Waterproof epoxy resin adhesive as well as preparation method and application thereof

By using modified epoxy resin glue in Mini LED display, combining hydrophobic groups and nanofillers to form an interpenetrating network structure, the oxidative corrosion problem caused by humidity in the outdoor environment is solved, and high The combination of waterproofing and mechanical properties ensures the long-term stability of the equipment.

CN119019966APending Publication Date: 2024-11-26UNILUMIN GRP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411172094.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Mini LED displays are prone to excessive humidity in outdoor environments to oxidize and corrode the parts, causing dead lamp failures. The existing glue materials are difficult to meet the requirements of high waterproof performance, affecting the long-lasting stability of the equipment.

Method used

A waterproof epoxy resin glue is used, and its matrix includes hydrophobically modified cycloalienaceous epoxy resin and blended copolymer, combined with a modified amine-based curing agent and nanofiller, through the introduction of hydrophobic groups and the formation of an interpenetrating network Structure, improve the water resistance and mechanical properties of glue.

Benefits of technology

It achieves a balance of high waterproof performance and mechanical properties, ensuring the long-term stability and waterproof effect of Mini LED display in outdoor environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005010300270000011
    Figure BDA0005010300270000011
  • Figure BDA0005010300270000021
    Figure BDA0005010300270000021
  • Figure BDA0005010300270000031
    Figure BDA0005010300270000031
Patent Text Reader

Abstract

The invention provides a waterproof epoxy resin adhesive and a preparation method and application thereof, and provides the waterproof epoxy resin adhesive which comprises the following components in parts by weight: 5-65 parts of matrix resin; 10-30 parts by weight of a curing agent; 1.5 to 10 parts by weight of a toughening agent; 5-15 parts by weight of a filler; the matrix resin comprises an epoxy resin reactive diluent and epoxy resin; the epoxy resin comprises hydrophobic modified alicyclic epoxy resin and / or a blend copolymer; the blend copolymer comprises an alicyclic epoxy resin; the curing agent comprises a modified amine curing agent. Compared with the prior art, the water-resistant epoxy resin has the advantages that hydrophobic groups are introduced into the epoxy resin, or a hydrophobic blending material and the epoxy resin form an interpenetrating network structure through physical action, so that the water resistance of the epoxy resin is improved; the obtained waterproof epoxy resin adhesive has relatively high mechanical property and weather resistance and also has relatively high waterproof performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor packaging, and in particular relates to a waterproof epoxy resin adhesive, a preparation method and application thereof. Background Art

[0002] LED (Light Emitting Diode) has the advantages of high brightness, high efficiency, high reliability, and long life, and is widely used in electronics, lighting, traffic lights and other fields. Mini LED is one of the new improvements in LED technology. Compared with traditional LED, Mini LED has a smaller size (usually less than 0.2 mm), higher brightness, higher contrast and lower power consumption, so it has broad application prospects in the field of Mini LED display.

[0003] In recent years, as LED display products continue to develop towards higher pixel density and smaller pixel pitch, chip-on-board (COB) has become the direction of technological change for small-pitch LED displays. In terms of application scenarios, the scene value of outdoor media is increasingly prominent, and outdoor advertising covers various life and travel scenarios of consumers. Elevator frame media, building TV, cinema media, subway media, etc. can be seen everywhere. In terms of display effect, small-pitch LED displays will achieve higher resolution and more realistic picture effects.

[0004] However, during the use of LED display screens, excessive humidity can easily cause oxidation and corrosion of components such as lamps, PCB boards, power supplies, and power cords, which can lead to dead lamp failures. The waterproofing problem is always a difficult problem in the realization of diversified scenarios for outdoor products. The above problems also put forward higher requirements for the glue materials and process production of Mini-LED. Not only does the process require convenience and speed, but the selection of glue materials also requires excellent waterproof performance. Improving the waterproof performance of glue is a key factor in achieving diversified, long-lasting and stable outdoor screens. Therefore, developing a waterproof glue is of great significance and has broad market prospects. Summary of the invention

[0005] In view of this, the technical problem to be solved by the present invention is to provide a waterproof epoxy resin adhesive, a preparation method and application thereof.

