Inorganic-organic composite material protection liquid for reinforcing and protecting earthen ruins

By using an inorganic-organic fluorosilicone modified acrylic resin composite protective liquid, the problems of insufficient permeability of inorganic materials and decreased light transmittance of organic materials were solved, achieving efficient reinforcement and protection of earthen sites and maintaining their original appearance.

CN119019902AActive Publication Date: 2024-11-26ZHENGZHOU UNIV

Patent Information

Application Number
CN202411286190.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-26
Estimated Expiration
2044-09-13

AI Technical Summary

Technical Problem

The existing inorganic materials have insufficient penetration depth in the reinforcement of earthen sites, which leads to repeated dissolution and crystallization of soluble salts in water glass, causing damage to cultural relics. On the other hand, organic materials have reduced light transmittance and insufficient high temperature resistance and hydrolysis resistance.

Method used

Using inexpensive fluoroalcohols as monomers, fluorinated compounds with double bonds are synthesized to modify acrylic resins. These compounds are then mixed with nano-SiO2 to prepare an inorganic-organofluorosilicone modified acrylic resin composite protective liquid. This combines the advantages of both organofluorine modified acrylic resins and organofluorosilicone modified acrylic resins, overcoming defects such as insufficient permeability and decreased light transmittance.

Benefits of technology

It improves the water resistance, acid and alkali resistance, and salt resistance of earthen sites, enhances the internal structure, has a significant reinforcement effect, good light transmission, and excellent weather resistance, and does not damage the appearance and luster of earthen sites, which is in line with the protection principle of "restoring the old as it was".

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019902A_ABST
    Figure CN119019902A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of cultural relic protection, and is formed by uniformly mixing a mixture of organic fluorine modified acrylic resin emulsion, organic fluorine-silicon modified acrylic resin emulsion and nano silicon dioxide according to the weight ratio of (1-2): (1-2): (0.08-0.16), the water-proof and moisture-proof coating integrates permeation, water resistance, moisture resistance, reinforcement protection, acid, alkali and salt resistance and aging resistance, and is good in stability, low in viscosity, high in water resistance, high in water resistance, high in water resistance, high in water resistance and high in water resistance. According to the present invention, the prepared earthen ruins have characteristics of high transparency and strong fluidity, the advantages of high transparency and good weather resistance of the acrylic resin, and good water resistance, good weather resistance, good pollution resistance and the like of the fluorine-containing and silicon-containing compound are completely combined, and the advantages of good dispersibility and ultraviolet ray absorption of the nanometer SiO2 are combined so as to provide the earthen ruins with certain moisture-proof, water-proof, acid-base-salt-resistant, weather-resistant, wear-resistant and anti-aging effects. The soil sample has good compatibility with an earthen archaeological site base material, the mechanical strength and compressive strength of earthen archaeological site cultural relics are effectively enhanced, the original appearance, glossiness and weight change of the soil sample are not obvious, and the protective film can be removed under the condition of no damage or slight damage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cultural relics protection, and in particular to an inorganic-organic fluorine-silicon modified acrylic resin composite material protection liquid for reinforcing and protecting earthen sites. Background Art

[0002] Earthen sites refer to ancient relics left over from various activities such as production and life in human history, where earth is used as the main building material. There are a large number of earthen sites in my country, which are widely distributed. However, due to the deterioration of the geographical and ecological environment, climate change, and some unscientific management, random trampling, and development, the earthen sites are facing various damages such as wind erosion, rain erosion, and biological weathering. Earthen sites are one of the precious cultural heritages of mankind. Once damaged, they are irreversible. Appropriate reinforcement and protection methods will not only not affect the appearance and color of earthen sites, but also effectively delay the aging, cracking, powdering, and weathering of earthen sites, and can also enhance the internal strength of earthen sites, and play a role in toughening, water resistance, moisture resistance, and weather resistance. Chemical material reinforcement method has always been the key and difficult point in the research of earthen site protection, and is considered to be the most important protection and reinforcement measure for the long-term preservation of earthen sites. At present, there are two main categories of materials for the reinforcement and protection of earthen sites, namely inorganic materials and organic polymer materials. Inorganic materials include nano-SiO2, sodium silicate, potassium silicate, lithium silicate, etc., and organic polymer materials include silicone resin, polyurethane resin, acrylic resin, etc. Although there are many studies on the reinforcement and protection of earthen sites in China, most of them are currently reinforced with inorganic materials. However, the penetration depth of inorganic materials often fails to meet the ideal requirements, and the soluble salts in water glass are repeatedly dissolved and crystallized in a humid environment, which will cause damage to cultural relics. Although the use of organic materials for reinforcement can obtain the ideal penetration depth and strength, it will reduce the transmittance of the soil sample, and the high temperature resistance and hydrolysis resistance are insufficient. Therefore, the development of a new type of inorganic-organic composite material for the reinforcement and protection of earthen sites is the future development direction. Summary of the invention

