Epoxy adhesive for bonding bridge segments
By using mixed modulation of components A and components B and chemical synthesis of additives in the epoxy adhesive for bridge segment bonding, the problems of aging and insufficient performance of existing epoxy adhesives are solved, and efficient impact resistance is achieved , fatigue resistance and anti-aging properties ensure the safe and stable use of bridge segments.
Patent Information
- Application Number
- CN202411314436.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing epoxy adhesives for bridge segment bonding are prone to aging, powdering and discoloration after long-term use, which affects the safety of use and lacks effective impact and fatigue resistance.
Using an epoxy adhesive prepared from a mixture of component A and component B, component A includes bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, diluent, toughener and filler, component B includes modification Alicyclic amines and modified fillers, the additive contains benzophenone, hindered phenol and hindered amine structures, and is prepared through chemical reactions and catalytic synthesis to form additives and fillers with excellent anti-thermal oxygen aging and anti-ultraviolet aging properties. Improve the suspension and construction properties of the adhesive.
It realizes the efficient impact resistance, fatigue resistance and aging resistance of epoxy adhesives, extends service life, and improves the safety and stability of bridge segment bonding.
Smart Images

Figure 7ZI7Q7HAFLTAWDV5GNND4KPMKTQ2DROBCBYL0HAG 
Figure LMRJZBV1RDPPTA9VHGIHLAU8CBICMBRK9VGOB7QO 
Figure OTBO8UGNWMNMIGX5EHIE10XQNA3TCAWV0WRDM4AM
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adhesives, and in particular, relates to an epoxy adhesive for bonding bridge segments. Background Art
[0002] Due to its excellent comprehensive properties, epoxy resin is widely used in various fields of the national economy. According to its application method, it can be used as coating, casting material, fiber reinforcement material, adhesive, molding material, injection material and foam material. As an adhesive, epoxy resin is mainly used in transportation, optical instruments, electrical and electronic equipment, civil engineering and mechanical industry, etc. In civil engineering, it is used for fixing concrete prefabricated parts, connecting new and old cement, and repairing roads. Epoxy resin itself is a high molecular prepolymer with a thermoplastic linear structure. It cannot be used directly as an adhesive. It must be added with a curing agent and cured and cross-linked under certain conditions to form an infusible and insoluble body network structure before it can show a series of excellent properties.
[0003] Since segmental prefabricated assembled bridges are mainly used in urban expressway viaducts, light rails, high-speed railways and other fields, and are exposed to wind and sun for a long time, the epoxy adhesive used for bonding bridge segments is very likely to powder and discolor due to aging, which in turn affects the use and even poses a threat to safety. Therefore, it is urgent to design an epoxy adhesive for bonding bridge segments. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide an epoxy adhesive for bonding bridge segments.
[0005] The purpose of the present invention can be achieved through the following technical solutions: The epoxy adhesive used for bonding bridge segments is prepared by mixing component A and component B.
[0006] Furthermore, the component A comprises the following raw materials in parts by weight: 20-40 parts of bisphenol A epoxy resin, 30-50 parts of hydrogenated bisphenol A epoxy resin, 10-20 parts of diluent, 8-20 parts of toughening agent, 75-130 parts of filler, 1-4 parts of auxiliary agent, and 0.1-0.5 parts of defoaming agent.
[0007] Furthermore, the diluent is one or more of ethylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,2-cyclohexanediol diglycidyl ether, butyl glycidyl ether, phenyl glycidyl ether and octyl glycidyl ether.
[0008] Furthermore, the toughening agent is one or more of dibutyl phthalate, dioctyl phthalate, hydroxyl-terminated liquid nitrile rubber, carboxyl-terminated nitrile rubber, and polypropylene glycol diglycidyl ether.
[0009] Furthermore, the filler is a mixture of fumed silica, silicon powder, titanium dioxide and glass fiber in a mass ratio of (1-3):(12-18):(1-3):(1-2).
[0010] The cooperation between fumed silica, silica powder, titanium dioxide and glass fiber can not only ensure the suspension property of component A, facilitate construction, ensure the compressive strength of the system, reduce shrinkage rate, but also make the epoxy adhesive have good impact resistance, fatigue resistance and aging resistance.