[0006] The present invention provides a waterproof epoxy resin adhesive, comprising:

[0007]

[0008]

[0009] The matrix resin includes epoxy resin reactive diluent and epoxy resin; the epoxy resin includes hydrophobically modified alicyclic epoxy resin and / or blended copolymer; the blended copolymer includes alicyclic epoxy resin;

[0010] The curing agent includes a modified amine curing agent; the modified amine curing agent is obtained by reacting trimethylolpropane and / or a trimethylolpropane derivative with an aromatic amine.

[0011] Preferably, the epoxy resin reactive diluent is selected from polypropylene glycol diglycidyl ether;

[0012] And / or, the hydrophobically modified alicyclic epoxy resin is selected from alicyclic epoxy resins obtained by introducing hydrophobic groups methyl and / or phenyl;

[0013] And / or, the blended copolymer further comprises polyurethane and / or polyacrylate.

[0014] Preferably, the mass ratio of the epoxy resin reactive diluent to the epoxy resin is (2-8):1.

[0015] Preferably, the curing agent further comprises an anhydride curing agent and / or an acrylate curing agent; the mass ratio of the anhydride curing agent and / or the acrylate curing agent to the modified amine curing agent is (0.8-1.5):1.

[0016] Preferably, the trimethylolpropane derivative is selected from cyclotrimethylolpropane formal acrylate and / or cyclotrimethylolpropane formaldehyde;

[0017] And / or, the aromatic amine is selected from one or more of m-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenylmethane and 4,4'-diaminophenylsulfone;

[0018] And / or, the molar ratio of the trimethylolpropane and / or trimethylolpropane derivative to the aromatic amine is 1:1.

[0019] Preferably, the toughening agent is selected from hydrophobic fumed silica and / or a rubber toughening agent; the rubber toughening agent is selected from one or more of liquid polyurethane rubber, polyisobutylene, polybutadiene rubber, butadiene rubber, ethylene-propylene rubber and ethylene-octene copolymer.

[0020] Preferably, the filler is selected from one or more of nano fillers, resin microparticle fillers and blended modified resin microparticle fillers;

[0021] The nano filler is selected from nano silicon dioxide and / or nano aluminum oxide;

[0022] The resin microparticle filler is selected from Japan Sekisui SP-203 and / or Japan Sekisui GS220;

[0023] The blended modified resin microparticle filler is formed by blending a leveling agent with resin microparticles.

[0024] Preferably, including:

[0025]

[0026] The present invention provides a method for preparing the above-mentioned waterproof epoxy resin adhesive, comprising the following steps:

[0027] The epoxy resin active diluent, epoxy resin, curing agent, toughening agent and filler are mixed to obtain waterproof epoxy resin glue.

[0028] The present invention also provides an application of the waterproof epoxy resin adhesive as LED packaging adhesive.

[0029] The present invention provides a waterproof epoxy resin adhesive, comprising: 5 to 65 parts by weight of a base resin; 10 to 30 parts by weight of a curing agent; 1.5 to 10 parts by weight of a toughening agent; 5 to 15 parts by weight of a filler; the base resin comprises an epoxy resin reactive diluent and an epoxy resin; the epoxy resin comprises a hydrophobically modified alicyclic epoxy resin and / or a blended copolymer; the blended copolymer comprises an alicyclic epoxy resin; the curing agent comprises a modified amine curing agent; the modified amine curing agent is obtained by reacting trimethylolpropane and / or a trimethylolpropane derivative with an aromatic amine. Compared with the prior art, the present invention improves the water resistance of the epoxy resin by introducing a hydrophobic group into the epoxy resin or by using a hydrophobic blending material to form an interpenetrating network structure with the epoxy resin through physical action, and at the same time combines the interaction of a specific curing agent and other additives, so that the obtained waterproof epoxy resin adhesive has high mechanical properties and weather resistance as well as high waterproof performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 A schematic diagram of the structure of an LED packaging process provided by the present invention;

[0031] Figure 2 A schematic diagram of the structure of an LED packaging process provided by the present invention;

[0032] Figure 3 This is a photo of the waterproof epoxy resin glue prepared in Example 1 of the present invention;

[0033] Figure 4 is a photo of the waterproof epoxy resin glue prepared in Example 2 of the present invention;

[0034] Figure 5 This is a photo of the waterproof epoxy resin glue prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0036] The present invention provides a waterproof epoxy resin adhesive, comprising:

[0037]

[0038] The matrix resin includes epoxy resin reactive diluent and epoxy resin; the epoxy resin includes hydrophobically modified alicyclic epoxy resin and / or blended copolymer; the blended copolymer includes alicyclic epoxy resin;

[0039] The curing agent includes a modified amine curing agent; the modified amine curing agent is obtained by reacting trimethylolpropane and / or a trimethylolpropane derivative with an aromatic amine.

