Natural colored shell piece real stone paint and preparation method thereof

By preparing specific ratios and functional additives, the durability, weather resistance, and antibacterial properties of real stone paint are improved, solving the problem of insufficient performance of existing real stone paint and achieving a longer service life and beautiful decorative effect.

CN119019876AInactive Publication Date: 2024-11-26QUZHOU WEITEJIA COATING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411495881.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-25
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing stone-like paints have poor weather resistance, durability, and antibacterial properties, resulting in insufficient decorative effect and affecting service life and quality.

Method used

Using a specific ratio of polyacrylate emulsion, natural colored sand, nano titanium dioxide, natural colored shell flakes and other raw materials, and by preparing functional additives, including modifiers and defoamers, the durability and antibacterial properties of the paint are improved, and unique colors and textures are added.

Benefits of technology

The prepared natural shell flake stone paint has excellent durability, weather resistance and antibacterial properties, extending its service life, while also having unique colors and beautiful decorative effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of paint, in particular to natural colored shell piece real stone paint and a preparation method thereof. The natural colored shell piece real stone paint is prepared from the following raw materials in parts by weight: 120 to 150 parts of polyacrylate emulsion, 700 to 750 parts of natural colored sand, 4 to 7 parts of nano titanium dioxide, 20 to 30 parts of natural colored shell pieces, 2 to 4 parts of hydroxyethyl cellulose, 1.5 to 2.5 parts of sodium hydroxide, 7 to 10 parts of propylene glycol methyl ether acetate, 5 to 8 parts of functional additive, 3 to 5 parts of ethylene glycol, 2 to 4 parts of preservative, 6 to 9 parts of defoaming agent, 4 to 6 parts of thickening agent, 3 to 6 parts of dispersing agent and 100 to 120 parts of deionized water. The natural colored shell piece real stone paint prepared by the invention not only has excellent durability and weather resistance, but also has good antibacterial property, and the service life of the natural colored shell piece real stone paint is prolonged while the quality of the natural colored shell piece real stone paint is ensured; in addition, the prepared natural colored shell piece real stone paint has unique color and texture, and the decorative effect of the natural colored shell piece real stone paint is more attractive and personalized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, in particular to a natural colorful shell flake real stone paint and a preparation method thereof. Background Art

[0002] Real stone paint, also known as liquid stone, is a kind of paint with decorative effects similar to marble and granite. Real stone paint is mainly made of natural stone powder of various colors. According to the finishing effect, real stone paint can be divided into four categories: single-color real stone paint, multi-color real stone paint, rock flake real stone paint and imitation brick real stone paint. Real stone paint has the texture of natural stone, various grid designs, and can provide various three-dimensional pattern structures. It is a substitute for dry-hanging stone on the exterior wall; at the same time, the paint uses water-based emulsion, which is non-toxic and environmentally friendly, and can be used on cement brick walls, foam, gypsum and other base surfaces.

[0003] The patent document with application number "CN201810173942.8" discloses an anti-shedding graphene real stone paint and a preparation method thereof. The anti-shedding graphene real stone paint is composed of the following ingredients in weight ratio: 20 to 35 parts of emulsion; 3 to 5 parts of hydroxyethyl cellulose; 7 to 12 parts of graphene; 65 to 80 parts of natural colored sand; 0.8 to 1.4 parts of defoaming agent; 0.5 to 1.5 parts of adhesion promoter; 0.5 to 1 part of thickener; 5 to 10 parts of film-forming aid; 1 to 2 parts of N-aminopropyl-methylethanolamine; and 25 to 45 parts of water.

[0004] Although the real stone paint products prepared by the above patent documents have excellent bonding strength and are not prone to peeling, bubbling and other phenomena. However, its weather resistance, durability and antibacterial properties are relatively poor, which affects its service life and quality to a certain extent. Furthermore, it does not have unique color and texture, and the decorative effect is relatively insufficient. Based on this, the present invention provides a natural color shell flake real stone paint and a preparation method thereof to solve the above-mentioned technical problems! Summary of the invention

[0005] The object of the present invention is to provide a natural colored shell flake stone paint and a preparation method thereof, wherein the prepared natural colored shell flake stone paint not only has excellent durability and weather resistance, but also has good antibacterial properties, and while ensuring its quality, it also prolongs its service life to a certain extent. In addition, the natural colored shell flake stone paint prepared by the present invention also has unique color and texture, and its decorative effect is also more beautiful and personalized.

