High-strength composite insulating cross arm core and preparation method thereof

Through the combination of modified meta-aramid fiber and epoxy resin, the problems of fragility and poor wear resistance of glass fibers are solved, the mechanical properties and wear resistance of insulated transverse cores are improved, and lightweight and high-strength are achieved and low powder produces effects.

CN119019814APending Publication Date: 2024-11-26FANGLONG GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411121414.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Glass fiber is fragile when used in insulated cross-bars and insulated struts and poor wear resistance, resulting in problems of crushing and powder drop during processing.

Method used

The aramid fiber is modified by flexible polyurethane to form a strong interface bonding layer to enhance mechanical properties and wear resistance.

Benefits of technology

It improves the interlayer shear strength, reduces core fragility and powder generation, reduces material waste, enhances wear resistance and lightweight properties, and is suitable for power insulation equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019814A_ABST
    Figure CN119019814A_ABST
Patent Text Reader

Abstract

The invention relates to a high-strength composite insulating cross arm core and a preparation method thereof, and belongs to the technical field of insulating cross arms in overhead lines of power distribution networks, the high-strength composite insulating cross arm core comprises modified meta-aramid fibers, epoxy resin and a curing agent, and the modified meta-aramid fibers are flexible polyurethane modified meta-aramid fibers. According to the improved composite core, the intermolecular bonding force is higher, the interface bonding performance is higher, a flexible interface is formed between the improved meta-aramid fiber and a resin matrix, the interlayer shear strength is improved, and the mechanical property is more excellent. The problem of core body fragmentation easily caused by crimping of the core body and the hardware fitting in the processing process is solved. And unnecessary material scrapping and waste conditions in the actual production process are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of insulating cross arms in overhead lines of distribution networks, and in particular relates to a high-strength composite insulating cross arm core and a preparation method thereof. Background Art

[0002] In overhead lines of distribution networks, cores are commonly used in insulating crossarms, insulating pillars and other equipment. The main materials of the core are glass fiber and epoxy resin, and epoxy resin is used as a curing agent in composite materials. As a reinforcing material in composite materials, glass fiber has good insulation, corrosion resistance, high mechanical strength and high temperature resistance, and is bonded and cured by epoxy resin. It is used in the core of insulating equipment in power, and its adaptability is extremely high. However, there are also some aspects of performance that are not very good.

[0003] Glass fiber is a brittle material. When crimping with metal fittings such as insulating crossarms or insulating pillars, the crimping parts are prone to breakage or even shattering. The core may be scrapped if you are not careful during processing. In addition, the wear resistance of glass fiber is relatively poor. When the core is stored and transported as a whole, a large amount of powder may fall off due to contact and friction between the surfaces. Summary of the invention

[0004] The present invention provides a high-strength composite insulating cross-arm core and a preparation method thereof, wherein aramid fiber has the characteristics of low density, high strength, high modulus, high temperature resistance, acid and alkali resistance, light weight, good insulation and aging resistance, etc.; its strength is 5 to 6 times that of steel wire, its modulus is 2 to 3 times that of steel wire or glass fiber, its toughness is 2 times that of steel wire, but its weight is only 1 / 5 of that of steel wire. In view of the problem of glass fiber performance, aramid fiber is considered to be used as a reinforcing material in the composite core.

[0005] The technical solution adopted by the present invention to achieve its purpose is as follows:

[0006] A high-strength composite insulating cross-arm core comprises modified meta-aramid fiber, epoxy resin and curing agent, wherein the modified meta-aramid fiber is meta-aramid fiber modified by flexible polyurethane, and the mass ratio of the modified meta-aramid fiber, epoxy resin and curing agent is 77:17:6.

[0007] Preferably, the modified meta-aramid fiber is prepared by the following method: immersing the meta-aramid fiber fabric in an aqueous solution of flexible polyurethane for 30 to 32 seconds, and drying at 70° C. for 10 hours after immersion to obtain the meta-aramid fiber modified by flexible polyurethane.

[0008] Preferably, the aqueous solution of the flexible polyurethane comprises, by mass percentage, 2% of waterborne polyurethane and waterborne polyurethane curing agent, and the balance is water.

[0009] Preferably, the molar ratio of -NCO in the waterborne polyurethane curing agent to -OH in the waterborne polyurethane is 0.8:1.

[0010] Preferably, the hard segment of the waterborne polyurethane is toluene diisocyanate, the soft segment is polyethylene adipate diol with a relative molecular weight of 800±50, and the molar ratio of -NCO in toluene diisocyanate and -OH in polyethylene adipate diol is controlled to be 1:3.