[0040] According to the present invention, the content of the base resin in the waterproof epoxy resin glue is preferably 10 to 65 parts by weight, more preferably 20 to 65 parts by weight, more preferably 30 to 65 parts by weight, more preferably 40 to 65 parts by weight, more preferably 50 to 65 parts by weight, more preferably 55 to 65 parts by weight, and most preferably 58 to 62 parts by weight; the base resin includes an epoxy resin reactive diluent and an epoxy resin; the mass ratio of the epoxy resin reactive diluent to the epoxy resin is preferably (2 to 8): 1, more preferably (2.5 to 8), and more preferably (2.6 to 8); in the one provided by the present invention In some embodiments, the mass ratio of the epoxy resin reactive diluent to the epoxy resin is specifically 6.25:1, 2.65:1 or 8:1; the epoxy resin reactive diluent is preferably polypropylene glycol diglycidyl ether; the epoxy resin includes hydrophobically modified alicyclic epoxy resin and / or a blended copolymer; the hydrophobically modified alicyclic epoxy resin is preferably an alicyclic epoxy resin obtained by introducing hydrophobic groups methyl and / or phenyl, more preferably an alicyclic epoxy resin modified by methyl methacrylate; the hydrophobic group is introduced into the epoxy resin molecular chain by chemical reaction to make it hydrophobic. The blended copolymer includes alicyclic epoxy resin, and more preferably also includes polyurethane and / or polyacrylate. By blending alicyclic epoxy resin with other polymer materials with good water resistance, an interpenetrating network structure is formed through physical action, thereby improving the water resistance of epoxy resin.

[0041] According to the present invention, the content of the curing agent in the waterproof epoxy resin glue is preferably 15 to 30 parts by weight, more preferably 20 to 30 parts by weight, more preferably 22 to 28 parts by weight, more preferably 23 to 26 parts by weight, and most preferably 24 to 25 parts by weight; the curing agent includes a modified amine curing agent; the modified amine curing agent is obtained by reacting trimethylolpropane and / or trimethylolpropane derivatives with aromatic amines; the trimethylolpropane derivatives are preferably cyclotrimethylolpropane methylal acrylate and / or cyclic trimethylolpropane formaldehyde; the aromatic amine is preferably one or more of metaphenylenediamine, metaphenylenediamine, 4,4'-diaminodiphenylmethane and 4,4'-diaminophenylsulfone; the molar ratio of the trimethylolpropane and / or trimethylolpropane derivatives to the aromatic amine is preferably 1:1; the curing agent Preferably, an anhydride curing agent and / or an acrylate curing agent are also included; the mass ratio of the anhydride curing agent and / or the acrylate curing agent to the modified amine curing agent is preferably (0.8-1.5):1, more preferably (1-1.5):1, more preferably (1-1.3):1, and most preferably (1-1.2):1; in some embodiments provided by the present invention, the mass ratio of the anhydride curing agent and / or the acrylate curing agent to the modified amine curing agent is specifically 1.18:1 or 1.08:1; the anhydride curing agent can be an anhydride curing agent well known to those skilled in the art, and there is no special limitation. In the present invention, it is preferably one or more of maleic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride and methylhexahydrophthalic anhydride; the acrylate curing agent is preferably methyl methacrylate.