[0003] In view of the above situation, in order to overcome the defects of the prior art, the purpose of the present invention is to provide an inorganic-organic fluorine-silicon modified acrylic resin composite material protection liquid for the reinforcement and protection of earthen sites. The protection liquid prepared by the present invention has a great effect on improving the water resistance, acid, alkali and salt resistance of earthen sites and reinforcing the internal structure of earthen sites. In view of the shortcomings of the prior art of directly using expensive fluorine-containing acrylic acid with double bonds as a modified monomer to synthesize fluorine-containing acrylic polymers, the present invention uses low-priced fluoroalcohol as a monomer, first synthesizes fluorine-containing compounds with double bonds, and then modifies acrylic resin, which greatly reduces the cost; and the protection liquid prepared by mixing organic fluorine-modified acrylic resin and organic fluorine-silicon modified acrylic resin with nano-SiO2 can effectively overcome the defects of decreased transmittance, insufficient high temperature resistance and hydrolysis resistance caused by using organic materials alone or insufficient permeability, repeated dissolution and crystallization caused by using inorganic materials alone.

[0004] The technical solution provided by the present invention is an inorganic-organic fluorine-silicon modified acrylic resin composite material protection liquid for the reinforcement and protection of earthen ruins, and the preparation method thereof comprises the following steps:

[0005] 1) Preparation of fluorine-containing compounds

[0006] Fluoroalcohol and isophorone diisocyanate were added into a three-necked flask, and mechanically stirred at 85°C and 350 rpm for 2 h. During stirring, 2-3 drops of dibutyltin dilaurate (DBTDL) were added as a chain transfer agent. After 2 h, hydroxyethyl methacrylate was slowly added dropwise, and the reaction was continued for 2 h. After the reaction was completed, a fluorine-containing compound a with a double bond was obtained.

[0007] The fluorine-containing compound a is 2-((5-(((2,2,3,4,4,4-hexafluorobutoxy)carbonyl)amino)-1,3,3-trimethylcyclohexyl)methyl)carbamoyl)oxy)propyl methacrylate;

[0008] Wherein, the weight ratio of fluoroalcohol: isophorone diisocyanate: hydroxyethyl methacrylate is: 2-6: 5: 2-6;

[0009] 2) Preparation of organic fluorine-modified acrylic resin emulsion

[0010] Take a reactive emulsifier 1-allyloxy-3-(4-nonylphenol)-2-propanol polyoxyethylene (10) ether ammonium sulfate (DNS-86) and the first deionized water in a beaker, and mechanically stir at 350 rpm for 20 minutes to obtain an emulsifier aqueous solution A;

[0011] Add fluorinated compound a and acrylic monomers (functional monomers, hard monomers, and soft monomers) into a beaker and stir magnetically for 15 minutes to obtain a mixed solution B;

[0012] Adding the initiator into the second deionized water and stirring until dissolved to obtain an initiator aqueous solution C;

[0013] Preparation of pre-emulsified emulsion: add 1 / 2 of the emulsifier aqueous solution A into a three-necked flask equipped with a mechanical stirrer, keep the stirring speed at 330 rpm, use a dropping funnel to drop the mixed solution B into the three-necked flask at a rate of 1 to 2 seconds / drop, and continue stirring for 30 minutes after the dropwise addition is completed to obtain a pre-emulsified solution D;

[0014] Preparation of seed emulsion: add the remaining 1 / 2 emulsifier aqueous solution A to a four-necked flask equipped with a reflux condenser, a mechanical stirrer, a dropping funnel and a thermometer, add a buffer, and heat with a water bath, keep the stirring speed at 280-350 rpm, drop 1 / 5 of the pre-emulsion D, wait for the temperature in the four-necked flask to rise to 78-82° C., slowly drop 1 / 5 of the initiator aqueous solution C, and keep warm for 15-30 minutes after the reaction appears a blue phase, to obtain the seed emulsion;

[0015] Emulsion polymerization reaction: using two dropping funnels to drop the remaining pre-emulsion D and the initiator aqueous solution C into the seed emulsion at a constant rate of 6-7 seconds / drop within 3-3.5 hours, the pre-emulsion D is added earlier than the initiator aqueous solution C, and after the addition is completed, the mixture is stirred and reacted at 85-90°C for 1 hour; after the reaction is completed, the reaction liquid is cooled to room temperature, and then the pH is adjusted to 7-8 with 20% ammonia water by mass, and the material is filtered to obtain an organic fluorine-modified acrylic resin emulsion with a solid content of 32%-33%;

[0016] 3) Preparation of organic fluorine-silicone modified acrylic resin emulsion

[0017] Take the reactive emulsifier DNS-86 and the first deionized water in a beaker, and mechanically stir at 350 rpm for 20 minutes to obtain an emulsifier aqueous solution E;

[0018] Add fluorine-containing compound a, silicone, and acrylic monomers (functional monomers, hard monomers, and soft monomers) into a beaker and stir magnetically for 15 minutes to obtain a mixed solution F;