[0011] Furthermore, the auxiliary agent is prepared by the following steps: S1. Under nitrogen protection, add 2-hydroxy-4-acryloyloxybenzophenone, DBU (1,8-diazobisspiro[5.4.0]undec-7-ene) and ethanol into a three-necked flask, heat to 40°C, stir to dissolve, and then slowly add 2,2,6,6-tetramethylpiperidinamine. After the addition is complete, heat to 60°C and react for 48 hours. After the reaction is completed, distill under reduced pressure to obtain intermediate 1; the dosage ratio of 2,2,6,6-tetramethylpiperidinamine, 2-hydroxy-4-acryloyloxybenzophenone, DBU and ethanol is 14.7mL:21.5g:2.4mL:180mL; Under the catalytic action of DBU, the molar ratio of 2,2,6,6-tetramethylpiperidinamine and 2-hydroxy-4-acryloxybenzophenone is controlled to be 1.05-1.1:1, and 2,2,6,6-tetramethylpiperidinamine and 2-hydroxy-4-acryloxybenzophenone undergo Michael addition reaction. The reaction process is shown below: S2. Under nitrogen protection, 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, epichlorohydrin and DMF (N,N-dimethylformamide) were added to a three-necked flask, stirred evenly, and then anhydrous concentrated sulfuric acid was slowly added. The mixture was reacted at room temperature for 4 hours, and most of the solvent was removed by rotary evaporation. The mixture was purified by column chromatography (the eluent was a mixed solvent of benzene and ethyl acetate, and the volume ratio of benzene and ethyl acetate was 8:2). The eluent was removed by vacuum distillation to obtain intermediate 2. The dosage ratio of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, epichlorohydrin, anhydrous concentrated sulfuric acid and DMF was 21.4 g:5.5 mL:0.9 mL:130 mL. The molar ratio of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid to epichlorohydrin is controlled to be 1.05-1.1:1, and the carboxyl group of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid undergoes an addition reaction with the epoxy group of epichlorohydrin under the catalysis of concentrated sulfuric acid. The reaction process is as follows: S3. Add intermediate 1, intermediate 2, triethylamine and DMF into a three-necked flask under nitrogen protection, mix and stir evenly, heat to 80°C, keep at 80°C for reaction for 3 hours, cool to room temperature, distill under reduced pressure, purify by column chromatography (the eluent is a mixed solvent of benzene and acetone, the volume ratio of benzene and acetone is 9:1), remove the eluent by distillation under reduced pressure to obtain intermediate 3; the amount ratio of intermediate 1, intermediate 2, triethylamine and DMF is 25.5g:23.4g:12.5mL:200mL; Triethylamine is used as an acid-binding agent to control the molar ratio of intermediate 1 to intermediate 2 to be 1:1.05-1.1, and the -NH- of intermediate 1 and the -Cl of intermediate 2 undergo a nucleophilic substitution reaction. The reaction process is as follows: S4, under nitrogen protection, add intermediate 3, 1,2-bistrimethoxysilylethane and tetraisopropyl titanate into a three-necked flask filled with DMF, heat to 90°C and react for 24 hours, cool to room temperature after the reaction, distill under reduced pressure, wash with anhydrous ethanol 3 times, dry at 80°C for 6 hours, and purify by column chromatography (the eluent is a mixed solvent of chloroform and ether, and the volume ratio of chloroform and ether is 9:1), and finally distill under reduced pressure to remove the eluent to obtain intermediate 4; the amount ratio of intermediate 3, 1,2-bistrimethoxysilylethane, tetraisopropyl titanate and DMF is 22.8g:8.2mL:0.26g:180mL; The molar ratio of intermediate 3 and 1,2-bistrimethoxysilylethane is controlled to be 1:1.05-1.1. Then, under the catalysis of tetraisopropyl titanate, the hydroxyl group of intermediate 3 and the silyloxy group of 1,2-bistrimethoxysilylethane undergo the following chemical reaction. The reaction process is shown below: S5. Under nitrogen protection, add intermediate 4, glycidol and tetraisopropyl titanate into a three-necked flask containing DMF, heat to 100°C and react for 24 hours. After the reaction, cool to room temperature, distill under reduced pressure, wash with anhydrous ethanol three times, dry at 80°C for 12 hours, and purify by column chromatography (the eluent is a mixed solvent of benzene and ether, and the volume ratio of benzene and ether is 6:4). Finally, distill under reduced pressure to remove the eluent to obtain an auxiliary agent; the amount ratio of intermediate 4, glycidol, tetraisopropyl titanate and DMF is 21.5g:1.5g:0.17g:180mL.
