Anti-ultraviolet agricultural novel material beneficial to crop growth and preparation method thereof

By applying layered silicate, zinc oxide and modified composite TiO2 on the agricultural greenhouse film, the problem of insufficient protection against ultraviolet rays is solved, and efficient shielding of ultraviolet rays and infrared rays is achieved. Absorption promotes the growth and development of crops.

CN119019932AInactive Publication Date: 2024-11-26HEBEI SHIPUFENG FERTILIZER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411294393.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing agricultural greenhouse film has poor protection effect on ultraviolet rays, resulting in damage to crop growth. The comprehensive performance of existing coatings is insufficient, making it impossible to effectively extend the use time of greenhouse film.

Method used

Using a new agricultural material including layered silicate, zinc oxide, composite UV absorbing matrix, dispersant, cesium-doped tungsten oxide and antibacterial agent, the preparation of modified composite TiO2 and salicylic acid-epoxy soybean oil The reaction is to form a composite ultraviolet absorption matrix with high absorption rate and thermal stability, and is applied to the surface of the greenhouse film to shield the ultraviolet rays and absorb infrared rays.

Benefits of technology

It realizes effective shielding of ultraviolet rays, improves the growth environment of crops, extends the service life of greenhouse membranes, and promotes crop growth through thermal radiation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005045497970000091
    Figure BDA0005045497970000091
  • Figure BDA0005045497970000101
    Figure BDA0005045497970000101
Patent Text Reader

Abstract

The invention belongs to the field of material preparation, and particularly relates to an anti-ultraviolet agricultural novel material beneficial to crop growth and a preparation method thereof. The novel agricultural material comprises the following components in parts by mass: 5-15 parts of layered silicate, 1-10 parts of zinc oxide, 100-200 parts of a composite ultraviolet absorption matrix, 1-3 parts of a dispersing agent, 0.1-1 part of cesium-doped tungsten oxide and 1-2 parts of an antibacterial agent. The novel agricultural material is smeared on the surface of agricultural greenhouse plastic, the novel agricultural material can be spontaneously cured under natural light, a coating with a good shielding effect on ultraviolet rays is obtained, the coating further has the characteristics of absorbing infrared rays and slowly releasing the infrared rays in a heat radiation mode, and growth of planted crops is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of material preparation, and in particular relates to a new agricultural material which is beneficial to the growth of crops and is UV-resistant, and a preparation method thereof. Background Art

[0002] During the growth of crops, the ultraviolet rays in sunlight will have different degrees of impact on crops. The right amount of ultraviolet rays is beneficial to crops, but excessive ultraviolet rays will have a negative impact on the growth and development of plants. Strong ultraviolet rays will destroy the chlorophyll in plant leaves, inhibit the efficiency of photosynthesis, and reduce the growth rate and yield of plants. In addition, ultraviolet rays can also cause spots, fading, and withering on plant leaves, making plants more susceptible to diseases and climate change, and also reducing crop yields. The infrared rays in sunlight can promote the elongation of crop stems and the germination of seeds.

[0003] As a modern agricultural facility, greenhouses bring many advantages to traditional planting methods, which can improve the yield and quality of agricultural products, save water resources, protect crops from extreme weather, and increase the sustainability of agricultural production. Greenhouse films have a certain shielding effect on ultraviolet rays. Patent CN 108997686A discloses a PVA-based greenhouse film that can be degraded at any time. The degradable PVA-based film is formed by casting a mixture of polyvinyl alcohol and starch, and then dried, and a grease waterproof layer is applied on one side of the surface of the two sides, and a paraffin waterproof layer is applied on the other side. Although the PVA-based greenhouse film has good density, gas barrier, light transmittance, elongation, tensile strength and unique water-soluble degradability, it does not mention the protective effect against ultraviolet rays. At present, there is research and development of coatings that are applied to the outer surface of the greenhouse and have the function of blocking ultraviolet rays to achieve the purpose of protecting crops and extending the service life of the greenhouse film, but the comprehensive performance of most coatings is still not ideal.