[0019] Add the initiator into the second deionized water and stir until dissolved to obtain an initiator aqueous solution G;

[0020] Preparation of pre-emulsified emulsion: add 1 / 2 of the emulsifier aqueous solution E into a three-necked flask equipped with a mechanical stirrer, keep the stirring speed at 330 rpm, use a dropping funnel to drop the mixed solution F into the flask at a rate of 1 to 2 seconds / drop, and continue stirring for 30 minutes after the dropwise addition is completed to obtain a pre-emulsified solution H;

[0021] Preparation of seed emulsion: add 1 / 2 of the emulsifier aqueous solution E to a four-necked flask equipped with a reflux condenser, a mechanical stirrer, a dropping funnel and a thermometer, add a buffer, and heat with a water bath, keep the stirring speed at 280-350 rpm, drop 1 / 5 of the pre-emulsion H, wait for the temperature in the four-necked flask to rise to 78-82° C., slowly drop 1 / 5 of the initiator aqueous solution G, and keep warm for 15-30 minutes after the reaction appears a blue phase, to obtain the seed emulsion;

[0022] Emulsion polymerization reaction: using two dropping funnels to drip the remaining pre-emulsion H and the initiator aqueous solution G into the seed emulsion at a rate of 6-7 seconds / drop within 3-3.5 hours, the pre-emulsion H is added earlier than the initiator aqueous solution G. After the addition is completed, the mixture is stirred and reacted at 85-90° C. for 1 hour; after the reaction is completed, the reaction liquid is cooled to room temperature, the pH is adjusted to 7-8 with 20% ammonia water by mass, and the material is filtered to obtain an organic fluorine-silicon modified acrylic resin emulsion with a solid content of 31%-33%;

[0023] 4) Preparation of fluorosilicone modified acrylic resin protective liquid

[0024] The mixture of organic fluorine modified acrylic resin emulsion: organic fluorine silicon modified acrylic resin emulsion: nano silicon dioxide in a weight ratio of 1-2: 1-2: 0.08-0.16 is mixed evenly, and stirred evenly at room temperature and 800 rpm magnetic stirring to obtain an inorganic-organic fluorine silicon modified acrylic resin composite material protective liquid;

[0025] In the preparation process of the organic fluorine-modified acrylic resin emulsion, the weight ratio of the fluorine-containing compound a, the hard monomer, the soft monomer, the functional monomer, the initiator, the reactive emulsifier, the buffer, the first deionized water, and the second deionized water is: 0.6-2.4: 2-20: 2-20: 0.6: 0.15-0.27: 0.6-2.1: 0.25-0.5: 30: 30;

[0026] In the preparation process of the organic fluorine-silicone modified acrylic resin emulsion, the weight ratio of the fluorine-containing compound a, organic silicon, hard monomer, soft monomer, functional monomer, initiator, reactive emulsifier, buffer, first deionized water and second deionized water is: 0.6-2.4: 0.6-2.4: 2-20: 2-20: 0.6: 0.15-0.27: 0.6-2.1: 0.25-0.5: 30: 30.

[0027] The hard monomer is one of methyl methacrylate, ethyl methacrylate and styrene.

[0028] The soft monomer is one of butyl acrylate, ethyl acrylate and isooctyl acrylate.

[0029] The functional monomer is one of acrylic acid, methacrylic acid and acrylonitrile.

[0030] The buffer is one of sodium bicarbonate, disodium hydrogen phosphate and potassium dihydrogen phosphate.

[0031] The initiator is one of potassium persulfate, ammonium persulfate and sodium persulfate.

[0032] The fluoroalcohol is one of hexafluorobutanol and decafluoropentanol.

[0033] The organic silicon is one of triethoxy methacrylate silane and methacryloxypropyl trimethoxy silane.

[0034] The invention is scientific and reasonable, has abundant raw materials, good use effect, no pollution, environmental protection and safety, is easy to produce and prepare, and integrates penetration, waterproof and moisture-proof, reinforcement protection, acid, alkali and salt resistance and aging resistance. At the same time, the prepared reinforcement protection material has good stability, low viscosity, strong fluidity, fully combines the high transparency of acrylic resin, good weather resistance, fluorine-containing and silicon compounds have good water resistance, weather resistance, stain resistance and other three advantages, and combines the advantages of good dispersibility and ultraviolet absorption of nano-SiO2, giving the earthen ruins certain moisture-proof and waterproof, acid, alkali and salt resistance, weather resistance, wear resistance and aging resistance effects. In addition, the protective liquid prepared by the present invention has good compatibility with the earthen ruins substrate, can effectively enhance the mechanical strength and compressive strength of the earthen ruins cultural relics, and the original appearance and glossiness and weight changes of the soil sample are not obvious, and the protective film can be removed under the condition of no damage or slight damage, which meets the principle of "repairing the old as the old, keeping the original appearance", is an innovation in the protection of earthen ruins cultural relics, and has remarkable economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 is a synthetic reaction route diagram of fluorine-containing compound a;

