Weather-resistant water-based vehicle body paint and preparation method thereof

By optimizing the formulation and process of water-based car body paint, and using components such as weather-resistant acrylic copolymer and modified talc, a car body paint with high cross-linking density is formed and a waterproof silicone film is formed on the surface. This solves the problems of insufficient wear resistance, weather resistance and corrosion resistance of water-based car body paint, and achieves better adhesion and waterproof performance.

CN119019901AActive Publication Date: 2024-11-26JIANGYIN RONGXIN PLASTICIZING CO LTD

Patent Information

Application Number
CN202411246638.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-26
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

Existing water-based car body paints are insufficient in terms of abrasion resistance, weather resistance, and corrosion resistance, and are prone to problems such as wear, fading, and blistering, especially when used in harsh environments.

Method used

By using weather-resistant acrylic copolymer, modified talc, and perfluorooctyltriethoxysilane as components, and through optimized formulation design and process flow, a car body paint with high cross-linking density is formed and a waterproof silicone film is formed on the surface, enhancing adhesion and weather resistance.

Benefits of technology

It significantly improves the wear resistance, weather resistance and corrosion resistance of the car body paint, enhances adhesion and hardness, and strengthens waterproof performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses weather-resistant water-based vehicle body paint and a preparation method thereof, and relates to the technical field of paint. The weather-resistant water-based vehicle body paint is prepared from the following raw material components in parts by weight: 100 parts by mass of a component A, 10 to 13 parts by mass of a component B and 6 to 12 parts by mass of a component C, the component A is prepared from the following components in parts by mass: 15 to 20 parts of water, 35 to 40 parts of weather-resistant acrylic acid copolymer, 1.4 to 1.6 parts of dispersing agent, 0.08 to 0.1 part of defoaming agent, 9 to 11 parts of antirust pigment, 1 to 3 parts of carbon black powder, 7 to 9 parts of 800-mesh sericite powder, 11 to 13 parts of modified talcum powder, 0.15 to 0.2 part of wetting agent, 1.5 to 2 parts of catalyst, 0.3 to 0.35 part of thickening agent and 3 to 3.5 parts of cosolvent ethylene glycol monobutyl ether; the component B is prepared from the following components in parts by weight: 95 to 98 parts of waterborne epoxy emulsion, 2 to 2.5 parts of coalescing agent dipropylene glycol butyl ether, 2 to 5 parts of water and 0.3 part of ammonium persulfate; and the component C comprises the following components in parts by weight: 4-8 parts of fluorosiloxane and 2-4 parts of water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to a weather-resistant water-based vehicle body paint and a preparation method thereof. Background Art

[0002] With the development of the automobile industry and the increasing demand of consumers for automobile quality, body paint needs to have not only good aesthetics and decorative properties, but also excellent durability. The quality of body paint directly affects the appearance retention time, durability and service life of the vehicle. Therefore, the development of high-performance body paint, especially body paint with excellent wear resistance, weather resistance, corrosion resistance and adhesion performance, has become one of the important research directions of the automobile manufacturing industry.

[0003] At present, the body paints commonly used in the market mainly include two categories: solvent-based and water-based. Among them, although solvent-based body paints have good coating performance, they contain a large amount of organic solvents, which not only pollutes the environment but is also harmful to human health. In contrast, water-based body paints have attracted more and more attention and favor due to their low VOC (volatile organic compound) emissions, easy cleaning, and environmental protection. However, the existing water-based body paints still have shortcomings in terms of wear resistance, weather resistance, and corrosion resistance. In particular, when the vehicle is used for a long time in a harsh environment, the paint surface is prone to wear, fading, blistering, and other problems.

[0004] In order to overcome the above problems, researchers have been exploring how to improve the formulation and preparation process of water-based body paint to enhance its overall performance. This involves selecting suitable raw materials such as film-forming substances, pigments, fillers, additives, and optimizing the proportions and preparation conditions of each component. For example, by introducing polymers, nanomaterials or other functional additives with special functions, the wear resistance, weather resistance and corrosion resistance of body paint can be significantly improved. In addition, improving the adhesion between the substrate and the coating is also one of the key factors to improve the overall performance of body paint.

[0005] In view of this, the present invention aims to provide a new type of weather-resistant water-based body paint and a preparation method thereof, and to achieve comprehensive improvement in the wear resistance, weather resistance, corrosion resistance and adhesion of the body paint by optimizing the formula design and process flow, thereby meeting the demand of the modern automobile industry for high-quality body paint. Summary of the invention

[0006] The object of the present invention is to provide a weather-resistant water-based vehicle body paint and a preparation method thereof, so as to solve the problems existing in the prior art.

[0007] In order to solve the above technical problems, the present invention provides the following technical solutions: a weather-resistant water-based car body paint, wherein the raw material components include 100 parts by weight of component A, 10 to 13 parts by weight of component B, and 6 to 12 parts by weight of component C; component A includes, by weight, 15 to 20 parts by weight of water, 35 to 40 parts by weight of weather-resistant acrylic copolymer, 1.4 to 1.6 parts by weight of dispersant, 0.08 to 0.1 parts by weight of defoamer, 9 to 11 parts by weight of anti-rust pigment, 1 to 3 parts by weight of carbon black powder, and 7 to 9 parts by weight of 8 00 mesh sericite powder, 11-13 parts by weight of modified talc, 0.15-0.2 parts by weight of wetting agent, 1.5-2 parts by weight of catalyst, 0.3-0.35 parts by weight of thickener, 3-3.5 parts by weight of co-solvent ethylene glycol monobutyl ether; component B includes, by weight: 95-98 parts by weight of aqueous epoxy emulsion, 2-2.5 parts by weight of film-forming aid dipropylene glycol butyl ether, 2-5 parts by weight of water, and 0.3 parts by weight of ammonium persulfate; component C includes, by weight, 4-8 parts by weight of fluorosilicone and 2-4 parts by weight of water.