[0042] According to the present invention, the content of the toughener in the waterproof epoxy resin glue is preferably 2 to 10 parts by weight, more preferably 4 to 9 parts by weight, more preferably 5 to 8 parts by weight, and most preferably 5.5 to 7 parts by weight; the toughener is preferably hydrophobic fumed silica and / or a rubber toughener, more preferably at least a rubber toughener; the content of the rubber toughener in the toughener is greater than or equal to 70%; the rubber toughener is preferably one or more of liquid polyurethane rubber, polyisobutylene, polybutadiene rubber, butadiene rubber, ethylene-propylene rubber and ethylene-octene copolymer. These tougheners are added to epoxy resins to effectively block water vapor due to their efficient non-water-absorbing properties, while improving the elongation at break, ductility, corrosion resistance, weather resistance and thickening and hydrophobicity of the cured product, achieving a strong ability to resist environmental impact.

[0043] According to the present invention, the content of the filler in the waterproof epoxy resin glue is preferably 6 to 13 parts by weight, more preferably 7 to 12 parts by weight, and even more preferably 7.5 to 11 parts by weight; the filler is preferably one or more of a nanofiller, a resin microparticle filler and a blended modified resin microparticle filler; the nanofiller is preferably nano-silicon dioxide and / or nano-alumina; the resin microparticle filler is preferably one or more of Japan Sekisui SP-203 and Japan Sekisui GS220; the blended modified resin microparticle filler is preferably formed by blending a leveling agent with resin microparticles; the mass ratio of the leveling agent to the resin microparticles is preferably 1:(1 to 2), more preferably 1:(1.3 to 1.8), even more preferably 1:(1.4 to 1.6), and most preferably 1:1.5.

[0044] According to the different fillers, the composition of the waterproof epoxy resin glue has slight differences. In a specific embodiment provided by the present invention, the waterproof epoxy resin glue includes: 5 to 65 parts by weight of base resin; 10 to 25 parts by weight of curing agent; 1.5 to 7 parts by weight of toughening agent; 5 to 15 parts by weight of nano filler. Nanomaterials are one of the new ultra-fine materials. Because of their small particle size and strong surface adsorption, they also take into account stability, reinforcement, thickening and thixotropic properties. In addition, the high specific surface area of ​​nanomaterials themselves can effectively improve the water resistance of epoxy resin.

[0045] In a specific embodiment provided by the present invention, the waterproof epoxy resin glue comprises: 15 to 65 parts by weight of base resin; 10 to 25 parts by weight of curing agent; 1.5 to 5.5 parts by weight of toughening agent; and 5 to 10 parts by weight of resin microparticle filler. Adding resin microparticle materials (such as modified powders SP-203, KJ155, GS220, etc.) to epoxy resin can enhance sealing, water resistance and high heat resistance, reduce stress and give epoxy resin anti-cracking and cold and hot shock capabilities. If cost is considered, domestic resin microparticles are preferred.

[0046] In a specific embodiment provided by the present invention, the waterproof epoxy resin adhesive comprises: 8 to 60 parts by weight of base resin; 15 to 25 parts by weight of curing agent; 1.5 to 5.5 parts by weight of toughening agent; and 5 to 10 parts by weight of blended modified resin microparticle filler.

[0047] In another specific embodiment provided by the present invention, the waterproof epoxy resin adhesive comprises: 58 to 62 parts by weight of base resin; 24 to 25 parts by weight of curing agent; 5.5 to 7 parts by weight of toughening agent; and 7.5 to 11 parts by weight of filler.

[0048] The present invention improves the water resistance of the epoxy resin by introducing hydrophobic groups into the epoxy resin or using hydrophobic blending materials to form an interpenetrating network structure with the epoxy resin through physical action, and at the same time combines with a specific curing agent and other auxiliary agents to interact, so that the obtained waterproof epoxy resin glue has high mechanical properties and weather resistance as well as high waterproof performance.

[0049] The present invention also provides a method for preparing the waterproof epoxy resin glue, comprising the following steps: mixing epoxy resin active diluent, epoxy resin, curing agent, toughening agent and filler to obtain the waterproof epoxy resin glue.

[0050] The present invention has no particular limitation on the sources of all raw materials, and any raw materials available on the market can be used.

[0051] The epoxy resin active diluent, epoxy resin, curing agent, toughening agent and filler are mixed; the mixing speed is preferably 500-1200rpm, more preferably 800-1200rpm, and more preferably 800-1000rpm; the mixing time is preferably 10-60min, more preferably 20-50min, and more preferably 30min; the mixing is preferably carried out at room temperature.