[0004] Therefore, a new type of agricultural material that can be applied to the outer surface of agricultural greenhouse film is invented, which can shield ultraviolet light, absorb infrared rays and slowly release them in the form of thermal radiation, providing a favorable environment for plant growth and promoting the growth and development of crops in greenhouses, which is of great significance to the development of agriculture. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a new agricultural material that is beneficial to the growth of crops and is resistant to ultraviolet rays and a preparation method thereof. The production process is simple, the cost is low, and it has a good function of shielding ultraviolet rays, and can provide a favorable environment for plant growth.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] The first aspect of the present invention provides a new agricultural material that is beneficial to the growth of crops and is UV-resistant. The material comprises the following components, measured by weight: 5-15 parts of layered silicate, 1-10 parts of zinc oxide, 100-200 parts of a composite UV-absorbing matrix, 1-3 parts of a dispersant, 0.1-1 parts of cesium-doped tungsten oxide, and 1-2 parts of an antibacterial agent.

[0008] In some embodiments, the preparation steps of the composite ultraviolet absorbing matrix are:

[0009] Mix epoxidized soybean oil, salicylic acid, triphenylphosphine, hydroquinone and modified composite TiO2, stir at 80-90°C for 0.5-1h, then heat to 110-120°C and keep warm for 8-10h to obtain a composite ultraviolet absorbing matrix.

[0010] In some embodiments, the molar ratio of the epoxidized soybean oil to salicylic acid is 1:(2-4); and the modified composite TiO2 is 1-6 wt % of the total mass of the epoxidized soybean oil and salicylic acid.

[0011] Preferably, the molar ratio of the epoxidized soybean oil to salicylic acid is 1:3; and the modified composite TiO2 is 3.5wt% of the total mass of the epoxidized soybean oil and salicylic acid.

[0012] In some embodiments, the epoxidation value of the epoxidized soybean oil is ≥ 6 wt %.

[0013] In some embodiments, the preparation steps of the modified composite TiO2 are:

[0014] (1) After ethyl titanate and anhydrous ethanol are mixed evenly, distilled water is added to mix evenly, and dried to obtain a white solid;

[0015] (2) dispersing the white solid and microcrystalline muscovite of step (1) in a hydrogen peroxide solution, adding urea and adjusting the pH of the system to 5-9, placing in a reactor for hydrothermal reaction, cooling to room temperature after the hydrothermal reaction, centrifuging, washing, and drying to obtain a modified composite TiO2;

[0016] (3) Adding a silane coupling agent to anhydrous ethanol, and then adding the composite TiO2 of step (2), adjusting the pH, and heating in a water bath to obtain a modified composite TiO2.

[0017] In some embodiments, the volume ratio of ethyl titanate, anhydrous ethanol and distilled water in step (1) is 1:(4-6):(0.3-0.5).

[0018] Preferably, in step (1), the volume ratio of ethyl titanate, anhydrous ethanol and distilled water is 1:5:0.4.

[0019] In some embodiments, the mass ratio of the white solid, microcrystalline muscovite and urea in step (2) is (0.8-1.7):1:(0.7-1.6).

[0020] Preferably, in step (2), the mass ratio of white solid, microcrystalline muscovite and urea is 1.2:1:1.1.

[0021] In some embodiments, the hydrothermal reaction is carried out at a temperature of 180-200° C. and for a time of 12-24 h.

[0022] Preferably, the temperature of the hydrothermal reaction is 190° C. and the time is 20 h.

[0023] In some embodiments, the layered silicate is sericite and / or montmorillonite.

[0024] The second aspect of the present invention provides a method for preparing a new agricultural material that is beneficial to crop growth and UV-resistant, comprising the following steps:

[0025] Layered silicate, zinc oxide, dispersant, cesium-doped tungsten oxide and antibacterial agent are stirred at 1000-2500 r / min for 10-20 min, the obtained mixture is added to the composite ultraviolet absorption matrix, and stirred at 1000-2500 r / min for 20-60 min to obtain the novel agricultural material.

[0026] The invention obtains a high-performance new agricultural material by compounding layered silicate, zinc oxide, a composite ultraviolet absorbing matrix, a dispersant, cesium-doped tungsten oxide and an antibacterial agent. The new agricultural material is applied to the surface of agricultural greenhouse plastic and can be spontaneously cured under natural light to obtain a coating with good ultraviolet shielding effect. The cesium-doped tungsten oxide added to the coating can absorb infrared rays and slowly release them in the form of thermal radiation, which is beneficial to the growth of crops.