[0011] A method for preparing a high-strength composite insulating cross-arm core comprises the following steps:

[0012] S1. Preparation of an aqueous solution of a flexible polyurethane: toluene diisocyanate and polyethylene adipate diol having a relative molecular weight of 800±50 are reacted at 70°C for 6h to obtain an aqueous polyurethane, which is then mixed with a hexamethylene diisocyanate biuret water-based curing agent and water to obtain an aqueous solution of a flexible polyurethane;

[0013] S2. Preparation of flexible polyurethane-modified meta-aramid fiber: passing the meta-aramid fiber fabric through a rubber tank containing an aqueous solution of flexible polyurethane, and immersing the meta-aramid fiber in an aqueous solution of flexible polyurethane for 30 to 32 seconds, and after dipping, drying at 70 ° C for 10 hours to obtain a flexible polyurethane-modified meta-aramid fiber;

[0014] S3. Preparation of high-strength composite insulating cross-arm core: apply a layer of release agent to the cleaned mold, dry it naturally overnight, mix the epoxy resin and curing agent in a certain mass ratio, stir evenly, and dip the wound flexible polyurethane modified meta-aramid fiber. The coatings on both sides of the flexible polyurethane modified meta-aramid fiber are dipped with epoxy resin. During the dipping process, the total volume content of the epoxy resin is 34-36%. Then, the dipped flexible polyurethane modified meta-aramid fiber is placed in the mold for closing the mold and curing. The curing process is: first cure at 100°C for 2 hours, then adjust the temperature to 120°C for curing for 2 hours, and finally adjust the temperature to 150°C for curing for 1 hour.

[0015] Preferably, the molar ratio of -NCO in toluene diisocyanate to -OH in polyethylene adipate diol is 1:3, and the molar ratio of -NCO in the waterborne polyurethane curing agent to -OH in the waterborne polyurethane is 0.8:1.

[0016] The beneficial effects of the present invention are:

[0017] 1. The improved composite core has stronger intermolecular bonding force and stronger interface bonding performance. The improved meta-aramid fiber forms a flexible interface with the resin matrix, which improves the interlayer shear strength and has better mechanical properties. It solves the problem of core fragmentation caused by crimping of the core and hardware during processing. It reduces unnecessary material scrapping and waste in the actual production process.

[0018] 2. The improved meta-aramid fiber has stronger mechanical meshing and chemical bonding with the resin matrix, which enhances its wear resistance and does not produce a large amount of powder due to friction during actual storage and transportation.

[0019] 3. The density of meta-aramid fiber is about 1.44g / cm 3 Its density is much lower than that of glass fiber (2.4-2.76 g / cm 3 ), so the meta-aramid fiber is lighter and easier to transport, install and construct; compared with glass fiber, the same volume of meta-aramid fiber greatly reduces the mass of the core.

[0020] 4. During the actual production process, the environmental pollution is relatively small.

[0021] 5. Meta-aramid fiber has a higher tensile strength than glass fiber and is a plastic material. Therefore, it is not easy to break when the hardware is crimped during processing. Therefore, the vulnerability of the core is significantly reduced.

[0022] 6. After modification, meta-aramid fiber has strong wear resistance and is not easy to wear and break. Therefore, the core is not easy to wear and produce a lot of powder during storage, transportation and processing. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is the molecular structure of toluene diisocyanate.

[0024] Figure 2 This is a diagram of the molecular structure of polyethylene adipate glycol.

[0025] Figure 3 It is a molecular structure diagram of synthetic water-based polyurethane.

[0026] Figure 4 This is the molecular structure diagram of hexamethylene diisocyanate biuret water-based curing agent.

[0027] Figure 5 is a diagram of the structure of a flexible polyurethane coating.

[0028] Figure 6 This is a diagram of the molecular structure of meta-aramid fiber.

[0029] Figure 7 It is a schematic diagram of the transition layer of the molecular structure of meta-aramid fiber and epoxy resin. DETAILED DESCRIPTION

[0030] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work should belong to the scope of protection of the present invention.

[0031] During the bonding process of aramid fiber and epoxy resin, there are a large number of benzene rings on the main chain of meta-aramid fiber. The benzene rings have special stability and are difficult to react with the resin matrix. In addition, aramid fiber contains a large number of amide bonds (—CO—NH—), and there are a large number of hydrogen bonds between molecules. The surface of aramid fiber has a high degree of crystallinity and is relatively smooth. The interaction between meta-aramid fiber and the resin matrix is ​​limited to the weak secondary atomic force, which makes the interface adhesion of the composite material poor and the interlayer shear strength small. In addition, the molecular structures of aramid fiber and resin are quite different, and the transition layer is relatively thin during the bonding process. Therefore, it is necessary to thicken the transition layer during the bonding process to improve the performance of the composite material.