[0008] Furthermore, the weather-resistant acrylic copolymer is obtained by copolymerizing acrylic acid, N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine-modified 2-chloro-4,6-diallyl triazine, methyl methacrylate, and hydroxyethyl acrylate.

[0009] Furthermore, the modified talc powder is allylglycine intercalated calcium aluminum hydrotalcite.

[0010] Furthermore, the D50 of the modified talc is 2-6 μm.

[0011] The present invention also provides a method for preparing a weather-resistant water-based vehicle body paint, comprising the following preparation steps: (1) Mixing the raw materials according to the raw material components and proportions of claim 1; (2) 15-20 parts by weight of water, 35-40 parts by weight of weather-resistant acrylic copolymer, 1.4-1.6 parts by weight of dispersant, 0.08-0.1 parts by weight of defoamer, 9-11 parts by weight of anti-rust pigment, 1-3 parts by weight of carbon black powder, 7-9 parts by weight of 800-mesh sericite powder, 11-13 parts by weight of modified talc powder, 0.15-0.2 parts by weight of wetting agent, 1.5-2 parts by weight of catalyst, 0.3-0.35 parts by weight of thickener, and 3-3.5 parts by weight of co-solvent ethylene glycol monobutyl ether were poured into a ball mill and dispersed for 6 hours, discharged, and sealed for standby use to obtain component A; (3) 95-98 parts by weight of aqueous epoxy emulsion, 2-2.5 parts by weight of film-forming aid dipropylene glycol butyl ether, 2-5 parts by weight of water, and 0.3 parts by weight of ammonium persulfate were mixed and stirred at 100-200 rpm for 2-4 hours, discharged, sealed and set aside to obtain component B; (4) Mix 4 to 8 parts by mass of fluorosilicone and 2 to 4 parts by mass of water, discharge the mixture, seal it and set it aside to obtain component C; (5) 100 parts by mass of component A, 10 to 13 parts by mass of component B, and 6 to 12 parts by mass of component C are packaged separately and combined into a group to obtain a weather-resistant water-based vehicle body paint.

[0012] Furthermore, the preparation method of the weather-resistant acrylic copolymer is as follows: 0.5 parts by mass of acrylic acid, 2 to 6 parts by mass of N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine-modified 2-chloro-4,6-diallyl triazine, 14 parts by mass of methyl methacrylate, 18 parts by mass of hydroxyethyl acrylate, 0.3 parts by mass of initiator benzoyl peroxide, 10 parts by mass of dipropylene glycol butyl ether, and 0.26 parts by mass of chain transfer agent mercaptoethanol are mixed to obtain a monomer mixture; under nitrogen protection, 1 / 3 of the monomer mixture is heated to 80° C. for copolymerization for 1 hour, and then the remaining 2 / 3 of the monomer mixture is added dropwise, and the addition is completed within 1.5 to 2 hours, and the reaction is continued at a temperature of 2 hours, and then the temperature is lowered to 60° C., dimethylethanolamine is added dropwise at 400 to 600 rpm to adjust the pH to 8 to 9, and then distilled water is added dropwise to adjust the solid content to 40% to obtain a weather-resistant acrylic copolymer.

[0013] Furthermore, the preparation method of the N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine-modified 2-chloro-4,6-diallyl triazine is as follows: Mix 17-18 parts by mass of N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine, 17-18 parts by mass of 2-chloro-4,6-diallyltriazine and 170-172 parts by mass of m-xylene, stir at 60°C for 4 hours, slowly add 18 parts by mass of 20% sodium hydroxide solution, continue stirring and react for 3.5-4.5 hours, separate the organic phase after the reaction, wash and separate it with 10% sodium chloride solution, freeze it in a refrigerator for 12 hours, filter it, and dry it in a vacuum oven at 80°C for 12 hours.

[0014] Furthermore, the preparation steps of the modified talc are as follows: Aluminum nitrate and calcium nitrate are dissolved in water at a molar ratio of 1:2 to obtain a solution A with an aluminum nitrate content of 0.1 mol / L and a calcium nitrate content of 0.2 mol / L; allylglycine and sodium hydroxide are dissolved in water to obtain a solution B, wherein the volume of water in solution B is the same as the volume of water in solution A, the amount of allylglycine is equal to the amount of calcium nitrate, and the amount of sodium hydroxide is 2.77 times the sum of the amounts of aluminum nitrate and calcium nitrate; under nitrogen protection, solution B is added dropwise to solution A, after the addition is completed, the pH is adjusted to 8.5-9.5 with nitric acid, stirred for 12 hours, aged at 150°C for 12 hours, filtered and washed after cooling, dried in an oven at 80°C for 12 hours, and ground to obtain modified talc.