[0036] Figure 2 This is the reaction route for the synthesis of organic fluorine-modified acrylic resin;

[0037] Figure 3 This is the reaction route of organic fluorine-silicon modified acrylic resin. DETAILED DESCRIPTION

[0038] The specific implementation methods of the present invention are described in detail below in conjunction with the examples and specific circumstances. It should be understood that these examples are used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0039] Example 1

[0040] An inorganic-organic fluorine-silicon modified acrylic resin composite material protection liquid for earthen ruins reinforcement and protection, and a preparation method thereof comprises the following steps:

[0041] 1) Preparation of fluorine-containing compounds

[0042] Weigh 4 g of fluoroalcohol and 5 g of isophorone diisocyanate, add them into a three-necked flask, stir mechanically for 2 h at 85 ° C and 350 rpm, add 2 to 3 drops of dibutyltin dilaurate (DBTDL) as a chain transfer agent during stirring, slowly add 4 g of hydroxyethyl methacrylate after 2 h, continue the reaction for 2 h, and the reaction is completed to obtain a fluorine-containing compound a with a double bond;

[0043] The fluorine-containing compound a is 2-((5-(((2,2,3,4,4,4-hexafluorobutoxy)carbonyl)amino)-1,3,3-trimethylcyclohexyl)methyl)carbamoyl)oxy)propyl methacrylate;

[0044] 2) Preparation of organic fluorine-modified acrylic resin emulsion

[0045] 1.5 g of reactive emulsifier 1-allyloxy-3-(4-nonylphenol)-2-propanol polyoxyethylene (10) ether ammonium sulfate (DNS-86) and 30 g of first deionized water were weighed in a beaker, and mechanically stirred at 350 rpm for 20 minutes to obtain an emulsifier aqueous solution A;

[0046] Weigh 1.5 g of fluorine-containing compound a and acrylic monomer (0.6 g of functional monomer, 13.95 g of hard monomer, 13.95 g of soft monomer) into a 100 mL beaker and stir magnetically for 15 minutes to obtain a mixed solution B;

[0047] Weigh 0.27 g of initiator and add it into 30 g of the second deionized water and stir until dissolved to obtain an initiator aqueous solution C;

[0048] Preparation of pre-emulsified emulsion: add 1 / 2 of the emulsifier aqueous solution A into a 100 mL three-necked flask equipped with a mechanical stirrer, keep the stirring speed at 330 rpm, use a dropping funnel to drop the mixed solution B into the three-necked flask at a rate of 1 to 2 seconds / drop, and continue stirring for 30 minutes after the dropwise addition is completed to obtain a pre-emulsified solution D;

[0049] Preparation of seed emulsion: add the remaining 1 / 2 emulsifier aqueous solution A to a 250mL four-necked flask equipped with a reflux condenser, a mechanical stirrer, a dropping funnel and a thermometer, add 0.3g of a buffer, and heat with a water bath, keep the stirring speed at 280-350rpm, drop 1 / 5 of the pre-emulsion D, wait for the temperature in the four-necked flask to rise to 78-82°C, slowly drop 1 / 5 of the initiator aqueous solution C, and keep warm for 15-30 minutes after the reaction appears a blue phase, to obtain a seed emulsion;

[0050] Emulsion polymerization reaction: using two dropping funnels to drop the remaining pre-emulsion D and the initiator aqueous solution C into the seed emulsion at a constant rate of 6-7 seconds / drop within 3-3.5 hours, the pre-emulsion D is added earlier than the initiator aqueous solution C, and after the addition is completed, the mixture is stirred and reacted at 85-90°C for 1 hour; after the reaction is completed, the reaction liquid is cooled to room temperature, and then the pH is adjusted to 7-8 with 20% ammonia water by mass, and the material is filtered to obtain an organic fluorine-modified acrylic resin emulsion with a solid content of 32%-33%;

[0051] 3) Preparation of organic fluorine-silicone modified acrylic resin emulsion

[0052] 1.5 g of reactive emulsifier DNS-86 and 30 g of first deionized water were weighed in a beaker, and mechanically stirred at 350 rpm for 20 minutes to obtain an emulsifier aqueous solution E;

[0053] Weigh 1.5 g of fluorine-containing compound a, 1.2 g of silicone, and acrylic monomer (0.6 g of functional monomer, 13.35 g of hard monomer, and 13.35 g of soft monomer) into a 100 mL beaker and stir magnetically for 15 minutes to obtain a mixed solution F;

[0054] Weigh 0.27 g of initiator and add it into 30 g of second deionized water and stir until dissolved to obtain an initiator aqueous solution G;