[0032] Therefore, the surface of meta-aramid fiber needs to be modified during the bonding process with epoxy resin. Introducing a strong and tough interface between the two can not only increase the bonding, but also have the function of interface relaxation, organically combining the reinforcing fiber and the matrix into a whole, and finally realize the effective transmission of interface stress, jointly bear the external force load, and improve the interface bonding effect between aramid fiber and resin matrix.

[0033] The principle of improving the combination of meta-aramid fiber and epoxy resin is to coat a layer of polymer resin or low molecular weight substance (flexible polyurethane coating) on ​​the surface of meta-aramid fiber to modify the fiber surface flexibility. This can heal the defects and damage on the fiber surface to a certain extent, thereby promoting the bonding force between aramid fiber and resin matrix, increasing the interlaminar shear strength of composite materials, and improving the fiber strength conversion rate of composite materials.

[0034] The flexible polyurethane coating consists of water-based polyurethane, water-based polyurethane curing agent and water.

[0035] Preparation principle of the scheme: The flexible polyurethane aqueous solution is used as a modified flexible coating on the surface of the meta-aramid fiber, which can achieve good interlayer bonding between the meta-aramid fiber and the resin material. By controlling the ratio of soft and hard segments in the waterborne polyurethane, the dispersibility and stability of the waterborne polyurethane in the aqueous solution are guaranteed. The polar polyurethane has a good bundling and coating effect on the aramid fiber, which is convenient for forming a transition layer on the surface of the meta-aramid fiber, thereby increasing the surface roughness and polar group content of the fiber, which is beneficial to the mechanical engagement and chemical bonding between the meta-aramid fiber and the resin matrix, and improving the interfacial bonding performance between the two. At the same time, the interfacial transition layer (i.e., the transition layer formed on the surface of the meta-aramid fiber modified by the flexible polyurethane) improves the infiltration and penetration of the resin matrix into the meta-aramid fiber, so that a flexible interface is formed in the meta-aramid fiber-resin composite material, which is beneficial to the interfacial stress transfer between the meta-aramid fiber and the matrix, and improves the interlaminar shear strength of the meta-aramid fiber and the resin composite material.

[0036] Example 1

[0037] A high-strength composite insulating cross-arm core comprises modified meta-aramid fiber, epoxy resin and curing agent, wherein the modified meta-aramid fiber is meta-aramid fiber modified by flexible polyurethane, and the mass ratio of the modified meta-aramid fiber, epoxy resin and curing agent is 77:17:6.

[0038] A preparation process of a high-strength composite insulating cross-arm core:

[0039] S1. Preparation process of flexible coating: Toluene diisocyanate (see Figure 1 ) and polyethylene adipate glycol with a relative molecular weight of 800 ± 50 (see Figure 2 ) was reacted at 70℃ for 6h to obtain waterborne polyurethane (see Figure 3 ), with hexamethylene diisocyanate biuret water-based curing agent (see Figure 4 ) and water to obtain an aqueous solution of flexible polyurethane, i.e., a flexible polyurethane coating (see Figure 5 ). The molar ratio of -NCO in toluene diisocyanate to -OH in polyethylene adipate glycol is 1:3, the molar ratio of -NCO in the curing agent to -OH in the obtained waterborne polyurethane is 0.8:1, and the aqueous solution of the flexible polyurethane comprises 2% of the waterborne polyurethane and the waterborne polyurethane curing agent by mass percentage, and the balance is water.

[0040] S2. The process of modifying meta-aramid fiber with flexible polyurethane coating: passing the meta-aramid fiber fabric through a glue tank containing an aqueous solution of flexible polyurethane, and immersing the meta-aramid fiber in the aqueous solution of flexible polyurethane for 30 to 32 seconds. During the dipping process, the substances in the aqueous solution of flexible polyurethane will be adsorbed on the fiber surface, and then a layer of coating mainly composed of polyurethane will be added to the fiber surface. After dipping, the meta-aramid fiber coated with the flexible coating is dried at 70°C for 10 hours to obtain meta-aramid fiber modified with the flexible polyurethane coating.