[0006] To achieve the above object, the present invention provides the following technical solutions: A natural colored shell flake real stone paint is composed of the following raw materials in parts by weight: 120-150 parts of polyacrylate emulsion, 700-750 parts of natural colored sand, 4-7 parts of nano titanium dioxide, 20-30 parts of natural colored shell flakes, 2-4 parts of hydroxyethyl cellulose, 1.5-2.5 parts of sodium hydroxide, 7-10 parts of propylene glycol methyl ether acetate, 5-8 parts of functional additives, 3-5 parts of ethylene glycol, 2-4 parts of preservatives, 6-9 parts of defoaming agents, 4-6 parts of thickeners, 3-6 parts of dispersants and 100-120 parts of deionized water.

[0007] Furthermore, the preparation method of the functional additive is: to a spherical zinc oxide micropowder aqueous dispersion with a concentration of 20 to 50 mg / mL, a modifier with a mass of 20 to 40 times that of the spherical zinc oxide micropowder, 100 to 200 times that of N-hydroxyethyl acrylamide, 0.5 to 1 times that of p-hydroxyanisole, and 20 to 25 times that of ammonium persulfate are added respectively, and after mixing and stirring evenly, the mixture is kept warm for reaction at a temperature of 120 to 140° C. for 20 to 30 minutes; after the reaction is completed, the obtained product components are sequentially subjected to solid-liquid separation, washing and vacuum drying to obtain the functional additive.

[0008] Furthermore, the preparation method of the modifier comprises the following steps: Step 1, epichlorohydrin and N,N-dimethylhexylamine are mixed and stirred evenly at a mass ratio of 1:1.5-2.0, and the mixture is stirred and reacted at a temperature of 50-60° C. for 15-25 hours; after the reaction is completed, the precipitated product is washed with ether, and then dried under reduced pressure to obtain a first solid powder; Step 2, epichlorohydrin and N,N-dimethylpropylamine are mixed and stirred evenly in a mass ratio of 1:2-3, and the mixture is stirred and reacted at a temperature of 40-50° C. for 15-25 hours; after the reaction is completed, the precipitated product is washed with ether, and then dried under reduced pressure to obtain a second solid powder; Step 3: Adjust the pH value of the chitosan citrate aqueous solution at a temperature of 55-65°C and a concentration of 0.8-1 g / mL to 5.5-6.5, and add a mixed solution of 5-8% of the chitosan citrate aqueous solution by volume thereto, mix well, heat to 55-65°C, and keep the reaction at this temperature for 30-50 hours; after the reaction is completed, wash the precipitate obtained by the reaction with anhydrous ethanol for 3-4 times, and then vacuum dry it to obtain a modifier; the chitosan citrate has a deacetylation degree of 85% and an average molecular weight of 80,000.

[0009] Furthermore, the preparation method of the mixed solution is: put the first solid powder into deionized water at a solid-liquid ratio of 0.08-0.12 g / mL, and add the second solid powder whose mass is 1.5-2.0 times of the first solid powder, and mix and stir evenly to obtain the mixed solution.

[0010] Furthermore, the preservative is selected from any one of Rohm and Haas LXE preservative and Deqian MB-16 preservative.

[0011] Furthermore, the defoaming agent is selected from any one of Nopco SN-NXZ defoaming agent and BYK-024 defoaming agent.

[0012] Furthermore, the thickener is selected from any one of thickener DSX 3551, thickener SN-636, and thickener DSX 3290.

[0013] Furthermore, the dispersant is selected from any one of BYK-156 dispersant and Dow H-30A dispersant.

[0014] Furthermore, the particle size of the natural colored sand is 80-120 meshes; the natural colored shell pieces are selected from any one of cherry shells, light pink scallops, and flame shells, and the particle size of the natural colored shell pieces is 60-100 meshes.

[0015] A method for preparing natural colored shell flake real stone paint comprises the following steps: The first step is to weigh the raw materials required for preparing the natural colored shell flake real stone paint as needed, and then mix the hydroxyethyl cellulose and deionized water and stir them evenly, and the obtained hydroxyethyl cellulose mixed solution is stored and used for standby; The second step is to put half of the natural colored sand into the mixing equipment, add the hydroxyethyl cellulose mixed solution, and add the remaining raw materials except sodium hydroxide and thickener while stirring at a rate of 100-150r / min. After mixing and stirring for 5-10 minutes, add the remaining raw materials, continue mixing and stirring for 20-30 minutes, and then fill the obtained mixed slurry into a barrel to obtain natural colored shell flake real stone paint.