[0052] After mixing, in order to avoid the bubbles generated inside the epoxy glue during the preparation process affecting the mechanical properties of the epoxy glue, a defoaming agent is preferably added; the defoaming agent can be a defoaming agent well known to those skilled in the art, and there is no special limitation. In the present invention, it is preferably a silicone defoaming agent, and more preferably Shin-Etsu model 5680; the mass of the defoaming agent is preferably 1% to 3% of the mass of the waterproof epoxy resin glue.

[0053] Finally, the mixture is preferably filtered to obtain the waterproof epoxy resin glue; the filtration is preferably performed with 100-400 mesh filtration, and more preferably with 200-300 mesh filtration.

[0054] The present invention also provides an application of the waterproof epoxy resin adhesive as LED packaging adhesive.

[0055] Specifically, the LED packaging adhesive is an outdoor LED packaging adhesive.

[0056] The present invention also provides a LED packaging process, such as Figure 1As shown, 1 is a substrate, 2 is a filling glue, 3 is a waterproof epoxy resin glue, 4 is a protective film, 5 is a transparent waterproof matte nano material, and 6 is a waterproof translucent nano material. Specifically, the following steps are included: A1) Encapsulating the LED chip on the substrate; A2) Filling and curing the bottom of the LED chip; A3) Encapsulating the above waterproof epoxy resin glue on the surface for molding, curing, and then sticking a protective film on the surface; A4) Spraying transparent waterproof matte nano material on the surface, and applying waterproof translucent nano material on the side, which can fully achieve the waterproof effect and also prevent scratches. Specifically, the substrate is preferably a PCB substrate; the LED chip is Mini LED chip; the filling is preferably black matrix filling; the filling is preferably one-component epoxy resin; the refractive index of the one-component epoxy resin is preferably 1.52; the curing temperature in step A2) is preferably 140°C to 160°C, more preferably 150°C; the curing time in step A2) is preferably 20 to 40 minutes, more preferably 25 to 35 minutes, and more preferably 30 minutes; chip sealing protection is achieved by filling; the curing temperature in step A3) is preferably 125°C to 135°C; the curing time in step A3) is preferably 3 to 4 hours; secondary sealing by molding and curing waterproof epoxy resin glue can protect against water vapor entry; the transmittance of the cured waterproof epoxy resin glue is preferably 96%; the protective film is preferably an AG film with a transmittance of 55%; after the protective film is attached, it is preferably cut by CNC cutting process, and then a transparent waterproof matte nano material is sprayed on the surface; the transparent waterproof matte nano material is preferably a transparent waterproof matte nano material PC-W102; the waterproof and light-transmitting nano material is preferably PC-WJ103.

[0057] The present invention also provides another LED packaging process, such as Figure 2As shown, 1 is the functional area, 2 is the groove, 3 is the cutting retention colloid, and 4 is the process edge. Specifically, the following steps are included: B1) setting the groove outside the functional area of ​​the substrate; B2) mounting the chip on the back of the substrate and encapsulating the LED chip on the surface; B3) molding and curing the above-mentioned waterproof epoxy resin glue on the surface, and then applying black dam glue on both sides of the groove, curing, and cutting. Among them, the substrate is preferably a PCB substrate; the width of the gong groove is preferably 1-2 cm, more preferably 1.5 cm; the curing temperature of the waterproof epoxy resin glue in the step B3) is preferably 125°C-135°C; the curing time of the waterproof epoxy resin glue is preferably 3-4 hours; the transmittance of the cured waterproof epoxy resin glue is preferably 96%; the curing temperature of the black dam glue is preferably 125°C-135°C; the curing time of the black dam glue is preferably 3-4 hours; the function of the black dam glue is to form a wall, which can prevent the waterproof epoxy resin glue from overflowing; specifically, the black dam glue is cured at the gong groove by GKG equipment; the cutting is preferably carried out 1-1.5 cm outside the functional area, and its function is to leave 1-0.8 cm of waterproof epoxy resin glue, so as to achieve the waterproof effect of the side edge.

[0058] In order to further illustrate the present invention, a waterproof epoxy resin adhesive, a preparation method and an application thereof provided by the present invention are described in detail below in conjunction with embodiments.