[0055] Preparation of pre-emulsified emulsion: add 1 / 2 of the emulsifier aqueous solution E into a 100 mL three-necked flask equipped with a mechanical stirrer, keep the stirring speed at 330 rpm, use a dropping funnel to drop the mixed solution F into the flask at a rate of 1 to 2 seconds / drop, and continue stirring for 30 minutes after the dropwise addition is completed to obtain a pre-emulsified solution H;

[0056] Preparation of seed emulsion: add 1 / 2 of the emulsifier aqueous solution E to a 250 mL four-necked flask equipped with a reflux condenser, a mechanical stirrer, a dropping funnel and a thermometer, add 0.3 g of a buffer, and heat with a water bath, keep the stirring speed at 280-350 rpm, drop 1 / 5 of the pre-emulsion H, wait for the temperature in the four-necked flask to rise to 78-82° C., slowly drop 1 / 5 of the initiator aqueous solution G, and keep warm for 15-30 minutes after the reaction appears a blue phase, to obtain the seed emulsion;

[0057] Emulsion polymerization reaction: using two dropping funnels to drip the remaining pre-emulsion H and the initiator aqueous solution G into the seed emulsion at a rate of 6-7 seconds / drop within 3-3.5 hours, the pre-emulsion H is added earlier than the initiator aqueous solution G. After the addition is completed, the mixture is stirred and reacted at 85-90° C. for 1 hour; after the reaction is completed, the reaction liquid is cooled to room temperature, the pH is adjusted to 7-8 with 20% ammonia water by mass, and the material is filtered to obtain an organic fluorine-silicon modified acrylic resin emulsion with a solid content of 31%-33%;

[0058] 4) Preparation of fluorosilicone modified acrylic resin protective liquid

[0059] A mixture of organic fluorine-modified acrylic resin emulsion: organic fluorine-silicon-modified acrylic resin emulsion: nano-silicon dioxide in a weight ratio of 1:1:0.08 was mixed evenly, and stirred evenly under the conditions of room temperature and 800 rpm magnetic stirring to obtain an inorganic-organic fluorine-silicon-modified acrylic resin composite material protective liquid.

[0060] Embodiment 2:

[0061] The difference between this embodiment and embodiment 1 is that: in the preparation process of the organic fluorine-modified acrylic resin emulsion, the weight ratio of the fluorine-containing compound a, the hard monomer, the soft monomer, the functional monomer, the initiator, the reactive emulsifier, the buffer, the first deionized water, and the second deionized water is: 1.2: 14.1: 14.1: 0.6: 0.27: 1.5: 0.3: 30: 30;

[0062] In the preparation process of the organic fluorine-silicone modified acrylic resin emulsion, the weight ratio of the fluorine-containing compound a, organic silicon, hard monomer, soft monomer, functional monomer, initiator, reactive emulsifier, buffer, first deionized water, and second deionized water is: 1.5: 0.9: 13.5: 13.5: 0.6: 0.27: 1.5: 0.3: 30: 30;

[0063] The weight ratio of organic fluorine modified acrylic resin emulsion: organic fluorine silicone modified acrylic resin emulsion: nano silicon dioxide is 1:2:0.16.

[0064] Embodiment 3:

[0065] The difference between this embodiment and embodiment 1 is that: in the preparation process of the organic fluorine-modified acrylic resin emulsion, the weight ratio of the fluorine-containing compound a, the hard monomer, the soft monomer, the functional monomer, the initiator, the reactive emulsifier, the buffer, the first deionized water, and the second deionized water is: 1.8:13.8:13.8:0.6:0.27:1.5:0.3:30:30;

[0066] In the preparation process of the organic fluorine-silicone modified acrylic resin emulsion, the weight ratio of the fluorine-containing compound a, organic silicon, hard monomer, soft monomer, functional monomer, initiator, reactive emulsifier, buffer, first deionized water, and second deionized water is: 1.5:1.5:13.2:13.2:0.6:0.27:1.5:0.3:30:30;

[0067] The weight ratio of organic fluorine modified acrylic resin emulsion: organic fluorine silicone modified acrylic resin emulsion: nano silicon dioxide is: 2:1:0.08.

[0068] When in use, dilute the protective liquid and water in a volume ratio of 1:5 and mix them to carry out penetration reinforcement on the earthen ruins. Carry out penetration reinforcement every 2 hours until the emulsion penetrates completely and forms a film on the surface of the soil sample. After the soil sample reinforcement is completed, dry it naturally at room temperature.

