High-stability residue-free adhesive tape for wafer cutting and preparation method thereof

Through the coordination cross-linking of Zn+, acrylic acid and multi-arm semiconjugated trippyridine, the stability of wafer cutting tape under temperature and light irradiation conditions is solved, and high stability and residual-free tape preparation is achieved. It is suitable for Improve tape performance during wafer cutting.

CN119019946APending Publication Date: 2024-11-26AZUSA TECH (SHENZHEN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411115350.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing wafer cutting tape has reduced adhesion performance under temperature changes and light irradiation, poor thermal stability and optical stability, and it is easy to leave residue after peeling, affecting chip performance.

Method used

By using the coordination cross-linking between Zn+, acrylic acid and multi-arm semiconjugated trippyridine, the multi-arm semiconjugated trippyridine compound is prepared, and combined with materials such as isooctyl acrylate. A high stability and residual wafer cutting glue was formed and the tape was prepared by applying it to a polyethylene acetate film.

Benefits of technology

The thermal stability and optical stability of the tape are improved, the residual problem of the tape is avoided during peeling, the temperature range is expanded, and the optical performance of the tape is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019946A_ABST
    Figure CN119019946A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-stability and residue-free adhesive tape for wafer cutting. The preparation method specifically comprises the following steps: step 1, synthesizing a multi-arm precursor; 2, preparing a multi-arm semi-conjugated terpyridine compound according to a product obtained in the step 1; 3, wafer cutting glue is prepared according to a product obtained in the step 2; and 4, preparing the wafer cutting adhesive tape from the wafer cutting adhesive prepared in the step 3. The invention further discloses the high-stability and residue-free adhesive tape for wafer cutting prepared by adopting the preparation method, the adhesive residue during adhesive tape stripping is avoided by utilizing the coordination cross-linking effect among Zn < + >, acrylic acid and terpyridyl, and meanwhile, the optical stability of the adhesive in the adhesive tape is improved through the terpyridyl structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer composite materials, and relates to a highly stable, residue-free wafer dicing tape. The invention also relates to a preparation method of the highly stable, residue-free wafer dicing tape. Background Art

[0002] Wafer cutting is an indispensable step in chip processing and preparation. The grains are cut from wafers. Due to the small size of the grains, bevel edges, edge damage, particle splashing and other problems are prone to occur during cutting. Therefore, wafer protective tape is usually used for protection during wafer cutting. However, the existing wafer cutting tape is used at a temperature of 10-30°C. Exceeding this temperature will lead to reduced adhesive properties and insufficient thermal stability. At the same time, the adhesion of the tape decreases under natural light conditions, resulting in poor optical stability. In addition, when the protective tape is used for wafer cutting, the protective tape needs to be peeled off after the cutting is completed. If there is glue residue after peeling, it will have an adverse effect on the performance of the wafer chip. Therefore, it is of great significance to achieve improved stability (including thermal stability and optical stability) and no residue of the protective glue. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a highly stable, residue-free wafer dicing tape, which utilizes the coordination cross-linking effect between Zn+, acrylic acid and terpyridine to avoid adhesive residue when the tape is peeled off, and at the same time improves the optical stability of the adhesive in the tape through the terpyridine structure.

[0004] Another object of the present invention is to provide a stable, residue-free wafer dicing tape.

[0005] The first technical solution adopted by the present invention is a method for preparing a highly stable and residue-free wafer dicing tape, which specifically comprises the following steps:

[0006] Step 1, synthesizing a multi-arm precursor;

[0007] Step 2, preparing a multi-arm semi-conjugated terpyridine compound according to the product obtained in step 1;

[0008] Step 3, preparing wafer dicing adhesive according to the product obtained in step 2;

[0009] Step 4, preparing wafer dicing tape using the wafer dicing adhesive prepared in step 3.

[0010] The first technical solution of the present invention is also characterized in that:

[0011] The specific process of step 1 is:

[0012] Step 1, dissolve 19.1 g to 57.3 g of nitrilotriacetic acid and 40.1 to 120.3 g of 4-aminobenzaldehyde in 50 to 100 mL of N,N-dimethylacetamide solution, and stir at room temperature for 5 to 15 minutes;

[0013] Step 1.2, add 0.2-0.6 g of catalyst to the product obtained in step 1.1, heat the reaction solution to 60-120° C. and continue the reaction for 3-9 hours. After the reaction is completed, pour the solution into 500-1500 mL of deionized water, filter and collect the precipitate, add 200-600 mL of ethanol to the collected precipitate, and recrystallize the precipitate to obtain a colorless multi-arm precursor.