[0016] Compared with the prior art, the present invention has the following beneficial effects: The present invention uses epichlorohydrin and N, N-dimethylpropylamine as raw materials to prepare a first solid powder, and uses epichlorohydrin and N, N-dimethylpropylamine as raw materials to prepare a second solid powder. The prepared first solid powder and the second solid powder are prepared into a mixed solution and added to a chitosan citrate aqueous solution, and a modifier is prepared after a heat preservation reaction. Then the modifier, spherical zinc oxide micropowder, N-hydroxyethyl acrylamide and p-hydroxyanisole are used as raw materials, and a chemical reaction occurs between the relevant raw materials under the action of ammonium persulfate, and the surface of the spherical zinc oxide micropowder is successfully bonded to the modifier, so that the prepared functional additive not only has excellent durability and weather resistance, but also prolongs its service life to a certain extent, and also has a good antibacterial effect. The prepared functional additive is used as a raw material for natural color shell flake real stone paint, which not only prolongs its service life to a certain extent, but also effectively guarantees its quality. In addition, the natural color shell flake real stone paint prepared by the present invention has a unique color and texture, and its decorative effect is also more beautiful and personalized. DETAILED DESCRIPTION

[0017] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] Example 1: A natural colored shell flake real stone paint is composed of the following raw materials in parts by weight: 120 parts of polyacrylate emulsion, 700 parts of natural colored sand, 4 parts of nano titanium dioxide, 20 parts of natural colored shell flakes, 2 parts of hydroxyethyl cellulose, 1.5 parts of sodium hydroxide, 7 parts of propylene glycol methyl ether acetate, 5 parts of functional additives, 3 parts of ethylene glycol, 2 parts of Rohm and Haas LXE preservative, 6 parts of Nopco SN-NXZ defoamer, 4 parts of thickener DSX 3551, 3 parts of BYK-156 dispersant and 100 parts of deionized water; wherein, the particle size of the natural colored sand is 80 mesh; the natural colored shell flakes are selected from cherry shells, and the particle size of the natural colored shell flakes is 60 mesh.

[0019] The preparation method of the functional additive is as follows: to a spherical zinc oxide micropowder aqueous dispersion with a concentration of 20 mg / mL, a modifier with a mass 20 times that of the spherical zinc oxide micropowder, 100 times that of N-hydroxyethyl acrylamide, 0.5 times that of p-hydroxyanisole, and 20 times that of ammonium persulfate are added respectively, and the mixture is mixed and stirred evenly, and then kept warm for reaction at a temperature of 120°C for 20 minutes; after the reaction is completed, the obtained product components are sequentially subjected to solid-liquid separation, washing, and vacuum drying to obtain the functional additive; wherein, the spherical zinc oxide micropowder is purchased from Ningbo Beijiaer New Materials Co., Ltd., and its average particle size is 300 nm.

[0020] The preparation method of the modifier comprises the following steps: Step 1, epichlorohydrin and N,N-dimethylhexylamine are mixed and stirred evenly at a mass ratio of 1:1.5, and the mixture is stirred and reacted at a temperature of 50° C. for 15 hours; after the reaction is completed, the precipitated product is washed with ether, and then dried under reduced pressure to obtain a first solid powder; Step 2, epichlorohydrin and N,N-dimethylpropylamine are mixed and stirred evenly in a mass ratio of 1:2, and the mixture is stirred and reacted at a temperature of 40° C. for 15 hours; after the reaction is completed, the precipitated product is washed with ether, and then dried under reduced pressure to obtain a second solid powder; Step 3, the pH of the chitosan citrate aqueous solution at a temperature of 55°C and a concentration of 0.8g / mL is adjusted to 5.5, and a mixed solution with a volume of 5% of the chitosan citrate aqueous solution is added thereto, the mixture is mixed evenly, the temperature is raised to 55°C, and the reaction is kept at this temperature for 30 hours; after the reaction is completed, the precipitate obtained by the reaction is washed 3 times with anhydrous ethanol, and then vacuum dried to obtain a modifier; the deacetylation degree of chitosan citrate is 85%, and the average molecular weight is 80,000; wherein, the preparation method of the mixed solution is: the first solid powder is put into deionized water at a solid-liquid ratio of 0.08g / mL, and the second solid powder with a mass 1.5 times that of the first solid powder is added thereto, and the mixed solution is obtained after mixing and stirring evenly.