[0069] The present invention prepares an inorganic-organic fluorine-silicon modified acrylic resin composite material protection liquid for the reinforcement and protection of earthen sites, which has the excellent properties of acrylate, organosilicon, organofluorine and inorganic materials. The main chain of each monomer of the acrylate is composed of C-C bonds, and the side chain is a polar group such as a carboxylate group, which has strong light transmittance, good film-forming property, strong adhesion, good oxidation resistance and mildew resistance. The molecular structure of the organosilicon coupling agent contains alkyl and silicon oxygen chain, which has the flexibility and water resistance of polymers, and the anti-aging and weather resistance of inorganic polymer materials. It has good permeability and can adapt to earthen sites with various porosities. The fluorine atom has a large electronegativity and a high CF bond energy, which can significantly reduce the surface tension of water and has excellent hydrophobicity. The modified material has good self-cleaning property and can prevent atmospheric dust from damaging the earthen sites. A certain number of organofluorine-silicon groups are introduced into the acrylic resin structure for modification, so that the obtained resin has the advantages of the three resins and can make up for their respective shortcomings. Siloxane with reactive groups can form a network of hydrophobic siloxane films through the interaction of active groups, which can be evenly distributed on the micropore walls of porous soil substrates, thereby playing a protective role. In addition, the protective liquid also has the advantages of low viscosity and good permeability, and will not destroy the original appearance of the earthen site or block the internal pore structure. The protective material can also fall off or dissolve in the acetone / ethyl acetate mixed solvent, and has a certain reversibility, which can be effectively used for the reinforcement and protection of earthen site cultural relics.

[0070] When the present invention is used specifically, a tablet compactor is used to press the soil sample into a cylindrical reshaped soil of "20 mm in height × 50 mm in diameter". The reinforcement method is to use a dripping method for reinforcement, dilute and mix the protective liquid prepared in the embodiment of the present invention and water in a volume ratio of 1:5, and then perform infiltration reinforcement on the earthen site, and perform infiltration reinforcement once every 2 hours until the emulsion is completely penetrated and a film is formed on the surface of the soil sample. After the soil sample is reinforced, it is naturally dried at room temperature for about a week for performance measurement. In the same way, a blank control is made with a soil sample without the protective liquid. In order to verify the use effect of the present invention, the soil samples of the products of the embodiments of the present invention are treated with the above method respectively, and the hydrolysis resistance, acid and alkali resistance, weight change, water absorption performance, freeze-thaw resistance, and air permeability of the soil samples before and after the treatment are tested. The results are shown in the table below. Among them, the weight of earthen sites is measured in accordance with my country's national standard GB / T50123-1999; the hydrolysis resistance of earthen sites is measured in accordance with my country's national standard GB / T457-2008; the acid, alkali and salt resistance of earthen sites is measured in accordance with my country's national standard GB / 455-2002; the water absorption of earthen sites is measured in accordance with my country's national standard GB / T8941-2013; the air permeability of earthen sites is measured in accordance with GB / T 17146-2015; the freeze-thaw resistance of earthen sites is measured according to the test method in the "Highway Engineering Stone Test Code" T 021194;

[0071] The comparison of the performance index test results of the protective liquid prepared by the methods of Examples 1, 2 and 3 of the present invention on the reinforced soil samples is shown in the following table:

[0072] Table 1 Weight change determination

[0073]

[0074]

[0075] Table 2 Determination of water resistance, acid, alkali and salt resistance of reinforced soil samples

[0076]

[0077] Table 3 Determination of water absorption of reinforced soil samples

[0078]

[0079] Table 4 Determination of freeze-thaw resistance of soil samples reinforced with reinforcement liquid

[0080]

[0081]

[0082] Table 5 Determination of air permeability of reinforced soil samples

[0083]

[0084] The above tests show that compared with blank soil samples, the weight change of the protective liquid prepared by the method of the present invention is not obvious after being used to reinforce the soil samples compared with the original soil samples. The hydrolysis resistance, acid, alkali and salt resistance and water resistance of the reinforced soil samples are significantly better than those of the blank soil samples. In addition, the freeze-thaw resistance and air permeability of the reinforced soil samples are significantly improved, indicating that the reinforcement liquid enhances the stability of the soil samples and improves the physical properties of the soil samples.

[0085] The method of the present invention is scientific and reasonable, with abundant raw materials, and the solvent used is water, which is pollution-free, environmentally friendly and safe, and easy to produce and prepare. The prepared reinforcement and protection material has good stability, low viscosity, strong fluidity, and fully combines the high transparency and good weather resistance of acrylic ester, the water resistance, weather resistance, and stain resistance of organic fluorine monomer, and the heat resistance of organic silicon, and is not easily decomposed by ultraviolet light. In addition, due to the advantages of -OH in organic silicon being easy to hydrolyze and easy to combine with nano-SiO2, the hydrophobic effect is enhanced, so it has good hydrophobicity, high and low temperature resistance and weather resistance, and then the prepared protection liquid has certain moisture-proof, waterproof, acid, alkali and salt resistance properties for earthen sites, and has obvious effects on the reinforcement and protection of earthen sites. The reinforcement protection liquid prepared by the present invention has good compatibility with the earthen site substrate, can effectively enhance the freeze-thaw resistance and air permeability of the earthen site cultural relics, and the original appearance, glossiness and weight of the soil sample do not change significantly, and the protective film can be removed under non-destructive or minimally damaging conditions, which complies with the principle of "repairing the old as it is and maintaining the original appearance". It is an innovation in the protection liquid for earthen site cultural relics protection, and has significant economic and social benefits.