[0014] In step 1.2, the catalyst is 4-dimethylaminopyridine.

[0015] The specific process of step 2 is:

[0016] Step 2.1, 3-9 g of the multi-arm precursor was dissolved in 50-100 mL of a mixed solvent of N,N-dimethylacetamide and ethanol, and then 0.23-0.69 g of NaH was added and stirred at room temperature for 30 min;

[0017] Step 2.2, dissolve 3-9 mL of 2-acetylpyridine in 10 mL of ethanol solution and add dropwise to the solution prepared in step 2.1, the addition time is 30-60 min, and stirring is continued for 2-4 h. After the reaction is completed, cool to room temperature, add 10-30 mL of ammonia water to the reaction solution, continue stirring for 24-48 h, filter and collect the solid product, wash the filtered filter cake with 30-60 mL of ethanol at 0°C to obtain a multi-arm semi-conjugated terpyridine compound.

[0018] The specific process of step 3 is:

[0019] Take 0.2-0.4g of a multi-arm semi-conjugated terpyridine compound, 0.01-0.05g of zinc chloride, 1-3g of isooctyl acrylate, 1-3g of isooctyl acrylate oligomer, 0.2-0.6mL of acrylic acid, 0.2-0.6g of dodecyl acrylate, and 0.1-0.2g of 1-hydroxycyclohexyl phenone, add them successively into 5-10mL of tetrahydrofuran solvent and mix evenly to obtain a wafer dicing adhesive.

[0020] The specific process of step 4 is: coating the wafer dicing adhesive prepared in step 3 on a 5-10 cm thick polyvinyl acetate film, and drying at 45-60° C. for 1-2 hours to obtain a wafer dicing tape.

[0021] The second technical solution adopted by the present invention is that the highly stable and residue-free wafer dicing tape is prepared by adopting the preparation method of the highly stable and residue-free wafer dicing tape.

[0022] The beneficial effects of the present invention are that the present invention constructs a multi-arm semi-conjugated terpyridine compound, utilizes the multi-arm semi-conjugated structure to improve the thermal stability of wafer dicing glue and reduce the viscosity-flow transition temperature, thereby expanding the use temperature range of the dicing glue; and utilizes the terpyridine structure to adjust the optical stability of the glue. 2+ The coordination cross-linking between metal ions, acrylic acid and terpyridine structural elements solves the problem of adhesive residue. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a comparative diagram of ultraviolet absorption of the adhesive contained in the tapes prepared in Example 1 of the method for preparing the highly stable and residue-free wafer dicing tape of the present invention and Comparative Examples 1 to 3. DETAILED DESCRIPTION

[0024] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0025] The method for preparing the highly stable and residue-free wafer dicing tape of the present invention specifically comprises the following steps:

[0026] Step 1, synthesis of multi-arm precursor, specifically:

[0027] Take 19.1-57.3g of nitrilotriacetic acid and 40.1-120.3g of 4-aminobenzaldehyde and dissolve them in 50-100mL of N,N-dimethylacetamide solution, and stir at room temperature for 5-15 minutes. Further add 0.2-0.6g of 4-dimethylaminopyridine catalyst. Heat the reaction solution to 60-120℃ and continue the reaction for 3-9h. After the reaction is completed, pour the solution into 500-1500mL of deionized water, filter and collect the precipitate, add 200-600mL of ethanol to the collected precipitate, recrystallize the precipitate, and obtain a colorless multi-arm precursor.

[0028] Step 2, a multi-arm semi-conjugated terpyridine compound, specifically:

[0029] Step 2.1, 3-9 g of the multi-arm precursor was dissolved in 50-100 mL of a mixed solvent of N,N-dimethylacetamide and ethanol (v:v=1:2), and 0.23-0.69 g of NaH was further added, and stirred at room temperature for 30 min.