[0015] The present invention also provides an application method of weather-resistant water-based vehicle body paint, and the application steps are as follows: first, 100 parts by mass of component A and 10-13 parts by mass of component B are mixed and ball-milled for 5-7 hours to obtain a mixture, the mixture is sprayed on a polished vehicle body, placed in a drying room at 93-97°C under nitrogen protection for 50-70 minutes, then taken out, and 6-12 parts by mass of component C are continuously sprayed, and the mixture is continuously placed in a drying room at 113-117°C for 10-14 hours and taken out.

[0016] Compared with the prior art, the beneficial effects achieved by the present invention are: The weather-resistant water-based vehicle body paint of the present invention comprises, by weight, 100 parts by weight of component A, 10 to 13 parts by weight of component B, and 6 to 12 parts by weight of component C; the component A comprises, by weight, 15 to 20 parts by weight of water, 35 to 40 parts by weight of weather-resistant acrylic copolymer, 1.4 to 1.6 parts by weight of dispersant, 0.08 to 0.1 parts by weight of defoamer, 9 to 11 parts by weight of rust-proof pigment, 1 to 3 parts by weight of carbon black powder, 7 to 9 parts by weight of 800-mesh sericite powder, 11 to 13 parts by weight of modified talc powder, 0.15 to 0.2 parts by weight of wetting agent, 1.5 to 2 parts by weight of catalyst, 0.3 to 0.35 parts by weight of thickener, 3 to 3 .5 parts by weight of co-solvent ethylene glycol monobutyl ether; component B includes, by weight: 95-98 parts by weight of aqueous epoxy emulsion, 2-2.5 parts by weight of film-forming aid dipropylene glycol butyl ether, 2-5 parts by weight of water, and 0.3 parts by weight of ammonium persulfate; component C includes, by weight, 4-8 parts by weight of perfluorooctyltriethoxysilane and 2-4 parts by weight of water; the weather-resistant acrylic copolymer is obtained by copolymerization of acrylic acid, N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine-modified 2-chloro-4,6-diallyl triazine, methyl methacrylate, and hydroxyethyl acrylate; the modified talc is allylglycine intercalated calcium aluminum hydrotalcite.

[0017] The present invention adopts the weather-resistant acrylic copolymer in component A and the water-based epoxy emulsion in component B as the base resin, introduces a large number of polar groups such as hydroxyl and carboxyl into the weather-resistant water-based vehicle body paint, so that the weather-resistant water-based vehicle body paint can be better adhered to the polished vehicle body, thereby enhancing the adhesion performance of the weather-resistant water-based vehicle body paint.

[0018] The invention obtains a weather-resistant acrylic copolymer with a hyperbranched structure by copolymerizing acrylic acid, N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine-modified 2-chloro-4,6-diallyl triazine, methyl methacrylate and hydroxyethyl acrylate. An anti-aging agent hindered amine and a triazine ring are introduced into the weather-resistant acrylic copolymer, which can effectively improve the incompatibility between the anti-aging agent hindered amine and a base resin, thereby improving the heat resistance and rigidity of the weather-resistant acrylic copolymer, making the weather-resistant acrylic copolymer have weather resistance, and increasing the crosslinking degree of the weather-resistant acrylic copolymer, thereby enhancing the mechanical properties and wear resistance of the weather-resistant acrylic copolymer.

[0019] The invention prepares component A by mixing water, weather-resistant acrylic copolymer, dispersant, defoamer, rust-proof pigment, carbon black powder, 800-mesh sericite powder, modified talcum powder, wetting agent, catalyst, thickener and cosolvent ethylene glycol monobutyl ether; allyl glycine is introduced into the modified talcum powder so that the modified talcum powder is uniformly dispersed in component A; more cavities exist in the weather-resistant acrylic copolymer with a hyperbranched structure; the modified talcum powder is embedded in the cavities after being mixed into component A, so that the modified talcum powder is further uniformly dispersed in component A, thereby ensuring the mechanical properties of the weather-resistant water-based vehicle body paint.

[0020] When the present invention is used, component A and component B are mixed, and then placed in an oven at 93-97°C for 50-70 minutes, and the modified talcum powder and the weather-resistant acrylic copolymer are polymerized through unsaturated bonds under the action of an initiator, and the weather-resistant acrylic copolymer and water-based epoxy emulsion in components A and B are mixed, and the epoxy polymer molecular chains in the water-based epoxy emulsion penetrate into the cavity of the weather-resistant acrylic copolymer, and the talcum powder is evenly dispersed in the weather-resistant water-based vehicle body paint, and after curing, a high cross-linking density vehicle body paint is formed, and at the same time, a dense and uniform hydrotalcite film layer is formed, thereby enhancing the weather-resistant water-based vehicle body paint. The corrosion resistance and hardness of the weather-resistant water-based car body paint are improved; however, the introduction of components A and B introduces more hydrophilic groups such as hydroxyl, amino, and carboxyl into the weather-resistant water-based car body paint, which easily leads to poor water resistance of the car paint. When in use, after spraying the mixture of components A and B, component C prepared by perfluorooctyl triethoxy silane is sprayed. Perfluorooctyl triethoxy silane reacts with the hydrophilic groups on the paint surface formed by spraying the mixture of components A and B and self-polymerizes to form a waterproof silicon film on the surface of the weather-resistant water-based car body paint, thereby enhancing the wear resistance, weather resistance, and water resistance of the weather-resistant water-based car body paint. DETAILED DESCRIPTION

[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0022] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the weather-resistant water-based vehicle body paint prepared in the following examples are as follows: Use 80-mesh sandpaper to grind a cold-rolled steel plate with a size of 120 mm×50 mm×0.5 mm, clean it with alcohol, first mix component A and component 1B prepared in each embodiment and comparative example and ball-mill for 6 hours to obtain a mixture, spray the mixture on the grinded cold-rolled steel plate, put it in a drying room at 95°C under nitrogen protection for 60 minutes, then take it out, continue to spray component C prepared in each embodiment and comparative example, continue to put it in a drying room at 115°C for 12 hours, take it out, and obtain a painted cold-rolled steel plate.