[0041] S3. Preparation process of composite materials of meta-aramid fiber and epoxy resin: apply a layer of release agent on the cleaned mold, dry it naturally overnight, then mix the epoxy resin and curing agent (hexamethylene diisocyanate biuret water-based curing agent) in a certain mass ratio, stir evenly, dip the wound fiber in the resin, and dip the coating on both sides of the meta-aramid fiber in the resin. The total volume content of the resin during the dipping process is 34-36%. Then put the dipped fiber in the mold and close the mold. The curing process is: first cure at 100°C for 2 hours, then adjust the temperature to 120°C for curing for 2 hours, and finally adjust the temperature to 150°C for curing for 1 hour to obtain a high-strength composite insulating crossarm core.

[0042] This scheme controls the ratio of soft and hard segments in waterborne polyurethane to form a transition layer on the surface of meta-aramid fiber, thereby increasing the surface roughness and polar groups of the fiber, which is beneficial to the mechanical meshing and chemical bonding of the meta-aramid fiber and the resin matrix, improves the interfacial bonding performance of the two, forms a flexible interface in the meta-aramid fiber and resin composite material, and improves the interlaminar shear strength.

[0043] Performance Indicators

[0044] Table 1

[0045] index Standard parameters Example 1 Tensile strength(MPa) ≥1100 1427 Bending strength(MPa) ≥900 1055.01 Compression strength(MPa) ≥450 478 In-plane shear strength (MPa) ≥45 119 Torsional strength (MPa) ≥90 98

Claims

1. A high-strength composite insulating cross-arm core, characterized in that: The invention comprises modified meta-aramid fiber, epoxy resin and curing agent, wherein the modified meta-aramid fiber is meta-aramid fiber modified by flexible polyurethane, and the mass ratio of the modified meta-aramid fiber, epoxy resin and curing agent is 77:17:

6.

2. A high-strength composite insulating cross-arm core according to claim 1, characterized in that: The modified meta-aramid fiber is prepared by the following method: the meta-aramid fiber fabric is immersed in an aqueous solution of flexible polyurethane for 30 to 32 seconds, and after dipping, it is dried at 70° C. for 10 hours to obtain the meta-aramid fiber modified by flexible polyurethane.

3. The high-strength composite insulating cross-arm core according to claim 2, characterized in that: The aqueous solution of the flexible polyurethane comprises, by mass percentage, 2% of waterborne polyurethane and waterborne polyurethane curing agent, and the balance is water.

4. The high-strength composite insulating cross-arm core according to claim 3, characterized in that: The molar ratio of -NCO in the waterborne polyurethane curing agent to -OH in the waterborne polyurethane is 0.8:

1.

5. The high-strength composite insulating cross-arm core according to claim 3, characterized in that: The hard segment of the waterborne polyurethane is toluene diisocyanate, the soft segment is polyethylene adipate diol with a relative molecular weight of 800±50, and the molar ratio of -NCO in toluene diisocyanate and -OH in polyethylene adipate diol is controlled to be 1:

3.

6. A method for preparing a high-strength composite insulating cross-arm core, characterized in that: The following steps are involved: S1. Preparation of an aqueous solution of a flexible polyurethane: toluene diisocyanate and polyethylene adipate diol having a relative molecular weight of 800±50 are reacted at 70°C for 6h to obtain an aqueous polyurethane, which is then mixed with a hexamethylene diisocyanate biuret water-based curing agent and water to obtain an aqueous solution of a flexible polyurethane; S2. Preparation of flexible polyurethane-modified meta-aramid fiber: passing the meta-aramid fiber fabric through a rubber tank containing an aqueous solution of flexible polyurethane, and immersing the meta-aramid fiber in an aqueous solution of flexible polyurethane for 30 to 32 seconds, and after dipping, drying at 70 ° C for 10 hours to obtain a flexible polyurethane-modified meta-aramid fiber; S3. Preparation of high-strength composite insulating cross-arm core: apply a layer of release agent to the cleaned mold, dry it naturally overnight, mix the epoxy resin and curing agent in a certain mass ratio, stir evenly, and dip the wound flexible polyurethane modified meta-aramid fiber. The coatings on both sides of the flexible polyurethane modified meta-aramid fiber are dipped with epoxy resin. During the dipping process, the total volume content of the epoxy resin is 34-36%. Then, the dipped flexible polyurethane modified meta-aramid fiber is placed in the mold for closing the mold and curing. The curing process is: first cure at 100°C for 2 hours, then adjust the temperature to 120°C for curing for 2 hours, and finally adjust the temperature to 150°C for curing for 1 hour.

7. The method for preparing a high-strength composite insulating cross-arm core according to claim 6, characterized in that: The molar ratio of -NCO in toluene diisocyanate and -OH in polyethylene adipate glycol is 1:3, and the molar ratio of -NCO in the waterborne polyurethane curing agent and -OH in the waterborne polyurethane is 0.8:1.