Nano ceramic liquid, preparation method and magnesium alloy plate surface treatment process

By preparing the surface treatment process of nanoceramic liquid and magnesium alloy plates, the problems of complex surface treatment of magnesium alloy plates and poor performance of existing coatings are solved, and ceramic coatings with strong corrosion resistance, high hardness and wear resistance are realized, and the process is simplified. Reduce costs.

CN119019873APending Publication Date: 2024-11-26邓宏论
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411122081.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The surface treatment of magnesium alloy plates is complex, has long processes, high cost, and the existing coatings are low hardness, wear-resistant and high thickness, making it difficult to meet diversified needs.

Method used

Using nanoceramic liquid, including ceramic resin, glass powder, zinc sulfate, mica powder, talc powder, alpha alumina powder, pigment and anhydrous alcohol, is prepared by grinding device, combined with plasma treatment and spraying technology, magnesium alloy plate surface treatment .

Benefits of technology

It realizes a ceramic coating with strong corrosion resistance, high hardness, wear resistance and good feel, simplifies the process and reduces costs, and has a small coating thickness and adjustable color.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides nano ceramic liquid, a preparation method and a magnesium alloy plate surface treatment process. The nano ceramic liquid comprises the following components in parts by mass: 40-50 parts of ceramic resin; 8 to 12 parts of glass powder; 9-13 parts of zinc sulfate; 5-7 parts of mica powder; 5-7 parts of talcum powder; 6-10 parts of alpha alumina powder; 13 to 16 parts of pigment; 2-4 parts of a dispersant; anhydrous alcohol; and 8 to 11 parts. The nano ceramic liquid disclosed by the invention belongs to a ceramic coating, is high in corrosion resistance, high in hardness, wear-resistant, good in hand feeling and adjustable in color, and can meet diversified requirements of customers on surface treatment; the preparation method of the nano ceramic liquid is simple and high in preparation efficiency; the magnesium alloy plate surface treatment process is simple in procedure, low in cost and small in coating weight increment, and the ceramic coating is high in corrosion resistance, high in hardness, resistant to abrasion, good in hand feeling and adjustable in color.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of nano coatings, and in particular to a nano ceramic liquid, a preparation method and a magnesium alloy plate surface treatment process. Background Art

[0002] Magnesium alloy is an alloy composed of magnesium and other elements. Its characteristics are: low density, high specific strength, large specific elastic modulus, good heat dissipation, good shock absorption, and greater impact load bearing capacity than aluminum alloy. It is often used to make notebook panels. However, the surface treatment of magnesium alloy plates is more difficult because magnesium alloys are prone to corrosion. The surface treatment of existing magnesium alloy plates is complicated, the process is long, the cost is high, and the effect is poor. The current process is to passivate or micro-arc oxidize the surface of the magnesium alloy plate, then apply a primer, a mid-coat, and then a top coat. In addition, organic coatings are used, which have low hardness, poor wear resistance, thick thickness, and heavy weight. Summary of the invention

[0003] In view of the above problems, the present invention proposes a nano ceramic liquid, a preparation method and a magnesium alloy plate surface treatment process.

[0004] The specific technical solutions of the present invention are as follows:

[0005] The present invention first proposes a nano ceramic liquid, comprising the following components in parts by weight:

[0006] Ceramic resin: 40-50 parts;

[0007] Glass powder: 8-12 parts;

[0008] Zinc sulfate: 9-13 parts;

[0009] Mica powder: 5-7 parts;

[0010] Talc: 5-7 parts;

[0011] α-alumina powder: 6-10 parts;

[0012] Pigment: 13-16 parts;

[0013] Dispersant: 2-4 parts;

[0014] Anhydrous alcohol; 8-11 parts.

[0015] Preferably, the particle sizes of the glass powder, the mica powder, the talc powder and the α-alumina powder are 500-800 nanometers.

[0016] Preferably, the glass powder is low-melting-point glass powder.

[0017] The present invention secondly proposes a method for preparing the nano ceramic liquid described above, using a grinding device, first adding ceramic resin, then adding glass powder, zinc sulfate, mica powder, talcum powder, α-alumina powder, pigment, dispersant in sequence, and finally adding anhydrous alcohol. When the particle size is less than 1 micron, the grinding can be stopped.

[0018] Preferably, the grinding device is a stirred mill, in which zirconium oxide grinding balls with a diameter of 3-5 mm are placed, the mass of the added zirconium oxide grinding balls is 30%-50% of the mass of the material to be produced, and the rotation speed is set to 300-1200, and the rotation speed is gradually increased as the amount of added raw materials increases. Alternatively, the grinding device can also be a sand mill.