[0027] The present invention first prepares TiO2 by a hydrothermal method in an ethyl titanate system, then uses microcrystalline muscovite as a carrier, strictly controls the hydrothermal temperature, hydrothermal time, the amount of a crystal form control agent and the pH value of the system, and loads the prepared TiO2 of a special crystal form onto the surface of the microcrystalline muscovite sheet to obtain a modified composite TiO2. The present invention can transform the crystal form of TiO2 into a rutile crystal form with a high absorption rate to ultraviolet rays by controlling the conditions of the hydrothermal reaction and the amount of raw materials used, thereby improving the absorption rate of ultraviolet rays. In addition, the microcrystalline muscovite can provide a good attachment site for TiO2, and reduce the size of the loaded TiO2 grains, thereby improving its dispersibility, which may be due to the fact that the interface effect of the microcrystalline muscovite limits the growth of TiO2 grains to a certain extent, and improves the state of easy agglomeration of TiO2, which is conducive to its dispersion in the new agricultural material system, and better plays the role of shielding ultraviolet rays.

[0028] The present invention utilizes salicylic acid and epoxidized soybean oil to react under the action of triphenylphosphine as a catalyst to obtain salicylic acid-epoxidized soybean oil, and adds modified composite TiO2 during the reaction process to form a composite ultraviolet absorption matrix. In the present invention, salicylic acid is grafted onto the epoxidized soybean oil to form a salicylic acid-epoxidized soybean oil with a cross-linked network structure, and has a certain absorption effect on ultraviolet rays. A certain amount of modified composite TiO2 is then added to the salicylic acid-epoxidized soybean oil system, which can be well dispersed in the system, blocking the transmission of part of the ultraviolet rays, and has a significant interlayer reflection effect, so that the ultraviolet light transmittance is reduced, achieving the effect of ultraviolet shielding. In addition, due to the presence of benzene rings and modified composite TiO2 in the composite ultraviolet absorption matrix, the formed coating also has good thermal stability and ultraviolet shielding effect at high temperatures.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1. The present invention provides a high-performance new agricultural material, which is applied to the plastic surface of an agricultural greenhouse and can be spontaneously cured under natural light to obtain a coating. The coating has a good shielding effect against ultraviolet rays, can absorb infrared rays and slowly release them in the form of thermal radiation, which is beneficial to the growth of crops.

[0031] 2. The present invention uses microcrystalline muscovite as a carrier and prepares modified composite TiO2 by a hydrothermal method. The microcrystalline muscovite can provide a good attachment site for TiO2, reduce the grain size of the loaded TiO2, improve its dispersibility in the system, and further improve its absorption rate of ultraviolet rays.

[0032] 3. The present invention utilizes salicylic acid and epoxidized soybean oil to react in the presence of triphenylphosphine as a catalyst to obtain salicylic acid-epoxidized soybean oil, and adds modified composite TiO2 during the reaction to form a composite ultraviolet absorbing matrix with good thermal stability and ultraviolet shielding effect. DETAILED DESCRIPTION

[0033] Now describe in detail various exemplary embodiments of the present invention, this detailed description should not be considered as limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing a particular embodiment, and are not used to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper limit and the lower limit of the range is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the range.

[0034] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as commonly understood by those skilled in the art. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention. Various modifications and variations may be made to the specific embodiments of the present invention specification without departing from the scope or spirit of the present invention, which will be apparent to those skilled in the art. Other embodiments obtained from the present invention specification will be apparent to the technician. The present application specification and examples are exemplary only.

[0035] The words “include,” “including,” “have,” or “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0036] The antibacterial agent used in the present invention is isothiazolinone; the layered silicate used is montmorillonite K-10, purchased from Shanghai McLean Biochemical Technology Co., Ltd.; the microcrystalline muscovite (400 mesh) used is purchased from Sichuan Xinju Mining Resources Development Co., Ltd.; the epoxy soybean oil (epoxy value ≥6.6wt%) used is purchased from Shandong Qilu Petrochemical; the TiO2 powder (rutile type, average particle size of 1 micron) and zinc oxide (average particle size of 1 micron) used are both purchased from Bohuas Nano Technology (Ningbo) Co., Ltd.; the dispersant used is polycarboxylate sodium salt dispersant 731A, purchased from Guangzhou Hengyu Chemical Co., Ltd.; the cesium-doped tungsten oxide used has a particle size of 80-100nm and is purchased from Guangzhou Hongwu Material Technology Co., Ltd.