[0023] Adhesion test: Test the adhesion of the paint film according to standard GB / T 9286-1998; place the painted cold-rolled steel plate at room temperature for one week and then test it; use a paint film grid to draw a uniform grid on the paint film; then use transparent tape to stick to the grid and press it tightly to ensure that there are no bubbles, then quickly tear off the tape, observe the damage results of the grid, and compare it with the standard to determine the adhesion of the paint film; repeat the test three times to ensure experimental error.

[0024] Hardness test: Test the hardness of the paint film according to standard GB / T 6739-2022; place the painted cold-rolled steel plate at room temperature for one week and then test it; put a pencil into the trolley pencil hardness tester, push the trolley pencil hardness tester to make the pencil draw a line larger than 7mm on the surface of the paint film, test in order from high to low hardness, observe the damage of the paint film, repeat the experiment five times, and record the maximum hardness without exposing the bottom as the paint film hardness.

[0025] Corrosion resistance: The neutral salt spray resistance of the paint film was tested according to the standard GB / T 1771-2007; the painted cold-rolled steel plate was placed at room temperature for one week and then tested; the steel plate was sealed with plastic tape before the test, and then the sample was placed in a salt spray chamber, and the corrosion degree of the sample was observed every 12 hours and returned to its original position after observation.

[0026] Water resistance: Use 3M tape to seal the edges of the painted cold-rolled steel plate, then soak about 2 / 3 of the steel plate in deionized water to observe whether there is bubbling, peeling or shedding on the surface of the paint film.

[0027] Flexibility: Test the flexibility of the paint film according to standard GB / T 6742-2007; place the painted cold-rolled steel plate at room temperature for one week and then test it; place the test plate with the paint film facing up, close to a fixed shaft rod, then bend it around the shaft rod, and then observe the damage of the paint film, record the minimum diameter of the shaft rod that does not cause paint film damage, and repeat the experiment three times.

[0028] Aging resistance: The painted cold-rolled steel sheets were placed at room temperature for one week and tested according to ASTM G154-2006. Cycle 2 was used and 313 nm lamps were used to irradiate the five groups of paint samples with ultraviolet light for 4 hours. The irradiation intensity was 0.71 W / (m 2 ·nm), blackboard temperature (60±3)℃ and 4h condensation, blackboard temperature (50±3)℃ are continuously alternating. The test cycle is 800h, and the 45° color of the sample is tested every 100h, and the color difference after 800h UV aging is tested.

[0029] Some of the raw materials used in the examples and comparative examples of the present invention are as follows: The dispersant used is Tego 760W from Evonik Degussa; The defoamer is Tego 810 produced by Evonik Degussa; The anti-rust pigment is SZP-391 from HALOX of the United States; The carbon black powder is MA-100 produced by Mitsubishi Chemical; The sericite powder is 800 mesh sericite powder from Chuzhou Baota Sericite Mining Co., Ltd. The wetting agent is Tego Win 4000 produced by Evonik Degussa; The catalyst is triphenylphosphine; The thickener is XS 71 from Gaotai Chemical; The water-based epoxy emulsion adopts WE-319 produced by Jili Water-based New Material Technology (Zhuhai) Co., Ltd., and the epoxy equivalent is 1250-1500. Example

[0030] A method for preparing a weather-resistant water-based vehicle body paint comprises the following preparation steps: (1) 15 parts by weight of water, 35 parts by weight of weather-resistant acrylic copolymer, 1.4 parts by weight of dispersant, 0.08 parts by weight of defoamer, 9 parts by weight of anti-rust pigment, 1 part by weight of carbon black powder, 7 parts by weight of 800-mesh sericite powder, 11 parts by weight of modified talc, 0.15 parts by weight of wetting agent, 1.5 parts by weight of catalyst, 0.3 parts by weight of thickener, and 3 parts by weight of co-solvent ethylene glycol monobutyl ether were poured into a ball mill and dispersed for 6 hours, discharged, and sealed for standby use to obtain component A; (2) 95 parts by weight of aqueous epoxy emulsion, 2 parts by weight of film-forming aid dipropylene glycol butyl ether, 2 parts by weight of water, and 0.3 parts by weight of ammonium persulfate were mixed and stirred at 100 rpm for 2 h, discharged, and sealed for standby use to obtain component B; (3) 4 parts by mass of perfluorooctyltriethoxysilane and 2 parts by mass of water are mixed, discharged, sealed and set aside to obtain component C; (4) 100 parts by mass of component A, 10 parts by mass of component B, and 6 parts by mass of component C are packaged separately and combined into a group to obtain a weather-resistant water-based vehicle body paint.