Claims

1. An inorganic-organic composite material protective liquid for the reinforcement and protection of earthen ruins, characterized in that: The preparation method comprises the following steps: 1) Preparation of fluorine-containing compounds Fluoroalcohol and isophorone diisocyanate were added into a three-necked flask, and mechanically stirred at 85°C and 350 rpm for 2 h. During stirring, 2-3 drops of dibutyltin dilaurate (DBTDL) were added as a chain transfer agent. After 2 h, hydroxyethyl methacrylate was slowly added dropwise, and the reaction was continued for 2 h. After the reaction was completed, a fluorine-containing compound a with a double bond was obtained. The fluorine-containing compound a is 2-((5-(((2,2,3,4,4,4-hexafluorobutoxy)carbonyl)amino)-1,3,3-trimethylcyclohexyl)methyl)carbamoyl)oxy)propyl methacrylate; Wherein, the weight ratio of fluoroalcohol: isophorone diisocyanate: hydroxyethyl methacrylate is: 2-6: 5: 2-6; 2) Preparation of organic fluorine-modified acrylic resin emulsion Take a reactive emulsifier 1-allyloxy-3-(4-nonylphenol)-2-propanol polyoxyethylene (10) ether ammonium sulfate (DNS-86) and the first deionized water in a beaker, and mechanically stir at 350 rpm for 20 minutes to obtain an emulsifier aqueous solution A; Add fluorinated compound a and acrylic monomers (functional monomers, hard monomers, and soft monomers) into a beaker and stir magnetically for 15 minutes to obtain a mixed solution B; Adding the initiator into the second deionized water and stirring until dissolved to obtain an initiator aqueous solution C; Preparation of pre-emulsified emulsion: add 1 / 2 of the emulsifier aqueous solution A into a three-necked flask equipped with a mechanical stirrer, keep the stirring speed at 330 rpm, use a dropping funnel to drop the mixed solution B into the three-necked flask at a rate of 1 to 2 seconds / drop, and continue stirring for 30 minutes after the dropwise addition is completed to obtain a pre-emulsified solution D; Preparation of seed emulsion: add the remaining 1 / 2 emulsifier aqueous solution A to a four-necked flask equipped with a reflux condenser, a mechanical stirrer, a dropping funnel and a thermometer, add a buffer, and heat with a water bath, keep the stirring speed at 280-350 rpm, drop 1 / 5 of the pre-emulsion D, wait for the temperature in the four-necked flask to rise to 78-82° C., slowly drop 1 / 5 of the initiator aqueous solution C, and keep warm for 15-30 minutes after the reaction appears a blue phase, to obtain the seed emulsion; Emulsion polymerization reaction: using two dropping funnels to drop the remaining pre-emulsion D and the initiator aqueous solution C into the seed emulsion at a constant rate of 6-7 seconds / drop within 3-3.5 hours, the pre-emulsion D is added earlier than the initiator aqueous solution C, and after the addition is completed, the mixture is stirred and reacted at 85-90°C for 1 hour; after the reaction is completed, the reaction liquid is cooled to room temperature, and then the pH is adjusted to 7-8 with 20% ammonia water by mass, and the material is filtered to obtain an organic fluorine-modified acrylic resin emulsion with a solid content of 32%-33%; 3) Preparation of organic fluorine-silicone modified acrylic resin emulsion Take the reactive emulsifier DNS-86 and the first deionized water in a beaker, and mechanically stir at 350 rpm for 20 minutes to obtain an emulsifier aqueous solution E; Add fluorine-containing compound a, silicone, and acrylic monomers (functional monomers, hard monomers, and soft monomers) into a beaker and stir magnetically for 15 minutes to obtain a mixed solution F; Add the initiator into the second deionized water and stir until dissolved to obtain an initiator aqueous solution G; Preparation of pre-emulsified emulsion: add 1 / 2 of the emulsifier aqueous solution E into a three-necked flask equipped with a mechanical stirrer, keep the stirring speed at 330 rpm, use a dropping funnel to drop the mixed solution F into the flask at a rate of 1 to 2 seconds / drop, and continue stirring for 30 minutes after the dropwise addition is completed to obtain a pre-emulsified solution H; Preparation of seed emulsion: add 1 / 2 of the emulsifier aqueous solution E to a four-necked flask equipped with a reflux condenser, a mechanical stirrer, a dropping funnel and a thermometer, add a buffer, and heat with a water bath, keep the stirring speed at 280-350 rpm, drop 1 / 5 of the pre-emulsion H, wait for the temperature in the four-necked flask to rise to 78-82° C., slowly drop 1 / 5 of the initiator aqueous solution G, and keep warm for 15-30 minutes after the reaction appears a blue phase, to obtain the seed emulsion; Emulsion polymerization reaction: using two dropping funnels to drip the remaining pre-emulsion H and the initiator aqueous solution G into the seed emulsion at a rate of 6-7 seconds / drop within 3-3.5 hours, the pre-emulsion H is added earlier than the initiator aqueous solution G. After the addition is completed, the mixture is stirred and reacted at 85-90° C. for 1 hour; after the reaction is completed, the reaction liquid is cooled to room temperature, the pH is adjusted to 7-8 with 20% ammonia water by mass, and the material is filtered to obtain an organic fluorine-silicon modified acrylic resin emulsion with a solid content of 31%-33%; 4) Preparation of fluorosilicone modified acrylic resin protective liquid The mixture of organic fluorine modified acrylic resin emulsion: organic fluorine silicon modified acrylic resin emulsion: nano silicon dioxide in a weight ratio of 1-2: 1-2: 0.08-0.16 is mixed evenly, and stirred evenly at room temperature and 800 rpm magnetic stirring to obtain an inorganic-organic fluorine silicon modified acrylic resin composite material protective liquid; In the preparation process of the organic fluorine-modified acrylic resin emulsion, the weight ratio of the fluorine-containing compound a, the hard monomer, the soft monomer, the functional monomer, the initiator, the reactive emulsifier, the buffer, the first deionized water, and the second deionized water is: 0.6-2.4: 2-20: 2-20: 0.6: 0.15-0.27: 0.6-2.1: 0.25-0.5: 30: 30; In the preparation process of the organic fluorine-silicone modified acrylic resin emulsion, the weight ratio of the fluorine-containing compound a, organic silicon, hard monomer, soft monomer, functional monomer, initiator, reactive emulsifier, buffer, first deionized water and second deionized water is: 0.6-2.4: 0.6-2.4: 2-20: 2-20: 0.6: 0.15-0.27: 0.6-2.1: 0.25-0.5: 30:

30.

2. The inorganic-organic composite material protection liquid for reinforcing and protecting earthen ruins according to claim 1 is characterized in that: The weight ratio of organic fluorine modified acrylic resin emulsion: organic fluorine silicone modified acrylic resin emulsion: nano silicon dioxide is: 1:1:0.

08.

3. The inorganic-organic composite material protection liquid for reinforcing and protecting earthen ruins according to claim 1 is characterized in that: The weight ratio of organic fluorine modified acrylic resin emulsion: organic fluorine silicone modified acrylic resin emulsion: nano silicon dioxide is 1:2:0.

16.

4. The inorganic-organic composite material protection liquid for reinforcing and protecting earthen ruins according to claim 1 is characterized in that: The weight ratio of organic fluorine modified acrylic resin emulsion: organic fluorine silicone modified acrylic resin emulsion: nano silicon dioxide is: 2:1:0.

08.

5. The inorganic-organic composite material protection liquid for reinforcing and protecting earthen ruins according to claim 1 is characterized in that: The hard monomer is one of methyl methacrylate, ethyl methacrylate and styrene, and the soft monomer is one of butyl acrylate, ethyl acrylate and isooctyl acrylate.

6. The inorganic-organic composite material protection liquid for reinforcing and protecting earthen ruins according to claim 1 is characterized in that: The functional monomer is one of acrylic acid, methacrylic acid and acrylonitrile.

7. The inorganic-organic composite material protection liquid for reinforcing and protecting earthen ruins according to claim 1 is characterized in that: The buffer is one of sodium bicarbonate, disodium hydrogen phosphate and potassium dihydrogen phosphate.

8. The inorganic-organic composite material protection liquid for reinforcing and protecting earthen ruins according to claim 1 is characterized in that: The initiator is one of potassium persulfate, ammonium persulfate and sodium persulfate.

9. The inorganic-organic composite material protection liquid for reinforcing and protecting earthen ruins according to claim 1 is characterized in that: The fluoroalcohol is one of hexafluorobutanol and decafluoropentanol.

10. The inorganic-organic composite material protection liquid for reinforcing and protecting earthen ruins according to claim 1 is characterized by: The organosilicon is one of triethoxy methacrylate silane or methacryloxypropyl trimethoxy silane.

Citation Information

Patent Citations

  • Fluorinated isocyanate and method for preparing fluorinated isocyanate-acrylate copolymer emulsion

    CN103992242A

  • Fluorine-containing polyurethane modified acrylic aqueous resin and preparation method thereof

    CN107903357A

  • Fluorosilicone polyurethane modified acrylic waterborne resin and preparation method thereof

    CN109369862A

  • Organic fluorosilicone-OvPOSS composite modified acrylate soap-free emulsion for earthen archaeological site protection

    CN116622035A

  • Fluoroalkylated allylurethane, its copolymer and water- and oil-repellent, anti-soiling processing agent containing the copolymer as an effective component

    EP0849392A2

Cited By

  • Reinforcing material for earthen archaeological site protection and preparation method thereof

    CN119841583A

  • A Reinforcement Material for the Protection of Earthen Sites and Its Preparation Method

    CN119841583B