[0021] A method for preparing natural colored shell flake real stone paint comprises the following steps: The first step is to weigh the raw materials required for preparing the natural colored shell flake real stone paint as needed, and then mix the hydroxyethyl cellulose and deionized water and stir them evenly, and the obtained hydroxyethyl cellulose mixed solution is stored and used for standby; The second step is to put half of the natural colored sand into the mixing equipment, add the hydroxyethyl cellulose mixed solution, and add the remaining raw materials except sodium hydroxide and thickener while stirring at a rate of 100r / min. After mixing and stirring for 5 minutes, add the remaining raw materials, continue mixing and stirring for 20 minutes, and then put the obtained mixed slurry into a barrel to obtain natural colored shell flake real stone paint.

[0022] Example 2: The preparation method of a natural colored shell flake stone paint provided in this example is basically the same as that in Example 1, except that the specific composition of the natural colored shell flake stone paint and the preparation method of the functional additives are not exactly the same, and the specific composition of the natural colored shell flake stone paint and the preparation method of the functional additives in this example are as follows: A natural colored shell flake real stone paint is composed of the following raw materials in parts by weight: 140 parts of polyacrylate emulsion, 720 parts of natural colored sand, 5 parts of nano titanium dioxide, 25 parts of natural colored shell flakes, 3 parts of hydroxyethyl cellulose, 2 parts of sodium hydroxide, 8 parts of propylene glycol methyl ether acetate, 6 parts of functional additives, 4 parts of ethylene glycol, 3 parts of Deqian MB-16 preservative, 8 parts of BYK-024 defoamer, 5 parts of thickener SN-636, 4 parts of Dow H-30A dispersant and 110 parts of deionized water; wherein the particle size of the natural colored sand is 100 meshes; the natural colored shell flakes are light pink scallops, and the particle size of the natural colored shell flakes is 80 meshes.

[0023] The preparation method of the functional additive is as follows: to a 30 mg / mL aqueous dispersion of spherical zinc oxide micropowder, 30 times the mass of a modifier, 150 times the mass of N-hydroxyethyl acrylamide, 0.8 times the mass of p-hydroxyanisole, and 20 times the mass of ammonium persulfate are added respectively, and the mixture is stirred evenly and then kept warm for reaction at a temperature of 130° C. for 25 minutes; after the reaction is completed, the obtained product components are sequentially subjected to solid-liquid separation, washing, and vacuum drying to obtain the functional additive.

[0024] The preparation method of the modifier comprises the following steps: Step 1, epichlorohydrin and N,N-dimethylhexylamine are mixed and stirred evenly at a mass ratio of 1:1.5, and the mixture is stirred and reacted at a temperature of 55° C. for 20 hours; after the reaction is completed, the precipitated product is washed with ether, and then dried under reduced pressure to obtain a first solid powder; Step 2, epichlorohydrin and N,N-dimethylpropylamine are mixed and stirred evenly in a mass ratio of 1:2, and the mixture is stirred and reacted at a temperature of 45° C. for 20 hours; after the reaction is completed, the precipitated product is washed with ether, and then dried under reduced pressure to obtain a second solid powder; Step 3, the pH of the chitosan citrate aqueous solution at a temperature of 60°C and a concentration of 0.8g / mL is adjusted to 6, and a mixed solution with a volume of 6% of the chitosan citrate aqueous solution is added thereto, the mixture is mixed evenly, the temperature is raised to 60°C, and the reaction is kept at this temperature for 40 hours; after the reaction is completed, the precipitate obtained by the reaction is washed 3 times with anhydrous ethanol, and then vacuum dried to obtain a modifier; the deacetylation degree of chitosan citrate is 85%, and the average molecular weight is 80,000; wherein, the preparation method of the mixed solution is: the first solid powder is put into deionized water at a solid-liquid ratio of 0.1g / mL, and the second solid powder with a mass 1.5 times that of the first solid powder is added thereto, and the mixed solution is obtained after mixing and stirring evenly.

[0025] Example 3: The preparation method of a natural colored shell flake stone paint provided in this example is basically the same as that in Example 1, except that the specific composition of the natural colored shell flake stone paint and the preparation method of the functional additives are not exactly the same, and the specific composition of the natural colored shell flake stone paint and the preparation method of the functional additives in this example are as follows: A natural colored shell flake real stone paint is composed of the following raw materials in parts by weight: 150 parts of polyacrylate emulsion, 750 parts of natural colored sand, 7 parts of nano titanium dioxide, 30 parts of natural colored shell flakes, 4 parts of hydroxyethyl cellulose, 2.5 parts of sodium hydroxide, 10 parts of propylene glycol methyl ether acetate, 8 parts of functional additives, 5 parts of ethylene glycol, 4 parts of Rohm and Haas LXE preservatives, 9 parts of Nopco SN-NXZ defoaming agents, 6 parts of thickener DSX 3290, 6 parts of BYK-156 dispersant and 120 parts of deionized water; wherein the particle size of the natural colored sand is 120 meshes; the natural colored shell flakes are flame shells; and the particle size of the natural colored shell flakes is 100 meshes.