[0030] Step 2.2, dissolve 3-9 mL of 2-acetylpyridine in 10 mL of ethanol solution and add dropwise to the solution prepared in step 2.1 for 30-60 min. Continue stirring for 2-4 h after the addition is completed. After the reaction is completed, cool to room temperature, add 10-30 mL of 35 wt% ammonia water to the reaction solution, continue stirring for 24-48 h, filter and collect the solid product, wash the filter cake with 30-60 mL of ethanol at 0 ° C to obtain a multi-arm semi-conjugated terpyridine compound;

[0031] Step 3, preparation of wafer dicing glue;

[0032] Take a multi-arm semi-conjugated terpyridine compound (0.2-0.4g), zinc chloride (0.01-0.05g), isooctyl acrylate (1-3g), isooctyl acrylate oligomer (1-3g, molecular weight of 1000-2000), acrylic acid (0.2-0.6mL), dodecyl acrylate (0.2-0.6g), 1-hydroxycyclohexyl phenyl ketone (0.1-0.2g), add them to 5-10mL of tetrahydrofuran solvent and mix them evenly to obtain a wafer dicing adhesive;

[0033] Step 4, coating the wafer dicing adhesive prepared in step 3 on a 5-10 cm thick polyvinyl acetate film, and drying at 45-60° C. for 1-2 hours to obtain a wafer dicing tape.

[0034] Example 1

[0035] Step 1, synthesis of multi-arm precursor, specifically:

[0036] Take 19.1g of nitrilotriacetic acid and 40.1g of 4-aminobenzaldehyde and dissolve them in 50mL of N,N-dimethylacetamide solution and stir at room temperature for 5 minutes. Further add 0.2g of 4-dimethylaminopyridine catalyst. Heat the reaction solution to 60℃ and continue the reaction for 3h. After the reaction is completed, pour the solution into 500mL of deionized water, filter and collect the precipitated product, add 200mL of ethanol for recrystallization to obtain a colorless multi-arm precursor.

[0037] Step 2, a multi-arm semi-conjugated terpyridine compound, specifically:

[0038] Take 3g of the multi-arm precursor and dissolve it in 50mL of a mixed solvent of N,N-dimethylacetamide and ethanol (v:v=1:2), further add 0.23g of NaH, and stir at room temperature for 30min. Dissolve 3mL of 2-acetylpyridine in 10mL of ethanol solution and add dropwise to the above solution for 30min. Continue stirring for 2h after the addition. After the reaction is completed, cool to room temperature, add 10mL of 35wt% ammonia water to the reaction solution, continue stirring for 24h, filter and collect the solid product, wash the filter cake with 30mL of ethanol (0℃), and obtain a multi-arm semi-conjugated terpyridine compound.

[0039] Step 3, preparation of wafer dicing glue, specifically:

[0040] Take a multi-arm semi-conjugated terpyridine compound (0.2g), zinc chloride (0.01g), isooctyl acrylate (1g), isooctyl acrylate oligomer (1g, molecular weight 1000), acrylic acid (0.2mL), dodecyl acrylate (0.2g), and 1-hydroxycyclohexyl phenyl ketone (0.1g), add them to 5mL of tetrahydrofuran solvent in sequence and mix well to obtain wafer dicing glue.

[0041] Step 4, coating the glue prepared in step 3 on a 5 cm thick polyvinyl acetate film, and drying at 45° C. for 1 hour to obtain a wafer dicing tape.

[0042] Comparative Example 1 (Zinc chloride is removed from the glue, and there is residue when the glue is peeled off)

[0043] Step 1, synthesis of multi-arm precursor, specifically:

[0044] Take 19.1g of nitrilotriacetic acid and 40.1g of 4-aminobenzaldehyde and dissolve them in 50mL of N,N-dimethylacetamide solution and stir at room temperature for 5 minutes. Further add 0.2g of 4-dimethylaminopyridine catalyst. Heat the reaction solution to 60℃ and continue the reaction for 3h. After the reaction is completed, pour the solution into 500mL of deionized water, filter and collect the precipitated product, and recrystallize it with 200mL of ethanol to obtain a colorless multi-arm precursor.

[0045] Step 2, a multi-arm semi-conjugated terpyridine compound, specifically:

[0046] Take 3g of the multi-arm precursor and dissolve it in 50mL of a mixed solvent of N,N-dimethylacetamide and ethanol (v:v=1:2), further add 0.23g of NaH, and stir at room temperature for 30min. Dissolve 3mL of 2-acetylpyridine in 10mL of ethanol solution and add dropwise to the above solution for 30min. Continue stirring for 2h after the addition. After the reaction is completed, cool to room temperature, add 10mL of 35wt% ammonia water to the reaction solution, continue stirring for 24h, filter and collect the solid product, wash the filter cake with 30mL of ethanol (0℃), and obtain a multi-arm semi-conjugated terpyridine compound;

[0047] Step 3, preparation of wafer dicing glue, the specific process is as follows:

[0048] Take a multi-arm semi-conjugated terpyridine compound (0.2 g), isooctyl acrylate (1 g), isooctyl acrylate oligomer (1 g, molecular weight 1000), acrylic acid (0.2 mL), dodecyl acrylate (0.2 g), and 1-hydroxycyclohexyl phenyl ketone (0.1 g), gradually add them into 5 mL of tetrahydrofuran solvent and mix well to obtain a wafer dicing adhesive.