[0037] Preparation Example 1

[0038] The preparation steps of modified composite TiO2 are:

[0039] (1) After 5 mL of ethyl titanate and 25 mL of anhydrous ethanol are mixed evenly, 0.4 mL of distilled water is added and mixed evenly, and dried at 85° C. to obtain a white solid;

[0040] (2) 6 g of the white solid of step (1) and 5 g of microcrystalline muscovite were dispersed in 200 mL of a 30 wt% aqueous hydrogen peroxide solution, and 5.5 g of urea was added and the pH of the system was adjusted to 6. The mixture was placed in a reactor and subjected to a hydrothermal reaction at 190° C. for 20 h. After the hydrothermal reaction was completed, the mixture was cooled to room temperature, centrifuged, washed with deionized water 3 times, and dried at 100° C. to constant weight to obtain a composite TiO2;

[0041] (3) Add 2 g of silane coupling agent KH570 to 100 mL of anhydrous ethanol, then add 10 g of the composite TiO2 prepared in step (2), adjust the pH to 4.5, and heat in a water bath at 85° C. and 200 r / min for 4 h to obtain a modified composite TiO2.

[0042] Preparation Example 2

[0043] The preparation steps of modified composite TiO2 are:

[0044] (1) After 5 mL of ethyl titanate and 25 mL of anhydrous ethanol are mixed evenly, 0.4 mL of distilled water is added and mixed evenly, and dried at 85° C. to obtain a white solid;

[0045] (2) 6 g of the white solid obtained in step (1) was dispersed in 200 mL of a 30 wt% aqueous hydrogen peroxide solution, and 5.5 g of urea was added to adjust the pH of the system to 6. The mixture was placed in a reactor and subjected to a hydrothermal reaction at 190° C. for 20 h. After the hydrothermal reaction was completed, the mixture was cooled to room temperature, centrifuged, washed with deionized water for 3 times, and dried at 100° C. to a constant weight to obtain a composite TiO2.

[0046] (3) Add 2 g of silane coupling agent KH570 to 100 mL of anhydrous ethanol, then add 10 g of the composite TiO2 prepared in step (2), adjust the pH to 4.5, and heat in a water bath at 85° C. and 200 r / min for 4 h to obtain a modified composite TiO2.

[0047] Preparation Example 3

[0048] The preparation steps of modified composite TiO2 are:

[0049] (1) After 5 mL of ethyl titanate and 25 mL of anhydrous ethanol are mixed evenly, 0.4 mL of distilled water is added and mixed evenly, and dried at 85° C. to obtain a white solid;

[0050] (2) 6 g of the white solid of step (1) and 8 g of microcrystalline muscovite were dispersed in 200 mL of a 30 wt% aqueous hydrogen peroxide solution, and 5.5 g of urea was added and the pH of the system was adjusted to 6. The mixture was placed in a reactor and subjected to a hydrothermal reaction at 190 ° C for 20 h. After the hydrothermal reaction was completed, the mixture was cooled to room temperature, centrifuged, washed with deionized water 3 times, and dried at 100 ° C to constant weight to obtain a composite TiO2;

[0051] (3) Add 2 g of silane coupling agent KH570 to 100 mL of anhydrous ethanol, then add 10 g of the composite TiO2 prepared in step (2), adjust the pH to 4.5, and heat in a water bath at 85° C. and 200 r / min for 4 h to obtain a modified composite TiO2.

[0052] Preparation Example 4

[0053] The preparation steps of modified composite TiO2 are:

[0054] (1) After 5 mL of ethyl titanate and 25 mL of anhydrous ethanol are mixed evenly, 0.4 mL of distilled water is added and mixed evenly, and dried at 85° C. to obtain a white solid;

[0055] (2) 6 g of the white solid of step (1) and 5 g of microcrystalline muscovite were dispersed in 200 mL of a 30 wt% aqueous hydrogen peroxide solution, and 5.5 g of urea was added and the pH of the system was adjusted to 6. The mixture was placed in a reactor and subjected to a hydrothermal reaction at 170 ° C for 20 h. After the hydrothermal reaction was completed, the mixture was cooled to room temperature, centrifuged, washed with deionized water 3 times, and dried at 100 ° C to constant weight to obtain a composite TiO2;

[0056] (3) Add 2 g of silane coupling agent KH570 to 100 mL of anhydrous ethanol, then add 10 g of the composite TiO2 prepared in step (2), adjust the pH to 4.5, and heat in a water bath at 85° C. and 200 r / min for 4 h to obtain a modified composite TiO2.