[0031] Furthermore, the preparation method of the weather-resistant acrylic copolymer is as follows: 0.5 parts by mass of acrylic acid, 2 parts by mass of N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine-modified 2-chloro-4,6-diallyl triazine, 14 parts by mass of methyl methacrylate, 18 parts by mass of hydroxyethyl acrylate, 0.3 parts by mass of initiator benzoyl peroxide, 10 parts by mass of dipropylene glycol butyl ether, and 0.26 parts by mass of chain transfer agent mercaptoethanol are mixed to obtain a monomer mixture; under nitrogen protection, 1 / 3 of the monomer mixture is heated to 80° C. for copolymerization for 1 hour, and then the remaining 2 / 3 of the monomer mixture is added dropwise, and the addition is completed within 1.5 hours, and the reaction is continued at a temperature of 2 hours, and then the temperature is lowered to 60° C., dimethylethanolamine is added dropwise at 400 rpm to adjust the pH to 8, and then distilled water is added dropwise to adjust the solid content to 40% to obtain a weather-resistant acrylic copolymer.

[0032] Furthermore, the preparation method of the N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine-modified 2-chloro-4,6-diallyl triazine is as follows: 17 parts by mass of N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine, 17 parts by mass of 2-chloro-4,6-diallyltriazine and 170 parts by mass of m-xylene were mixed, stirred at 60°C for 4 hours, 18 parts by mass of 20% sodium hydroxide solution were slowly added dropwise, and the stirring reaction was continued for 3.5 hours. After the reaction was completed, the organic phase was separated and then washed and separated with 10% sodium chloride solution, then frozen in a refrigerator for 12 hours, filtered, and dried in a vacuum oven at 80°C for 12 hours.

[0033] Furthermore, the preparation steps of the modified talc are as follows: Aluminum nitrate and calcium nitrate are dissolved in water at a molar ratio of 1:2 to obtain a solution A with an aluminum nitrate content of 0.1 mol / L and a calcium nitrate content of 0.2 mol / L; allyl glycine and sodium hydroxide are dissolved in water to obtain a solution B, wherein the volume of water in solution B is the same as the volume of water in solution A, the amount of allyl glycine is equal to the amount of calcium nitrate, and the amount of sodium hydroxide is 2.77 times the sum of the amounts of aluminum nitrate and calcium nitrate; under nitrogen protection, solution B is added dropwise to solution A, after the addition is completed, the pH is adjusted to 8.5 with nitric acid, the solution is stirred for 12 hours, aged at 150°C for 12 hours, filtered and washed after cooling, dried in an oven at 80°C for 12 hours, and ground to obtain a modified talc powder with a D50 of 2 μm. Example

[0034] A method for preparing a weather-resistant water-based vehicle body paint comprises the following preparation steps: (1) 18 parts by weight of water, 38 parts by weight of weather-resistant acrylic copolymer, 1.5 parts by weight of dispersant, 0.09 parts by weight of defoamer, 10 parts by weight of anti-rust pigment, 2 parts by weight of carbon black powder, 8 parts by weight of 800-mesh sericite powder, 12 parts by weight of modified talc, 0.18 parts by weight of wetting agent, 1.8 parts by weight of catalyst, 0.33 parts by weight of thickener, and 3.3 parts by weight of co-solvent ethylene glycol monobutyl ether were poured into a ball mill and dispersed for 6 hours, discharged, and sealed for standby use to obtain component A; (2) 97 parts by weight of aqueous epoxy emulsion, 2.3 parts by weight of film-forming aid dipropylene glycol butyl ether, 3 parts by weight of water, and 0.3 parts by weight of ammonium persulfate were mixed and stirred at 150 rpm for 3 hours, discharged, and sealed for standby use to obtain component B; (3) 6 parts by mass of perfluorooctyltriethoxysilane and 3 parts by mass of water are mixed, discharged, sealed and set aside to obtain component C; (4) 100 parts by mass of component A, 12 parts by mass of component B, and 9 parts by mass of component C are packaged separately and combined into a group to obtain a weather-resistant water-based vehicle body paint.

[0035] Furthermore, the preparation method of the weather-resistant acrylic copolymer is as follows: 0.5 parts by mass of acrylic acid, 4 parts by mass of N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine-modified 2-chloro-4,6-diallyl triazine, 14 parts by mass of methyl methacrylate, 18 parts by mass of hydroxyethyl acrylate, 0.3 parts by mass of initiator benzoyl peroxide, 10 parts by mass of dipropylene glycol butyl ether, and 0.26 parts by mass of chain transfer agent mercaptoethanol are mixed to obtain a monomer mixture; under nitrogen protection, 1 / 3 of the monomer mixture is heated to 80° C. for copolymerization for 1 hour, and then the remaining 2 / 3 of the monomer mixture is added dropwise, and the addition is completed within 1.8 hours, and the reaction is continued at a temperature of 2 hours, and then the temperature is lowered to 60° C., dimethylethanolamine is added dropwise at 500 rpm to adjust the pH to 8.5, and then distilled water is added dropwise to adjust the solid content to 40% to obtain a weather-resistant acrylic copolymer.

[0036] Furthermore, the preparation method of the N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine-modified 2-chloro-4,6-diallyl triazine is as follows: 17.5 parts by mass of N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine, 17.5 parts by mass of 2-chloro-4,6-diallyltriazine and 171 parts by mass of m-xylene were mixed, stirred at 60°C for 4 hours, 18 parts by mass of 20% sodium hydroxide solution were slowly added dropwise, and the stirring reaction was continued for 4 hours. After the reaction was completed, the organic phase was separated and then washed and separated with 10% sodium chloride solution, and then frozen in a refrigerator for 12 hours, filtered, and dried in a vacuum oven at 80°C for 12 hours.