[0049] Step 4, coating the glue prepared in step 3 on a 5 cm thick polyvinyl acetate film, and drying at 45° C. for 1 hour to obtain a wafer dicing tape.

[0050] Comparative Example 2 (the multi-arm semi-conjugated terpyridine compound was not added to the glue, and there was residue when the glue was peeled off, and the optical stability and thermal stability were reduced)

[0051] Take zinc chloride (0.01g), isooctyl acrylate (1g), isooctyl acrylate oligomer (1g, molecular weight 1000), acrylic acid (0.2mL), dodecyl acrylate (0.2g), and 1-hydroxycyclohexyl phenyl ketone (0.1g), add them to 5mL of tetrahydrofuran solvent in turn and mix well to obtain wafer dicing glue, apply the glue on a 5cm polyvinyl acetate film, and dry it at 45°C for 1h to obtain a wafer dicing tape.

[0052] Comparative Example 3 (When acrylic acid is not added to the adhesive structure, adhesive residue remains during peeling and viscosity decreases)

[0053] Step 1, synthesis of multi-arm precursor, specifically:

[0054] Take 19.1g of nitrilotriacetic acid and 40.1g of 4-aminobenzaldehyde and dissolve them in 50mL of N,N-dimethylacetamide solution and stir at room temperature for 5 minutes. Further add 0.2g of 4-dimethylaminopyridine catalyst. Heat the reaction solution to 60℃ and continue the reaction for 3h. After the reaction is completed, pour the solution into 500mL of deionized water, filter and collect the precipitated product, and recrystallize it with 200mL of ethanol to obtain a colorless multi-arm precursor.

[0055] Step 2, a multi-arm semi-conjugated terpyridine compound, specifically:

[0056] Take 3g of multi-arm precursor and dissolve it in 50mL of N,N-dimethylacetamide and ethanol mixed solvent (v:v=1:2), further add 0.23g of NaH, and stir at room temperature for 30min. Dissolve 3mL of 2-acetylpyridine in 10mL of ethanol solution and add dropwise to the above solution for 30min. Continue stirring for 2h after the addition. After the reaction is completed, cool to room temperature, add 10mL of 35wt% ammonia water to the reaction solution, continue stirring for 24h, filter and collect the solid product, and wash the filter cake with 30mL of ethanol (0℃).

[0057] Step 3, preparation of wafer dicing glue, the specific process is as follows:

[0058] Take a multi-arm semi-conjugated terpyridine compound (0.2 g), zinc chloride (0.01 g), isooctyl acrylate (1 g), isooctyl acrylate oligomer (1 g, molecular weight 1000), dodecyl acrylate (0.2 g), and 1-hydroxycyclohexyl phenyl ketone (0.1 g), and add them in sequence to 5 mL of tetrahydrofuran solvent to obtain wafer dicing glue.

[0059] Step 4, coating the glue prepared in step 3 on a 5 cm thick polyvinyl acetate film, and drying at 45° C. for 1 hour to obtain a wafer dicing tape.

[0060] The following table 1 is the analysis and test results of Example 1 and Comparative Examples 1-3:

[0061] Table 1

[0062]

[0063] Aging refers to whether the viscosity of the glue decreases when it is irradiated with a 45W UV lamp for 12 hours. The applicable temperature refers to the temperature at which no glue spots or wire drawing occur.

[0064] As shown in Table 1, in Comparative Example 3, acrylic acid is added, and there is a lack of hydrogen bonds formed by carboxyl groups between molecules, and there is a lack of ionic bonds between molecules and Zn2+, which leads to a decrease in the viscosity of the glue.

[0065] like Figure 1As shown, in Comparative Example 2, since no multi-arm semi-conjugated terpyridine compound was added, the molar absorption coefficient of the glue was low and could not effectively absorb ultraviolet rays. Among them, ultraviolet rays are the main factor causing the aging of the glue and the deterioration of performance. The terpyridine structural unit absorbs ultraviolet rays, effectively avoiding ultraviolet rays from aging the glue and achieving the wire isolation effect. After irradiation with a 45W ultraviolet lamp for 12 hours, only Comparative Example 2 showed aging.