[0057] Preparation Example 5

[0058] The preparation steps of modified composite TiO2 are the same as those in Preparation Example 1, except that 15 mL of anhydrous ethanol is used in step (1).

[0059] Preparation Example 6

[0060] The preparation steps of the composite ultraviolet absorbing matrix are:

[0061] Mix 0.1 mol of epoxidized soybean oil, 0.3 mol of salicylic acid, 1.5 g of triphenylphosphine, 0.3 g of hydroquinone, and 4.9 g of modified composite TiO2, stir at 85°C for 1 hour, then heat to 115°C and keep warm for 9 hours to obtain a composite ultraviolet absorbing matrix.

[0062] The modified composite TiO2 used is obtained from Preparation Example 1.

[0063] Preparation Example 7

[0064] The preparation steps of the composite ultraviolet absorbing matrix are:

[0065] 0.1 mol of epoxidized soybean oil, 0.3 mol of salicylic acid, 1.5 g of triphenylphosphine and 0.3 g of hydroquinone were mixed, stirred at 85°C for 1 hour, then heated to 115°C and kept warm for 9 hours to obtain a composite ultraviolet absorbing matrix.

[0066] Preparation Example 8

[0067] The preparation steps of the composite ultraviolet absorbing matrix are the same as those of Preparation Example 6, except that the modified composite TiO2 used is obtained from Preparation Example 2.

[0068] Preparation Example 9

[0069] The preparation steps of the composite ultraviolet absorbing matrix are the same as those of Preparation Example 6, except that the modified composite TiO2 used is obtained from Preparation Example 3.

[0070] Preparation Example 10

[0071] The preparation steps of the composite ultraviolet absorbing matrix are the same as those of Preparation Example 6, except that the modified composite TiO2 used is obtained from Preparation Example 4.

[0072] Preparation Example 11

[0073] The preparation steps of the composite ultraviolet absorbing matrix are the same as those of Preparation Example 6, except that the modified composite TiO2 used is obtained from Preparation Example 5.

[0074] Preparation Example 12

[0075] The preparation steps of the composite ultraviolet absorbing matrix are:

[0076] Mix 0.1 mol of epoxidized soybean oil, 0.3 mol of salicylic acid, 1.5 g of triphenylphosphine, 0.3 g of hydroquinone, and 9.2 g of modified composite TiO2, stir at 85°C for 1 hour, then heat to 115°C and keep warm for 9 hours to obtain a composite ultraviolet absorbing matrix.

[0077] The modified composite TiO2 used is obtained from Preparation Example 1.

[0078] Preparation Example 13

[0079] The preparation steps of the composite ultraviolet absorbing matrix are:

[0080] Mix 0.1 mol of epoxidized soybean oil, 0.3 mol of salicylic acid, 1.5 g of triphenylphosphine, 0.3 g of hydroquinone, and 4.9 g of TiO2 powder, stir at 85°C for 1 hour, then heat to 115°C and keep warm for 9 hours to obtain a composite ultraviolet absorbing matrix.

[0081] Preparation Example 14

[0082] The preparation steps of the composite ultraviolet absorbing matrix are:

[0083] Mix 0.1 mol of epoxidized soybean oil, 0.1 mol of salicylic acid, 1.5 g of triphenylphosphine, 0.3 g of hydroquinone, and 4.9 g of modified composite TiO2, stir at 85°C for 1 hour, then heat to 115°C and keep warm for 9 hours to obtain a composite ultraviolet absorbing matrix.

[0084] The modified composite TiO2 used is obtained from Preparation Example 1.

[0085] Example 1

[0086] A method for preparing a new agricultural material that is beneficial to crop growth and UV-resistant, comprising the following steps:

[0087] 5 g of layered silicate, 1 g of zinc oxide, 1 g of dispersant, and 0.1 g of cesium-doped tungsten oxide were stirred at 1000 r / min for 20 min, the obtained mixture and 1 g of antibacterial agent were added to 100 g of composite ultraviolet absorbing matrix, and stirred at 1000 r / min for 60 min to obtain the novel agricultural material.

[0088] The composite ultraviolet absorbing matrix used was obtained from Preparation Example 6.

