 halogen-free flame retardancy.

[0119] Compared with Example 1, in Comparative Example 6, an equal amount of TAIC was used to replace TAC, and the thermal oxygen aging resistance became worse, and the Df change rate increased from 47.22% to 66.67%.

[0120] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the resin composition, prepreg and metal foil-clad laminate of the present invention, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A resin composition, characterized in that The resin composition comprises triallyl cyanurate, an elastomeric block copolymer and a phosphorus-containing flame retardant; Based on the total mass of the resin components in the resin composition being 100%, the content of the triallyl cyanurate is 50-70%.

2. The resin composition according to claim 1, characterized in that The elastomeric block copolymer comprises any one or a combination of at least two of a styrene-butadiene copolymer, a styrene-butadiene-styrene triblock copolymer, a styrene-isoprene copolymer or a styrene-isoprene-styrene triblock copolymer; Preferably, the number average molecular weight of the elastomeric block copolymer is ≥50,000; Preferably, based on the total mass of the resin components in the resin composition being 100%, the content of the elastomeric block copolymer is 10-30%.

3. The resin composition according to claim 1 or 2, characterized in that The phosphorus-containing flame retardant is a reactive phosphorus-containing flame retardant or an additive phosphorus-containing flame retardant; Preferably, the phosphorus-containing flame retardant is selected from any one of tris(2,6-dimethylphenyl)phosphine, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 2,6-bis(2,6-dimethylphenyl)phosphinobenzene, p-xylylenebisdiphenylphosphine oxide, phenoxyphosphazene compounds, phosphates, polyphosphates, phosphonates, polyphosphonates, phosphonate-carbonate copolymers or phosphinates containing organic phosphorus, or a mixture of at least two thereof, preferably phosphinate flame retardants containing organic phosphorus; Preferably, based on 100% of the total mass of the resin components in the resin composition, the content of the phosphorus-containing flame retardant is 10-35%.

4. The resin composition according to any one of claims 1 to 3, characterized in that The resin composition also includes an initiator; Preferably, the initiator is an organic peroxide; Preferably, the initiator comprises any one or a combination of at least two of diisopropylbenzene peroxide, di-tert-butyl diisopropylbenzene peroxide, tert-butyl perbenzoate or 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne; Preferably, based on 100% of the total mass of the resin components in the resin composition, the content of the initiator is 0.1-8%.

5. The resin composition according to any one of claims 1 to 4, characterized in that The resin composition also includes a polyphenylene ether resin; Preferably, the polyphenylene ether resin is a polyphenylene ether resin containing an unsaturated group; Preferably, the unsaturated group-containing polyphenylene ether resin is an unsaturated group-terminated polyphenylene ether resin; Preferably, the unsaturated group includes any one or a combination of at least two of vinyl, vinylphenyl, vinylbenzyl or acrylate; Preferably, the polyphenylene ether in the polyphenylene ether resin containing unsaturated groups includes poly(2,6-dimethyl-1,4-phenylene) ether, poly(2,3,6-trimethyl-1,4-phenylene) ether, poly(2,6-diethyl-1,4-phenylene) ether, poly(2,6-dipropyl-1,4-phenylene) ether, poly(2-methyl-6-allyl-1,4-phenylene) ether, poly(di-tert-butyl-dimethoxy-1,4-phenylene) ether, poly(2,6-dichloromethyl-1,4-phenylene) ether, Any one or a combination of at least two of poly(2,5-dimethyl-1,4-phenylene) ether, poly(2,6-dibromomethyl-1,4-phenylene) ether, poly(2,6-di(2-chloroethyl)-1,4-phenylene) ether, poly(2,6-xylyl-1,4-phenylene) ether, poly(2,6-dichloro-1,4-phenylene) ether, poly(2,6-diphenyl-1,4-phenylene) ether or poly(2,5-dimethyl-1,4-phenylene) ether, and poly(2,6-dimethyl-1,4-phenylene) ether is more preferred; Preferably, based on the total mass of the resin components in the resin composition being 100%, the content of the polyphenylene ether resin is 1-30%; Preferably, the resin composition further comprises a filler; Preferably, the filler is a powder filler, including any one or a combination of at least two of crystalline silica, amorphous silica, spherical silica, angular silica, chemical silica, silicon powder, hollow glass microspheres, titanium dioxide, strontium titanate, barium titanate, boron nitride, aluminum nitride, silicon nitride, silicon carbide, aluminum oxide, polytetrafluoroethylene, polyphenylene sulfide or polyether sulfone; Preferably, based on 100% of the total mass of the resin composition, the content of the filler is 50-70%.

6. A resin glue, characterized in that: The resin glue is obtained by dissolving or dispersing the resin composition according to any one of claims 1 to 5 in a solvent.

7. A resin film, characterized in that: The material of the resin film comprises the resin composition as described in any one of claims 1 to 5; Preferably, the resin film is obtained by coating the resin composition on a release material and then drying and / or semi-curing the resin composition.

8. A prepreg, characterized in that: The prepreg comprises a reinforcing material and a resin composition as claimed in any one of claims 1 to 5 attached to the reinforcing material; Preferably, the resin composition is attached to the reinforcing material by impregnation and then drying.

9. A metal foil-clad laminate, characterized in that: The metal foil-clad laminate includes a metal foil and at least one of the resin film according to claim 7 or the prepreg according to claim 8 .

10. A printed circuit board, characterized in that: The printed circuit board includes at least one of the resin film according to claim 7 , the prepreg according to claim 8 , or the metal foil-clad laminate according to claim 9 .

Citation Information

Patent Citations

  • Thermosetting hydrocarbon polymer composition, and prepreg and thermosetting copper-clad plate prepared therefrom

    CN110605880A

  • Halogen-free wear-resistant cable sheath material

    CN103788596A

  • Resin composition, prepreg, metal-clad laminate, and wiring board

    CN107108820A

  • Thermosetting resin composition, prepreg using thermosetting resin composition and copper-clad laminate

    CN112724640A