[0066] Comparative Example 2 has a lower applicable temperature, since no multi-arm semi-conjugated terpyridine compound is added and a cross-linked network structure cannot be formed, which reduces its viscosity-flow transition temperature and narrows its applicable temperature range.

[0067] Since Comparative Example 1 lacks Zn 2+ The comparative example 2 lacks the coordination chelation points of the multi-arm semi-conjugated terpyridine compound, and the comparative example 3 lacks the carboxyl chelation points of acrylic acid, and both cannot form coordination cross-linking points. The center of gravity is easily displaced between molecules, resulting in glue residue when the glue is peeled off.

[0068] Example 2

[0069] Step 1, synthesis of multi-arm precursor, specifically:

[0070] Take 30.5g of nitrilotriacetic acid and 80.5g of 4-aminobenzaldehyde and dissolve them in 80mL of N,N-dimethylacetamide solution and stir at room temperature for 10 minutes. Further add 0.4g of 4-dimethylaminopyridine catalyst. Heat the reaction solution to 100℃ and continue the reaction for 6h. After the reaction is completed, pour the solution into 1000mL of deionized water, filter and collect the precipitated product, add 400mL of ethanol for recrystallization, and obtain a colorless multi-arm precursor.

[0071] Step 2, a multi-arm semi-conjugated terpyridine compound, specifically:

[0072] Take 6g of the multi-arm precursor and dissolve it in 80mL of a mixed solvent of N,N-dimethylacetamide and ethanol (v:v=1:2), further add 0.48g of NaH, and stir at room temperature for 30min. Dissolve 6mL of 2-acetylpyridine in 10mL of ethanol solution and add dropwise to the above solution for 40min. Continue stirring for 3h after the addition. After the reaction is completed, cool to room temperature, add 20mL of 35wt% ammonia water to the reaction solution, continue stirring for 36h, filter and collect the solid product, wash the filter cake with 40mL of ethanol (0℃), and obtain a multi-arm semi-conjugated terpyridine compound;

[0073] Step 3, preparation of wafer dicing glue, specifically:

[0074] Take a multi-arm semi-conjugated terpyridine compound (0.3g), zinc chloride (0.03g), isooctyl acrylate (2g), isooctyl acrylate oligomer (2g, molecular weight 1500), acrylic acid (0.4mL), dodecyl acrylate (0.4g), and 1-hydroxycyclohexyl phenyl ketone (0.15g), add them in 8mL of tetrahydrofuran solvent in sequence and mix well to obtain wafer dicing glue.

[0075] Step 4, coating the glue prepared in step 3 on a 8 cm thick polyvinyl acetate film, and drying at 50° C. for 1.5 h to obtain a wafer dicing tape.

[0076] Example 3

[0077] Step 1, synthesis of multi-arm precursor, specifically:

[0078] Take 57.3g of nitrilotriacetic acid and 120.3g of 4-aminobenzaldehyde and dissolve them in 100mL of N,N-dimethylacetamide solution and stir at room temperature for 15 minutes. Further add 0.6g of 4-dimethylaminopyridine catalyst. Heat the reaction solution to 100℃ and continue the reaction for 9h. After the reaction is completed, pour the solution into 1500mL of deionized water, filter and collect the precipitated product, add 600mL of ethanol for recrystallization, and obtain a colorless multi-arm precursor.

[0079] Step 2, a multi-arm semi-conjugated terpyridine compound, specifically:

[0080] Take 9g of the multi-arm precursor and dissolve it in 100mL of N,N-dimethylacetamide and ethanol mixed solvent (v:v=1:2), further add 0.69g of NaH, and stir at room temperature for 30min. Dissolve 9mL of 2-acetylpyridine in 10mL of ethanol solution and add dropwise to the above solution for 60min. Continue stirring for 4h after the addition. After the reaction is completed, cool to room temperature, add 30mL of 35wt% ammonia water to the reaction solution, continue stirring for 48h, filter and collect the solid product, wash the filter cake with 60mL of ethanol (0℃), and obtain a multi-arm semi-conjugated terpyridine compound.