[0019] The present invention again proposes a magnesium alloy plate surface treatment process, comprising the following steps:

[0020] (1) Preparation of nano-ceramic liquid: Use the nano-ceramic liquid described above, stir it so that there is no precipitation at the bottom of the container, and then check the viscosity to ensure that the viscosity is between 13 and 20 seconds. If the viscosity is too thick, add alcohol to dilute it. Filter the nano-ceramic liquid with a 400-mesh filter paper to filter out individual impurities and bubbles;

[0021] (2) Construction should be carried out in a cleanliness class 100,000 workshop with a temperature of 23-26 degrees and a humidity of no more than 80%. Construction operators should wear anti-static clothing;

[0022] (3) Wipe the surface of the magnesium alloy plate that has been passivated or micro-arc oxidized with alcohol, then use a plasma treatment machine to treat the surface, and then use the nano-ceramic liquid prepared in (1) for spraying. Use an upper tank spray gun, or a bottom-entry spray gun on an automatic production line, adjust the air intake pressure to 0.4-0.6MPA, and keep the spray gun 20-30cm away from the surface of the magnesium alloy plate. The spraying thickness should ensure that the cured coating is between 25-35μm.

[0023] (4) After spraying, place it in a clean place to dry on the surface for about 5-10 minutes, and then place it in an oven for baking and curing. The curing process is to heat it to 80 degrees in 10-15 minutes, maintain it for 30 minutes, then heat it to 120 degrees in 10 minutes, keep it warm for 60-80 minutes, then cool it down to below 100 degrees and take it out for routine inspection.

[0024] The beneficial effects of the present invention are as follows: 1. The nano-ceramic liquid of the present invention is a ceramic coating with strong corrosion resistance, high hardness, wear resistance, good hand feel, and adjustable color, which can meet the diversified surface treatment needs of customers; 2. The preparation method of the nano-ceramic liquid of the present invention is simple and has high preparation efficiency; 3. The surface treatment process of the magnesium alloy plate of the present invention has simple procedures, low cost, small coating weight gain, and is a ceramic coating with strong corrosion resistance, high hardness, wear resistance, good hand feel, and adjustable color. DETAILED DESCRIPTION

[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0026] Example 1

[0027] The present invention first proposes a nano ceramic liquid, comprising the following components in parts by weight:

[0028] Ceramic resin: 40-50 parts;

[0029] Glass powder: 8-12 parts;

[0030] Zinc sulfate: 9-13 parts;

[0031] Mica powder: 5-7 parts;

[0032] Talc: 5-7 parts;

[0033] α-alumina powder: 6-10 parts;

[0034] Pigment: 13-16 parts;

[0035] Dispersant: 2-4 parts;

[0036] Anhydrous alcohol; 8-11 parts.

[0037] Preferably, the particle sizes of the glass powder, the mica powder, the talc powder and the α-alumina powder are 500-800 nanometers.

[0038] Preferably, the glass powder is low melting point glass powder, and the dispersant is Byk dispersant.

[0039] Example 2

[0040] A method for preparing the nano-ceramic liquid of Example 1 comprises using a grinding device, first adding ceramic resin, then sequentially adding glass powder, zinc sulfate, mica powder, talcum powder, α-alumina powder, pigment, dispersant, and finally adding anhydrous alcohol. When the particle size is less than 1 micron, grinding can be stopped.

[0041] Preferably, the grinding device is a stirred mill, in which zirconium oxide grinding balls with a diameter of 3-5 mm are placed, the mass of the added zirconium oxide grinding balls is 30%-50% of the mass of the material to be produced, and the rotation speed is set to 300-1200, and the rotation speed is gradually increased as the amount of added raw materials increases. Alternatively, the grinding device can also be a sand mill.