[0059] The reagents used in the following examples are all commercially available; the bisphenol A and alicyclic resin copolymer used in the examples is WSR618 (E-51) from Shandong Yousu Chemical Technology Co., Ltd.; methyltetrahydrophthalic anhydride is from Jining Zhongjian Chemical Co., Ltd. (model HY-908); the cyclotrimethylolpropane methyl aromatic amine used in the examples is a compound prepared by reacting trimethylolpropane with aromatic amine in a molar ratio of 1:1; wherein the aromatic amine is Chuzhou Huisheng Electronic Materials (model: 32710B); the hydrophobic alicyclic resin copolymer used is a modified epoxy resin (http: / / www.keningxcl.com / aspcms / productlist / list-126-1.html) from Shanghai Kening New Materials Technology Co., Ltd.; butadiene rubber (model BR9000) is from Yanshan Petrochemical Rubber Chemical Co., Ltd.; ethylene octene copolymer is Dow POE 8180 from the United States; Toyobo polyacrylate is from BASF substrate EFKA FL 3772 from Germany.

[0060] Examples 1 to 3

[0061] Table 1 Formula of Example 1 Waterproof Epoxy Resin Glue

[0062]

[0063]

[0064] Table 2 Formula of Example 2 Waterproof Epoxy Resin Glue

[0065]

[0066] Table 3 Formula of Example 3 Waterproof Epoxy Resin Glue

[0067]

[0068] The selected formula is placed in a reaction container in a certain order, and the use environment of the epoxy resin adhesive is set to stir at room temperature for 30 minutes. Under the control of the stirring instrument, the stirring frequency is set to a fixed speed of 1000 rpm to keep the adhesive in a laminar state; in order to avoid the bubbles generated inside the adhesive during the preparation process affecting the mechanical properties of the adhesive, a defoamer is placed in the stirring container of the epoxy resin adhesive (generally added in an amount of 1% to 3% of the total amount of epoxy resin; after stirring, filter with 200 mesh; finally obtain. Note: The raw material warehouse mixer device is produced in a dark environment.

[0069] The performance of the waterproof epoxy resin glue obtained in Examples 1 to 3 was tested, the test standards are shown in Table 4, and the test results are shown in Tables 5 to 9, wherein the test products in Table 7 are the test data of five cured samples from the same production batch, and Table 8 is the test data of glass + glass cured bonding samples.

[0070] Among them, the transmittance (%T) in Table 7 becomes an important indicator when selecting epoxy glue, because in optoelectronic circuits, optical signals may need to pass through the epoxy glue layer on the bonding interface. The transmittance of the glue is required to be above 90%, and the commonly used detection instrument is measured by a UV-VIS spectrometer (spectrophotometer). The epoxy film is coated on a glass carrier and then cured according to the data sheet conditions. The thickness of the sample is often determined by the overall viscosity, surface tension, and wetting force of the product, and is marked on the light transmittance report curve. The cured sample is sent to a 300nm~2500nm light source (laser), and then a curve of the proportion of light absorbed or transmitted by the material in a specific band is obtained.

[0071] The compressive strength (also called tensile test) in Table 8 can be explained as how many MPa the film is deformed under the action of external force; the elongation at break can be explained as: clamp the two ends of the film there, and then pull it. There is a force when pulling, and it depends on how much force it is pulled to break; Test standard: tensile test and elongation at break test: a. Test equipment: universal tensile testing machine; b. Test method: IS0 527-1:2012&IS0 527-2:2012; c. Sample thickness: 2~4mm; d. Laboratory environmental conditions: 23+2℃, 50±5%RH; e. Qualification standard: The tensile strength of the product epoxy resin glue is greater than 10MPa, and the elongation at break is greater than or equal to 110%; Test standard basis: refer to the national standard GB / T7124-86 "Determination method of tensile shear strength of adhesives".