[0081] Step 3, preparation of wafer dicing glue, specifically:

[0082] Take a multi-arm semi-conjugated terpyridine compound (0.4 g), zinc chloride (0.05 g), isooctyl acrylate (3 g), isooctyl acrylate oligomer (3 g, molecular weight 1500), acrylic acid (0.6 mL), dodecyl acrylate (0.6 g), and 1-hydroxycyclohexyl phenyl ketone (0.2 g), add them to 10 mL of tetrahydrofuran solvent in sequence and mix well to obtain wafer dicing glue.

[0083] Step 4, coating the glue prepared in step 3 on a 10 cm thick polyvinyl acetate film, and drying at 60° C. for 2 h to obtain a wafer dicing tape.

[0084] The present invention utilizes the coordination cross-linking effect between Zn+, acrylic acid and terpyridine to avoid residues when the adhesive is peeled off. At the same time, terpyridine has high light absorption to improve the optical stability of the adhesive. Most multi-arm semi-conjugated terpyridine has high conjugation, which effectively adjusts the thermal stability and viscosity-flow transition temperature of the adhesive to improve its applicable temperature range.

Claims

1. Preparation method of highly stable and residue-free wafer dicing tape, Features: The specific steps include: Step 1, synthesizing a multi-arm precursor; Step 2, preparing a multi-arm semi-conjugated terpyridine compound according to the product obtained in step 1; Step 3, preparing wafer dicing adhesive according to the product obtained in step 2; Step 4, preparing wafer dicing tape using the wafer dicing adhesive prepared in step 3.

2. The method for preparing the highly stable, residue-free wafer dicing tape according to claim 1, Features: The specific process of step 1 is as follows: Step 1, dissolve 19.1 g to 57.3 g of nitrilotriacetic acid and 40.1 to 120.3 g of 4-aminobenzaldehyde in 50 to 100 mL of N,N-dimethylacetamide solution, and stir at room temperature for 5 to 15 minutes; Step 1.2, add 0.2-0.6 g of catalyst to the product obtained in step 1.1, heat the reaction solution to 60-120° C. and continue the reaction for 3-9 hours. After the reaction is completed, pour the solution into 500-1500 mL of deionized water, filter and collect the precipitate, add 200-600 mL of ethanol to the collected precipitate, and recrystallize the precipitate to obtain a colorless multi-arm precursor.

3. The method for preparing the highly stable, residue-free wafer dicing tape according to claim 2, Features: In the step 1.2, the catalyst is 4-dimethylaminopyridine.

4. The method for preparing the highly stable, residue-free wafer dicing tape according to claim 2, Features: The specific process of step 2 is as follows: Step 2.1, 3-9 g of the multi-arm precursor was dissolved in 50-100 mL of a mixed solvent of N,N-dimethylacetamide and ethanol, and then 0.23-0.69 g of NaH was added and stirred at room temperature for 30 min; Step 2.2, dissolve 3-9 mL of 2-acetylpyridine in 10 mL of ethanol solution and add dropwise to the solution prepared in step 2.1, the addition time is 30-60 min, and stirring is continued for 2-4 h. After the reaction is completed, cool to room temperature, add 10-30 mL of ammonia water to the reaction solution, continue stirring for 24-48 h, filter and collect the solid product, wash the filtered filter cake with 30-60 mL of ethanol at 0°C to obtain a multi-arm semi-conjugated terpyridine compound.

5. The method for preparing the highly stable, residue-free wafer dicing tape according to claim 4, Features: The specific process of step 3 is as follows: Take 0.2-0.4g of a multi-arm semi-conjugated terpyridine compound, 0.01-0.05g of zinc chloride, 1-3g of isooctyl acrylate, 1-3g of isooctyl acrylate oligomer, 0.2-0.6mL of acrylic acid, 0.2-0.6g of dodecyl acrylate, and 0.1-0.2g of 1-hydroxycyclohexyl phenone, add them successively into 5-10mL of tetrahydrofuran solvent and mix evenly to obtain a wafer dicing adhesive.

6. The method for preparing the highly stable, residue-free wafer dicing tape according to claim 5, Features: The specific process of step 4 is: coating the wafer dicing adhesive prepared in step 3 on a 5-10 cm thick polyvinyl acetate film, and drying at 45-60° C. for 1-2 hours to obtain a wafer dicing tape.

7. Highly stable, residue-free wafer dicing tape, Features: The invention is prepared by the method for preparing the highly stable and residue-free wafer dicing tape as claimed in any one of claims 1 to 6.