[0089] Example 2

[0090] A method for preparing a new agricultural material that is beneficial to crop growth and UV-resistant, comprising the following steps:

[0091] 15 g of layered silicate, 10 g of zinc oxide, 3 g of dispersant, and 1 g of cesium-doped tungsten oxide were stirred at 2500 r / min for 10 min, the obtained mixture and 2 g of antibacterial agent were added to 200 g of composite ultraviolet absorbing matrix, and stirred at 2500 r / min for 20 min to obtain the new agricultural material.

[0092] The composite ultraviolet absorbing matrix used was obtained from Preparation Example 6.

[0093] Example 3

[0094] A method for preparing a new agricultural material that is beneficial to crop growth and UV-resistant, comprising the following steps:

[0095] 10 g of layered silicate, 8 g of zinc oxide, 2 g of dispersant, and 0.5 g of cesium-doped tungsten oxide were stirred at 2000 r / min for 15 min, the obtained mixture and 1.5 g of antibacterial agent were added to 150 g of composite ultraviolet absorbing matrix, and stirred at 1500 r / min for 40 min to obtain the new agricultural material.

[0096] The composite ultraviolet absorbing matrix used was obtained from Preparation Example 6.

[0097] Example 4

[0098] A method for preparing a new agricultural material that is beneficial to crop growth and resistant to ultraviolet rays. The specific implementation method is the same as that of Example 3, except that the composite ultraviolet absorbing matrix used is obtained from Preparation Example 7.

[0099] Example 5

[0100] A method for preparing a new agricultural material that is beneficial to crop growth and UV-resistant. The specific implementation method is the same as that of Example 3, except that the composite ultraviolet absorbing matrix used is obtained from Preparation Example 8.

[0101] Example 6

[0102] A method for preparing a new agricultural material that is beneficial to crop growth and resistant to ultraviolet rays. The specific implementation method is the same as that of Example 3, except that the composite ultraviolet absorbing matrix used is obtained from Preparation Example 9.

[0103] Example 7

[0104] A method for preparing a new agricultural material that is beneficial to crop growth and resistant to ultraviolet rays. The specific implementation method is the same as that of Example 3, except that the composite ultraviolet absorbing matrix used is obtained from Preparation Example 10.

[0105] Example 8

[0106] A method for preparing a new agricultural material that is beneficial to crop growth and resistant to ultraviolet rays. The specific implementation method is the same as that of Example 3, except that the composite ultraviolet absorbing matrix used is obtained from Preparation Example 11.

[0107] Example 9

[0108] A method for preparing a new agricultural material that is beneficial to crop growth and resistant to ultraviolet rays. The specific implementation method is the same as that of Example 3, except that the composite ultraviolet absorbing matrix used is obtained from Preparation Example 12.

[0109] Example 10

[0110] A method for preparing a new agricultural material that is beneficial to crop growth and resistant to ultraviolet rays. The specific implementation method is the same as that of Example 3, except that the composite ultraviolet absorbing matrix used is obtained from Preparation Example 13.

[0111] Embodiment 11

[0112] A method for preparing a new agricultural material that is beneficial to crop growth and resistant to ultraviolet rays. The specific implementation method is the same as that of Example 3, except that the composite ultraviolet absorbing matrix used is obtained from Preparation Example 14.

[0113] Comparative Example 1

[0114] A method for preparing a new agricultural material that is beneficial to crop growth and resistant to ultraviolet rays. The specific implementation method is the same as that of Example 3, except that an equal mass of epoxy soybean oil is used instead of a composite ultraviolet absorbing matrix.

[0115] Performance testing of new agricultural materials

[0116] The new agricultural materials obtained in the embodiments and comparative examples were diluted ten times with pure water, ultrasonicated for 5 minutes, and evenly applied to the surface of a quartz glass sheet. After curing for 24 hours under natural light, the formed coating (thickness of 0.004 mm) was tested for UVA, UVB and UFP values ​​using an LH-125 ultraviolet irradiance meter. The specific test data are shown in Table 1.

[0117] Table 1

[0118]

[0119]

[0120] It can be seen from Table 1 that the coating formed on the greenhouse film by the new agricultural material prepared in Examples 1-3 has good ultraviolet protection performance, the transmittance of UVA and UVB is small, and the UFP value is ≥50.