[0072] Table 4 Testing standards

[0073] Serial number project Standard value 1 Appearance Colorless transparent liquid 2 Cleanliness No visible impurities 3 Viscosity / mPa.s@25℃60R / No.6 6500-7500 4 Hardness / Shore D / @25℃ After centrifugation, dry at 130℃ for 180 minutes 84±5 5 Refractive index / 25℃ 1.567±0.005

[0074] Table 5 Appearance test results

[0075]

[0076]

[0077] Table 6 Hardness test results after curing

[0078] Serial number Test value standard Example 1 83.6D 84D±5 Example 2 84.3D 84D±5 Example 3 84.7D 84D±5

[0079] Table 7 Transmittance test results after curing

[0080] Serial number Test value determination Example 1 91 qualified Example 2 91 qualified Example 3 92 qualified

[0081] Table 8 Mechanical properties test results

[0082] Serial number Test items Test value determination Example 1 Tensile strength(MPa) 12.8 qualified Example 2 Tensile strength(MPa) 13.5 qualified Example 3 Tensile strength(MPa) 14.7 qualified Example 1 Elongation at break (%) 160 qualified Example 2 Elongation at break (%) 158 qualified Example 3 Elongation at break (%) 162 qualified

[0083] Table 9 Reliability test results of waterproof epoxy resin glue

[0084]

[0085]

[0086] It can be seen from Tables 5 to 9 that the product provided by the present invention has passed the reliability test, has better performance and water resistance than similar products, and has better adhesion performance to glass and metal.

[0087] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A waterproof epoxy resin glue, It is characterized in that include: The matrix resin includes epoxy resin reactive diluent and epoxy resin; the epoxy resin includes hydrophobically modified alicyclic epoxy resin and / or blended copolymer; the blended copolymer includes alicyclic epoxy resin; The curing agent includes a modified amine curing agent; the modified amine curing agent is obtained by reacting trimethylolpropane and / or a trimethylolpropane derivative with an aromatic amine.

2. The waterproof epoxy resin glue according to claim 1, It is characterized in that The epoxy resin reactive diluent is selected from polypropylene glycol diglycidyl ether; And / or, the hydrophobically modified alicyclic epoxy resin is selected from alicyclic epoxy resins obtained by introducing hydrophobic groups methyl and / or phenyl; And / or, the blended copolymer further comprises polyurethane and / or polyacrylate.

3. The waterproof epoxy resin glue according to claim 1, It is characterized in that The mass ratio of the epoxy resin active diluent to the epoxy resin is (2-8):

1.

4. The waterproof epoxy resin glue according to claim 1, It is characterized in that The curing agent further comprises anhydride curing agent and / or acrylate curing agent; the mass ratio of the anhydride curing agent and / or acrylate curing agent to the modified amine curing agent is (0.8-1.5):

1.

5. The waterproof epoxy resin glue according to claim 1, It is characterized in that The trimethylolpropane derivative is selected from cyclotrimethylolpropane formal acrylate and / or cyclotrimethylolpropane formaldehyde; And / or, the aromatic amine is selected from one or more of m-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenylmethane and 4,4'-diaminophenylsulfone; And / or, the molar ratio of the trimethylolpropane and / or trimethylolpropane derivative to the aromatic amine is 1:

1.

6. The waterproof epoxy resin glue according to claim 1, It is characterized in that The toughening agent is selected from hydrophobic fumed silica and / or a rubber toughening agent; the rubber toughening agent is selected from one or more of liquid polyurethane rubber, polyisobutylene, polybutadiene rubber, butadiene rubber, ethylene-propylene rubber and ethylene-octene copolymer.

7. The waterproof epoxy resin glue according to claim 1, It is characterized in that The filler is selected from one or more of nano fillers, resin microparticle fillers and blended modified resin microparticle fillers; The nano filler is selected from nano silicon dioxide and / or nano aluminum oxide; The resin microparticle filler is selected from Japan Sekisui SP-203 and / or Japan Sekisui GS220; The blended modified resin microparticle filler is formed by blending a leveling agent with resin microparticles.

8. The waterproof epoxy resin glue according to claim 1, It is characterized in that include:

9. A method for preparing the waterproof epoxy resin adhesive according to claim 1, It is characterized in that The following steps are involved: The epoxy resin active diluent, epoxy resin, curing agent, toughening agent and filler are mixed to obtain waterproof epoxy resin glue.

10. Use of the waterproof epoxy resin glue according to any one of claims 1 to 8 or the waterproof epoxy resin glue prepared by the preparation method according to claim 9 as LED packaging glue.