[0042] Example 3

[0043] A magnesium alloy plate surface treatment process comprises the following steps:

[0044] (1) Preparation of nano-ceramic liquid: Use the nano-ceramic liquid described in Example 1 or the nano-ceramic liquid prepared by the method of Example 2, stir it so that there is no precipitation at the bottom of the container, and then check the viscosity to ensure that the viscosity is between 13 and 20 seconds. If the viscosity is too thick, add alcohol to dilute it, and filter the nano-ceramic liquid with a 400-mesh filter paper to filter out individual impurities and bubbles;

[0045] (2) Construction should be carried out in a cleanliness class 100,000 workshop with a temperature of 23-26 degrees and a humidity of no more than 80%. Construction operators should wear anti-static clothing;

[0046] (3) Wipe the surface of the magnesium alloy plate that has been passivated or micro-arc oxidized with alcohol, then use a plasma treatment machine to treat the surface, and then use the nano-ceramic liquid prepared in (1) for spraying. Use an upper tank spray gun, or a bottom-entry spray gun on an automatic production line, adjust the air intake pressure to 0.4-0.6MPA, and keep the spray gun 20-30cm away from the surface of the magnesium alloy plate. The spraying thickness should ensure that the cured coating is between 25-35μm.

[0047] (4) After spraying, place it in a clean place to dry on the surface for about 5-10 minutes, and then place it in an oven for baking and curing. The curing process is to heat it to 80 degrees in 10-15 minutes, maintain it for 30 minutes, then heat it to 120 degrees in 10 minutes, keep it warm for 60-80 minutes, then cool it down to below 100 degrees and take it out for routine inspection.

[0048] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A nano ceramic liquid, characterized in that: The composition comprises the following components in parts by weight: Ceramic resin: 40-50 parts; Glass powder: 8-12 parts; Zinc sulfate: 9-13 parts; Mica powder: 5-7 parts; Talc: 5-7 parts; α-alumina powder: 6-10 parts; Pigment: 13-16 parts; Dispersant: 2-4 parts; Absolute alcohol; 8-11 parts.

2. The nano ceramic liquid according to claim 1, characterized in that: The particle sizes of the glass powder, the mica powder, the talc powder and the α-alumina powder are 500-800 nanometers.

3. The nano ceramic liquid according to claim 1, characterized in that: The glass powder is low melting point glass powder.

4. A method for preparing a nano ceramic liquid, characterized in that: Use a grinding device, first add ceramic resin, then add glass powder, zinc sulfate, mica powder, talcum powder, α-alumina powder, pigment, dispersant in sequence, and finally add anhydrous alcohol. When the particle size is less than 1 micron, stop grinding.

5. The method for preparing the nano ceramic liquid according to claim 1, characterized in that: The grinding device is a stirred mill, in which zirconium oxide grinding balls with a diameter of 3-5 mm are placed. The mass of the added zirconium oxide grinding balls is 30%-50% of the mass of the material to be produced. The rotation speed is set to 300-1200, and the rotation speed is gradually increased as the amount of added raw materials increases.

6. The method for preparing nano ceramic liquid according to claim 1, characterized in that: The grinding device is a sand mill.

7. A magnesium alloy plate surface treatment process, characterized in that: The following steps are involved: (1) Preparation of nano-ceramic liquid: Use nano-ceramic liquid, stir it so that there is no precipitation at the bottom of the container, and then check the viscosity to ensure that the viscosity is between 13 and 20 seconds. If the viscosity is too thick, add alcohol to dilute it. Filter the nano-ceramic liquid with 400 mesh filter paper to filter out individual impurities and bubbles; (2) Construction should be carried out in a cleanliness class 100,000 workshop with a temperature of 23-26 degrees and a humidity of no more than 80%. Construction operators should wear anti-static clothing; (3) Wipe the surface of the magnesium alloy plate that has been passivated or micro-arc oxidized with alcohol, then use a plasma treatment machine to treat the surface, and then use the nano-ceramic liquid prepared in (1) for spraying. Use an upper tank spray gun, or a bottom-entry spray gun on an automatic production line, adjust the air intake pressure to 0.4-0.6MPA, and keep the spray gun 20-30cm away from the surface of the magnesium alloy plate. The spraying thickness should ensure that the cured coating is between 25-35μm. (4) After spraying, place it in a clean place to dry on the surface for about 5-10 minutes, and then place it in an oven for baking and curing. The curing process is to heat it to 80 degrees in 10-15 minutes, maintain it for 30 minutes, then heat it to 120 degrees in 10 minutes, keep it warm for 60-80 minutes, then cool it down to below 100 degrees and take it out for routine inspection.

Citation Information

Patent Citations

  • Preparation method of magnesium alloy surface micro-arc oxidation / spray coating compound film

    CN101871119A

  • Solar energy absorbing film and preparing method thereof

    CN105238091A

  • High-hardness nano ceramic resin

    CN106349934A

  • High-temperature-resistant compact anticorrosive paint and preparation method thereof

    CN110938321A

  • Heat dissipation coating, preparation method thereof and heating device

    CN116676000A