[0026] The preparation method of the functional additive is as follows: to a 50 mg / mL aqueous dispersion of spherical zinc oxide micropowder, 40 times the mass of a modifier, 200 times the mass of N-hydroxyethyl acrylamide, 1 times the mass of p-hydroxyanisole, and 25 times the mass of ammonium persulfate are added respectively, and the mixture is stirred evenly and then kept warm for reaction at a temperature of 140°C for 30 minutes; after the reaction is completed, the obtained product components are sequentially subjected to solid-liquid separation, washing, and vacuum drying to obtain the functional additive.

[0027] The preparation method of the modifier comprises the following steps: Step 1, epichlorohydrin and N,N-dimethylhexylamine are mixed and stirred evenly in a mass ratio of 1:2.0, and the mixture is stirred and reacted at a temperature of 60° C. for 25 hours; after the reaction is completed, the precipitated product is washed with ether, and then dried under reduced pressure to obtain a first solid powder; Step 2, epichlorohydrin and N,N-dimethylpropylamine are mixed and stirred evenly in a mass ratio of 1:3, and the mixture is stirred and reacted at a temperature of 50° C. for 25 hours; after the reaction is completed, the precipitated product is washed with ether, and then dried under reduced pressure to obtain a second solid powder; Step 3, the pH of the chitosan citrate aqueous solution at a temperature of 65°C and a concentration of 1g / mL is adjusted to 6.5, and a mixed solution with a volume of 8% of the chitosan citrate aqueous solution is added thereto, the mixture is mixed evenly, the temperature is raised to 65°C, and the reaction is kept at this temperature for 50 hours; after the reaction is completed, the precipitate obtained by the reaction is washed 4 times with anhydrous ethanol, and then vacuum dried to obtain a modifier; the deacetylation degree of chitosan citrate is 85%, and the average molecular weight is 80,000; wherein, the preparation method of the mixed solution is: the first solid powder is put into deionized water at a solid-liquid ratio of 0.12g / mL, and the second solid powder with a mass 2.0 times that of the first solid powder is added thereto, and the mixed solution is obtained after mixing and stirring evenly.

[0028] The difference between the comparative example and Example 1 is that in this example, an equal amount of spherical zinc oxide powder is used to replace the functional additive.

[0029] Performance test: The relevant properties of the natural colored shell flake real stone paint samples provided in Examples 1 to 3 and the comparative example were tested respectively, and the test data obtained were recorded in the following table:

[0030] By comparing and analyzing the relevant data in the table, it can be known that the natural color shell flake real stone paint prepared by the present invention not only has excellent durability and weather resistance, but also has good antibacterial properties, while ensuring its quality, it also prolongs its service life to a certain extent. In addition, the natural color shell flake real stone paint prepared by the present invention also has unique color and texture, and its decorative effect is also more beautiful and personalized. Thus it is shown that a kind of natural color shell flake real stone paint provided by the present invention and preparation method thereof have broader market prospects and are more suitable for promotion.

[0031] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0032] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A natural colored shell flake real stone paint, characterized in that: The invention is composed of the following raw materials in parts by weight: 120-150 parts of polyacrylate emulsion, 700-750 parts of natural colored sand, 4-7 parts of nano titanium dioxide, 20-30 parts of natural colored shell slices, 2-4 parts of hydroxyethyl cellulose, 1.5-2.5 parts of sodium hydroxide, 7-10 parts of propylene glycol methyl ether acetate, 5-8 parts of functional additives, 3-5 parts of ethylene glycol, 2-4 parts of preservatives, 6-9 parts of defoaming agents, 4-6 parts of thickeners, 3-6 parts of dispersants and 100-120 parts of deionized water.