[0037] Furthermore, the preparation steps of the modified talc are as follows: Aluminum nitrate and calcium nitrate are dissolved in water at a molar ratio of 1:2 to obtain a solution A with an aluminum nitrate content of 0.1 mol / L and a calcium nitrate content of 0.2 mol / L; allyl glycine and sodium hydroxide are dissolved in water to obtain a solution B, wherein the volume of water in solution B is the same as the volume of water in solution A, the amount of allyl glycine is equal to the amount of calcium nitrate, and the amount of sodium hydroxide is 2.77 times the sum of the amounts of aluminum nitrate and calcium nitrate; under nitrogen protection, solution B is added dropwise to solution A, after the addition is completed, the pH is adjusted to 9 with nitric acid, and the solution is stirred for 12 hours and aged at 150°C for 12 hours, filtered and washed after cooling, dried in an oven at 80°C for 12 hours, and ground to obtain a modified talc powder with a D50 of 4 μm. Example

[0038] A method for preparing a weather-resistant water-based vehicle body paint comprises the following preparation steps: (1) 20 parts by weight of water, 40 parts by weight of weather-resistant acrylic copolymer, 1.6 parts by weight of dispersant, 0.1 parts by weight of defoamer, 11 parts by weight of anti-rust pigment, 3 parts by weight of carbon black powder, 9 parts by weight of 800-mesh sericite powder, 13 parts by weight of modified talc, 0.2 parts by weight of wetting agent, 2 parts by weight of catalyst, 0.35 parts by weight of thickener, and 3.5 parts by weight of co-solvent ethylene glycol monobutyl ether were poured into a ball mill and dispersed for 6 hours, discharged, and sealed for standby use to obtain component A; (2) 98 parts by weight of aqueous epoxy emulsion, 2.5 parts by weight of film-forming aid dipropylene glycol butyl ether, 5 parts by weight of water, and 0.3 parts by weight of ammonium persulfate were mixed and stirred at 200 rpm for 4 hours, discharged, and sealed for standby use to obtain component B; (3) 8 parts by mass of perfluorooctyltriethoxysilane and 4 parts by mass of water are mixed, discharged, sealed and set aside to obtain component C; (4) 100 parts by mass of component A, 13 parts by mass of component B, and 12 parts by mass of component C are packaged separately and combined into a group to obtain a weather-resistant water-based vehicle body paint.

[0039] Furthermore, the preparation method of the weather-resistant acrylic copolymer is as follows: 0.5 parts by mass of acrylic acid, 6 parts by mass of N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine-modified 2-chloro-4,6-diallyl triazine, 14 parts by mass of methyl methacrylate, 18 parts by mass of hydroxyethyl acrylate, 0.3 parts by mass of initiator benzoyl peroxide, 10 parts by mass of dipropylene glycol butyl ether, and 0.26 parts by mass of chain transfer agent mercaptoethanol are mixed to obtain a monomer mixture; under nitrogen protection, 1 / 3 of the monomer mixture is heated to 80° C. for copolymerization for 1 hour, and then the remaining 2 / 3 of the monomer mixture is added dropwise, and the addition is completed within 2 hours, and the reaction is continued at a temperature of 2 hours, and then the temperature is lowered to 60° C., dimethylethanolamine is added dropwise at 600 rpm to adjust the pH to 9, and then distilled water is added dropwise to adjust the solid content to 40% to obtain a weather-resistant acrylic copolymer.

[0040] Furthermore, the preparation method of the N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine-modified 2-chloro-4,6-diallyl triazine is as follows: 18 parts by mass of N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine, 18 parts by mass of 2-chloro-4,6-diallyltriazine and 172 parts by mass of m-xylene were mixed, stirred at 60°C for 4 hours, 18 parts by mass of 20% sodium hydroxide solution were slowly added dropwise, and the stirring reaction was continued for 4.5 hours. After the reaction was completed, the organic phase was separated and then washed and separated with 10% sodium chloride solution, then frozen in a refrigerator for 12 hours, filtered, and dried in a vacuum oven at 80°C for 12 hours.

[0041] Furthermore, the preparation steps of the modified talc are as follows: Aluminum nitrate and calcium nitrate are dissolved in water at a molar ratio of 1:2 to obtain a solution A with an aluminum nitrate content of 0.1 mol / L and a calcium nitrate content of 0.2 mol / L; allyl glycine and sodium hydroxide are dissolved in water to obtain a solution B, wherein the volume of water in solution B is the same as the volume of water in solution A, the amount of allyl glycine is equal to the amount of calcium nitrate, and the amount of sodium hydroxide is 2.77 times the sum of the amounts of aluminum nitrate and calcium nitrate; under nitrogen protection, solution B is added dropwise to solution A, after the addition is completed, the pH is adjusted to 9.5 with nitric acid, the solution is stirred for 12 hours, aged at 150°C for 12 hours, filtered and washed after cooling, dried in an oven at 80°C for 12 hours, and ground to obtain a modified talc powder with a D50 of 6 μm.

[0042] Comparative Example 1 The only difference between Comparative Example 1 and Example 2 is that the weather-resistant acrylic copolymer is obtained by copolymerizing only acrylic acid, methyl methacrylate, and hydroxyethyl acrylate, and 0.5 parts by mass of an antioxidant N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine is added to component A; the remaining components, proportions, and processes are the same as those in Example 2.