[0121] Compared with Example 3, the modified composite TiO2 is not added to the composite ultraviolet absorbing matrix used in Example 4, so that the matrix does not have the function of protecting against ultraviolet rays; the preparation conditions of the modified composite TiO2 used in the composite ultraviolet absorbing matrix in the new agricultural material are changed in 5-8, resulting in a change in the crystal form of TiO2 in the modified composite TiO2, affecting its ultraviolet protection performance, thereby reducing the ultraviolet protection performance of the new agricultural material; the amount of modified composite TiO2 added to the composite ultraviolet absorbing matrix used in Example 9 is too much, which affects the synthesis of the composite ultraviolet absorbing matrix, weakens the ultraviolet protection effect of the matrix, and thus reduces the ultraviolet protection performance of the new agricultural material; Example 1 0, the addition of ordinary TiO2 powder to the composite ultraviolet absorbing matrix reduces the ultraviolet protection performance, weakens the ultraviolet protection effect of the matrix, and thus significantly reduces the ultraviolet protection performance of the new agricultural material; in the preparation process of the composite ultraviolet absorbing matrix used in Example 11, the ratio of epoxidized soybean oil and salicylic acid was changed, the grafting rate of salicylic acid on the epoxidized soybean oil was reduced, affecting the internal structure of the composite ultraviolet absorbing matrix, and significantly reducing the ultraviolet protection performance of the new agricultural material; in Comparative Example 1, an equal mass of epoxidized soybean oil was used to replace the composite ultraviolet absorbing matrix, and the epoxidized soybean oil did not have an ultraviolet protection effect, so the ultraviolet protection performance of the new agricultural material in Comparative Example 1 was the worst.

[0122] The above is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present application. Although the present application is disclosed as above in the preferred embodiment, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution.

Claims

1. A new agricultural material that is beneficial to crop growth and UV-resistant, characterized in that: The composition comprises the following components in parts by weight: 5-15 parts of layered silicate, 1-10 parts of zinc oxide, 100-200 parts of composite ultraviolet absorption matrix, 1-3 parts of dispersant, 0.1-1 parts of cesium-doped tungsten oxide and 1-2 parts of antibacterial agent.

2. The new agricultural material according to claim 1, characterized in that: The preparation steps of the composite ultraviolet absorbing matrix are as follows: Mix epoxidized soybean oil, salicylic acid, triphenylphosphine, hydroquinone and modified composite TiO2, stir at 80-90°C for 0.5-1h, then heat to 110-120°C and keep warm for 8-10h to obtain a composite ultraviolet absorbing matrix.

3. The new agricultural material according to claim 2, characterized in that: The molar ratio of the epoxy soybean oil and salicylic acid is 1:(2-4); the modified composite TiO2 is 1-6wt% of the total mass of the epoxy soybean oil and salicylic acid.

4. The new agricultural material according to claim 3, characterized in that: The epoxy value of the epoxy soybean oil is ≥6wt%.

5. The new agricultural material according to claim 2, characterized in that: The preparation steps of the modified composite TiO2 are: (1) After ethyl titanate and anhydrous ethanol are mixed evenly, distilled water is added to mix evenly, and dried to obtain a white solid; (2) dispersing the white solid and microcrystalline muscovite of step (1) in a hydrogen peroxide solution, adding urea and adjusting the pH of the system to 5-9, placing in a reactor for hydrothermal reaction, cooling to room temperature after the hydrothermal reaction, centrifuging, washing, and drying to obtain composite TiO2; (3) Adding a silane coupling agent to anhydrous ethanol, and then adding the composite TiO2 of step (2), adjusting the pH, and heating in a water bath to obtain a modified composite TiO2.

6. The new agricultural material according to claim 5, characterized in that: In the step (1), the volume ratio of ethyl titanate, anhydrous ethanol and distilled water is 1:(4-6):(0.3-0.5).

7. The new agricultural material according to claim 5, characterized in that: In the step (2), the mass ratio of the white solid, microcrystalline muscovite and urea is (0.8-1.7):1:(0.7-1.6).

8. The new agricultural material according to claim 5, characterized in that: The temperature of the hydrothermal reaction is 180-200° C. and the time is 12-24 hours.

9. The new agricultural material according to claim 1, characterized in that: The layered silicate is sericite and / or montmorillonite.

10. A method for preparing the new agricultural material according to any one of claims 1 to 9, characterized in that: The following steps are involved: Layered silicate, zinc oxide, dispersant, cesium-doped tungsten oxide and antibacterial agent are stirred at 1000-2500 r / min for 10-20 min, the obtained mixture is added to the composite ultraviolet absorption matrix, and stirred at 1000-2500 r / min for 20-60 min to obtain the novel agricultural material.