2. The natural colored shell flake real stone paint according to claim 1, characterized in that: The preparation method of the functional additive comprises the following steps: adding a modifier 20 to 40 times the mass of the spherical zinc oxide fine powder, 100 to 200 times the mass of N-hydroxyethyl acrylamide, 0.5 to 1 times the mass of p-hydroxyanisole, and 20 to 25 times the mass of ammonium persulfate to a spherical zinc oxide fine powder aqueous phase dispersion liquid with a concentration of 20 to 50 mg / mL, mixing and stirring evenly, and then heat-retaining and reacting at a temperature of 120 to 140° C. for 20 to 30 minutes; after the reaction is completed, sequentially performing solid-liquid separation, washing, and vacuum drying treatment on the obtained product components to obtain the functional additive.

3. A natural colored shell flake real stone paint according to claim 2, characterized in that: The preparation method of the modifier comprises the following steps: Step 1, epichlorohydrin and N,N-dimethylhexylamine are mixed and stirred evenly at a mass ratio of 1:1.5-2.0, and the mixture is stirred and reacted at a temperature of 50-60° C. for 15-25 hours; after the reaction is completed, the precipitated product is washed with ether, and then dried under reduced pressure to obtain a first solid powder; Step 2, epichlorohydrin and N,N-dimethylpropylamine are mixed and stirred evenly in a mass ratio of 1:2-3, and the mixture is stirred and reacted at a temperature of 40-50° C. for 15-25 hours; after the reaction is completed, the precipitated product is washed with ether, and then dried under reduced pressure to obtain a second solid powder; Step 3: Adjust the pH value of the chitosan citrate aqueous solution at a temperature of 55-65°C and a concentration of 0.8-1 g / mL to 5.5-6.5, and add a mixed solution of 5-8% of the chitosan citrate aqueous solution by volume thereto, mix well, heat to 55-65°C, and keep the reaction at this temperature for 30-50 hours; after the reaction is completed, wash the precipitate obtained by the reaction with anhydrous ethanol for 3-4 times, and then vacuum dry it to obtain a modifier; the chitosan citrate has a deacetylation degree of 85% and an average molecular weight of 80,000.

4. The natural colored shell flake real stone paint according to claim 3, characterized in that: The preparation method of the mixed solution is: adding the first solid powder into deionized water at a solid-liquid ratio of 0.08-0.12 g / mL, adding the second solid powder with a mass 1.5-2.0 times that of the first solid powder, and mixing and stirring to obtain the mixed solution.

5. The natural colored shell flake real stone paint according to claim 1, characterized in that: The preservative is selected from any one of Rohm and Haas LXE preservative and Deqian MB-16 preservative.

6. The natural colored shell flake real stone paint according to claim 1, characterized in that: The defoamer can be any one of Nopco SN-NXZ defoamer and BYK-024 defoamer.

7. The natural colored shell flake real stone paint according to claim 1, characterized in that: The thickener is selected from any one of thickener DSX 3551, thickener SN-636, and thickener DSX 3290.

8. The natural colored shell flake real stone paint according to claim 1, characterized in that: The dispersant is selected from any one of BYK-156 dispersant and Dow H-30A dispersant.

9. The natural colored shell flake real stone paint according to claim 1, characterized in that: The particle size of the natural colored sand is 80-120 meshes; the natural colored shell pieces are selected from any one of cherry shells, light pink scallops, and flame shells, and the particle size of the natural colored shell pieces is 60-100 meshes.

10. A method for preparing a natural colored shell flake real stone paint according to any one of claims 1 to 9, characterized in that: The following steps are involved: The first step is to weigh the raw materials required for preparing the natural colored shell flake real stone paint as needed, and then mix the hydroxyethyl cellulose and deionized water and stir them evenly, and the obtained hydroxyethyl cellulose mixed solution is stored and used for standby; The second step is to put half of the natural colored sand into the mixing equipment, add the hydroxyethyl cellulose mixed solution, and add the remaining raw materials except sodium hydroxide and thickener while stirring at a rate of 100-150r / min. After mixing and stirring for 5-10 minutes, add the remaining raw materials, continue mixing and stirring for 20-30 minutes, and then fill the obtained mixed slurry into a barrel to obtain natural colored shell flake real stone paint.

Citation Information

Patent Citations

  • Real stone paint and preparation method thereof

    CN103555082A

  • High-performance real-stone-like paint and preparation method thereof

    CN108300024A

  • Efficient air disinfectant and preparation method thereof

    CN115997790A

  • Microcapsule type antibacterial flame-retardant ABS (Acrylonitrile Butadiene Styrene) material and preparation process thereof

    CN118562244A

  • Stone paint formulation and methods for producing the same

    US20170305793A1