[0043] Comparative Example 2 The difference between Comparative Example 2 and Example 2 is that component A is prepared by mixing water, weather-resistant acrylic copolymer, dispersant, defoamer, rust-proof pigment, carbon black powder, 800 mesh sericite powder, talcum powder, wetting agent, catalyst, thickener, and co-solvent ethylene glycol monobutyl ether; the remaining components, proportions, and processes are the same as those in Example 2.

[0044] Comparative Example 3 The difference between Comparative Example 3 and Example 2 is that component A is prepared by mixing water, weather-resistant acrylic copolymer, dispersant, defoamer, anti-rust pigment, carbon black powder, 800 mesh sericite powder, 3000 mesh precipitated barium sulfate, wetting agent, catalyst, thickener, and co-solvent ethylene glycol monobutyl ether; the remaining components, proportions and processes are the same as those in Example 2.

[0045] Comparative Example 4 The only difference between Comparative Example 4 and Example 2 is that the weather-resistant water-based vehicle body paint only includes component A and component B; the remaining components, proportions and processes are the same as those of Example 2.

[0046] Effect example Table 1 below shows the performance analysis results of the weather-resistant water-based vehicle body paints of Examples 1 to 3 of the present invention and Comparative Examples 1 to 4.

[0047] Table 1 Adhesion / Grade Pencil hardness Flexibility / mm Neutral salt spray resistance Water resistance Weather resistance - color difference Example 1 0 3H 2 340h no rust 360h paint film without bubbles and rust 5.93 Example 2 0 3H 2 340h no rust 360h paint film without bubbles and rust 5.86 Example 3 0 3H 2 340h no rust 360h paint film without bubbles and rust 5.92 Comparative Example 1 0 2H 4 280h rust 360h paint film without bubbles and rust 8.64 Comparative Example 2 0 2H 6 260h rust 300h foaming 5.90 Comparative Example 3 0 H 4 290h rust 320h paint film blistering 5.93 Comparative Example 4 0 H 2 240h ​​rust 160h foaming 5.88 From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 1, it can be found that the weather-resistant water-based car body paint film prepared in the examples has good mechanical properties, adhesion properties, corrosion resistance, water resistance, and high coating hardness; from the comparison of the experimental data of Example 2 and Comparative Example 1, it can be found that the weather-resistant acrylic copolymer obtained by copolymerizing acrylic acid, N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine modified 2-chloro-4,6-diallyl triazine, methyl methacrylate, and hydroxyethyl acrylate is used to prepare the weather-resistant water-based car body paint film. The body paint, the weather-resistant water-based body paint film has high mechanical properties, corrosion resistance and coating hardness; from the comparison of the experimental data of Example 2 and Comparative Examples 2~3, it can be found that the weather-resistant water-based body paint is prepared by using allylglycine intercalated calcium aluminum hydrotalcite, and the prepared weather-resistant water-based body paint film has good mechanical properties, corrosion resistance and water resistance, and the coating hardness is high; from the comparison of the experimental data of Example 2 and Comparative Example 4, it can be found that the weather-resistant water-based body paint is also provided with a C component, and the prepared weather-resistant water-based body paint film has good corrosion resistance and water resistance, and the coating hardness is high.

[0048] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A weather-resistant water-based car body paint, It is characterized in that The raw material components include 100 parts by weight of component A, 10-13 parts by weight of component B, and 6-12 parts by weight of component C; component A includes: 15-20 parts by weight of water, 35-40 parts by weight of weather-resistant acrylic copolymer, 1.4-1.6 parts by weight of dispersant, 0.08-0.1 parts by weight of defoamer, 9-11 parts by weight of rust-proof pigment, 1-3 parts by weight of carbon black powder, 7-9 parts by weight of 800-mesh sericite powder, and 11-13 parts by weight of modified talcum powder, 0.15-0.2 parts by weight of wetting agent, 1.5-2 parts by weight of catalyst, 0.3-0.35 parts by weight of thickener, 3-3.5 parts by weight of co-solvent ethylene glycol monobutyl ether; component B includes, by weight: 95-98 parts by weight of aqueous epoxy emulsion, 2-2.5 parts by weight of film-forming aid dipropylene glycol butyl ether, 2-5 parts by weight of water, 0.3 parts by weight of ammonium persulfate; component C includes, by weight: 4-8 parts by weight of fluorosilicone and 2-4 parts by weight of water.

2. The weather-resistant water-based vehicle body paint according to claim 1, It is characterized in that The weather-resistant acrylic copolymer is obtained by copolymerizing acrylic acid, N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine-modified 2-chloro-4,6-diallyl triazine, methyl methacrylate and hydroxyethyl acrylate.

3. The weather-resistant water-based vehicle body paint according to claim 1, It is characterized in that The modified talc powder is allylglycine intercalated calcium aluminum hydrotalcite.

4. The weather-resistant water-based vehicle body paint according to claim 1, It is characterized in that The D50 of the modified talc is 2-6 μm.

5. A method for preparing a weather-resistant water-based vehicle body paint, It is characterized in that The method comprises the following preparation steps: (1) Mixing the raw materials according to the raw material components and proportions of claim 1; (2) 15-20 parts by weight of water, 35-40 parts by weight of weather-resistant acrylic copolymer, 1.4-1.6 parts by weight of dispersant, 0.08-0.1 parts by weight of defoamer, 9-11 parts by weight of anti-rust pigment, 1-3 parts by weight of carbon black powder, 7-9 parts by weight of 800-mesh sericite powder, 11-13 parts by weight of modified talc powder, 0.15-0.2 parts by weight of wetting agent, 1.5-2 parts by weight of catalyst, 0.3-0.35 parts by weight of thickener, and 3-3.5 parts by weight of co-solvent ethylene glycol monobutyl ether were poured into a ball mill and dispersed for 6 hours, discharged, and sealed for standby use to obtain component A; (3) 95-98 parts by weight of aqueous epoxy emulsion, 2-2.5 parts by weight of film-forming aid dipropylene glycol butyl ether, 2-5 parts by weight of water, and 0.3 parts by weight of ammonium persulfate were mixed and stirred at 100-200 rpm for 2-4 hours, discharged, sealed and set aside to obtain component B; (4) Mix 4 to 8 parts by mass of fluorosilicone and 2 to 4 parts by mass of water, discharge the mixture, seal it and set it aside to obtain component C; (5) 100 parts by mass of component A, 10 to 13 parts by mass of component B, and 6 to 12 parts by mass of component C are packaged separately and combined into a group to obtain a weather-resistant water-based vehicle body paint.

6. The method for preparing the weather-resistant water-based vehicle body paint according to claim 5, It is characterized in that The preparation method of the weather-resistant acrylic copolymer is as follows: 0.5 parts by mass of acrylic acid, 2-6 parts by mass of N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine-modified 2-chloro-4,6-diallyl triazine, 14 parts by mass of methyl methacrylate, 18 parts by mass of hydroxyethyl acrylate, 0.3 parts by mass of initiator benzoyl peroxide, 10 parts by mass of dipropylene glycol butyl ether, and 0.26 parts by mass of chain transfer agent mercaptoethanol are mixed to obtain a monomer mixture; under nitrogen protection, 1 / 3 of the monomer mixture is heated to 80° C. for copolymerization for 1 hour, and then the remaining 2 / 3 of the monomer mixture is dripped, and the dripping is completed within 1.5-2 hours, and the heat preservation reaction is continued for 2 hours, and then the temperature is lowered to 60° C., dimethylethanolamine is dripped at 400-600 rpm to adjust the pH to 8-9, and then distilled water is dripped to adjust the solid content to 40%, so as to obtain a weather-resistant acrylic copolymer.

7. The method for preparing the weather-resistant water-based vehicle body paint according to claim 6, It is characterized in that The preparation method of the N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine modified 2-chloro-4,6-diallyl triazine is as follows: Mix 17-18 parts by mass of N,N-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine, 17-18 parts by mass of 2-chloro-4,6-diallyltriazine and 170-172 parts by mass of m-xylene, stir at 60°C for 4 hours, slowly add 18 parts by mass of 20% sodium hydroxide solution, continue stirring and react for 3.5-4.5 hours, separate the organic phase after the reaction, wash and separate it with 10% sodium chloride solution, freeze it in a refrigerator for 12 hours, filter it, and dry it in a vacuum oven at 80°C for 12 hours.

8. The method for preparing the weather-resistant water-based vehicle body paint according to claim 5, It is characterized in that The preparation steps of the modified talcum powder are as follows: Aluminum nitrate and calcium nitrate are dissolved in water at a molar ratio of 1:2 to obtain a solution A with an aluminum nitrate content of 0.1 mol / L and a calcium nitrate content of 0.2 mol / L; allylglycine and sodium hydroxide are dissolved in water to obtain a solution B, wherein the volume of water in solution B is the same as the volume of water in solution A, the amount of allylglycine is equal to the amount of calcium nitrate, and the amount of sodium hydroxide is 2.77 times the sum of the amounts of aluminum nitrate and calcium nitrate; under nitrogen protection, solution B is added dropwise to solution A, after the addition is completed, the pH is adjusted to 8.5-9.5 with nitric acid, stirred for 12 hours, aged at 150°C for 12 hours, filtered and washed after cooling, dried in an oven at 80°C for 12 hours, and ground to obtain modified talc.

9. A method for applying the weather-resistant water-based vehicle body paint according to any one of claims 1 to 4, It is characterized in that The application steps are as follows: first, 100 parts by mass of component A and 10-13 parts by mass of component B are mixed and ball-milled for 5-7 hours to obtain a mixture, the mixture is sprayed on the polished car body, placed in a drying room at 93-97°C under nitrogen protection for 50-70 minutes, then taken out, and 6-12 parts by mass of component C are continuously sprayed, and the mixture is continuously placed in a drying room at 113-117°C for 10-14 hours and taken out.

Citation Information

Patent Citations

  • Preparation method of waterborne primer, intermediate coat and finishing coat for railway bearing system

    CN104140738A

  • Quick-drying type water-borne mental corrosive-resistant paint and preparation method thereof

    CN106867362A

  • Fluorosilicone polyurethane modified acrylic waterborne resin and preparation method thereof

    CN109369862A

  • Water-based anticorrosive primer and preparation method thereof

    CN111334160A

  • Preparation method of anti-ultraviolet silicon dioxide-acrylic resin composite coating

    CN115838567A

Cited By

  • Long-acting corrosion-resistant nano epoxy zinc-rich paint

    CN122356959A