[0012] The molar ratio of intermediate 4 to glycidol is controlled to be 1.05-1.1:1. Under the catalytic action of tetraisopropoxytitanium, the silanoloxy group of intermediate 4 and the hydroxyl group of glycidol undergo the following chemical reaction. The reaction process is shown below: The auxiliary agent contains benzophenone structure, hindered phenol structure and hindered amine structure. The benzophenone structure can absorb high-energy ultraviolet light, convert light energy into heat energy for release, or convert it into other harmless energy forms for release, and play a role in ultraviolet absorption; the hindered phenol structure is limited by steric barriers because the hydroxyl group is restricted, and the hydrogen atom is easy to fall off from the original molecular structure, thereby achieving the effect of donating protons and combining with peroxyl radicals, alkyl radicals, hydroxyl radicals, etc., causing them to lose their original activity, resulting in the termination of the oxygen aging reaction; the hindered amine structure achieves light protection effect by capturing free radicals, decomposing hydroperoxides, quenching singlet oxygen and capturing heavy metal ions, and the hindered amine structure has high light stabilization efficiency. The three structures work synergistically, so that the auxiliary agent of the present invention has excellent anti-thermal oxygen aging effect and anti-ultraviolet aging effect.
[0013] The additive contains multiple lipophilic benzene rings and heterocyclic rings, which effectively increase the compatibility between the additive and the other raw materials and preliminarily improve the dispersion of the additive; the additive also contains silaneoxy groups, which can form chemical bonds with the hydroxyl groups on the surface of the filler in component A, which further improves the dispersion of the additive, thereby allowing the additive to maximize its anti-thermal oxidative aging and anti-ultraviolet aging effects, and allows the filler to be evenly dispersed in component A, giving full play to the synergistic effect, increasing the suspension of component A, facilitating construction, and at the same time improving the impact strength and fatigue resistance of the epoxy adhesive.
[0014] Furthermore, the defoaming agent is one or both of BYK-A530 and BYK-065.
[0015] Furthermore, the B component comprises the following raw materials in parts by weight: 25-40 parts of modified alicyclic amine, 0.05-2 parts of curing accelerator, and 66-110 parts of modified filler.
[0016] Furthermore, the curing accelerator is one or more of 2,4,6-tris(dimethylaminomethyl)phenol, triethylamine, methylimidazole, triethanolamine, and DBU.
[0017] Furthermore, the modified filler is prepared by the following steps: Add inorganic filler and deionized water into a three-necked flask, adjust the pH value to 5 with concentrated hydrochloric acid, stir and heat to 55-75°C, then slowly add coupling agent KH-540 (3-aminopropyltrimethoxysilane), stir for 10 hours after the addition is completed, cool to room temperature, filter, wash with anhydrous ethanol 3-5 times, and after washing, vacuum dry the product at 80°C for 12 hours to obtain a modified filler; the mass ratio of the modified filler to the coupling agent KH-540 is 20:1.
[0018] Furthermore, the inorganic filler is a mixture of fumed silica, silicon powder and carbon black in a mass ratio of (1-3):(12-18):(0.2-1).
[0019] The trimethoxysilane on the coupling agent KH-540 can be hydrolyzed and then condensed to form Si-O-Si and Si-OH; the -OH in Si-OH can form a hydrogen bond with the -OH on the surface of the inorganic filler, and then dehydrate and condense to form a covalent bond, thereby significantly reducing the surface energy of the modified filler. The modified filler can also be highly dispersed in component B, ensuring that component B has suspension properties, facilitating construction, ensuring the compressive strength of the system, and reducing shrinkage.
[0020] Rich amino groups are introduced on the surface of the modified filler of component B, and the auxiliary agent of component A contains epoxy groups, and the epoxy groups and amino groups can be cured at room temperature. Therefore, the auxiliary agent of component A can react chemically with the modified alicyclic amine and the modified filler in component B, and the modified filler of component B can react chemically with the epoxy resin and auxiliary agent of component A. Therefore, the auxiliary agent, filler and modified filler of the present invention can be highly dispersed and stably present in the epoxy adhesive, giving full play to their own functions, so that the epoxy adhesive has excellent and stable resistance to thermal oxidation aging and ultraviolet aging, and at the same time has strong impact resistance and fatigue resistance, and can be used as an epoxy adhesive for bonding bridge segments.
[0021] Furthermore, the mass ratio of component A to component B is (2.5-3.5):1.
[0022] Beneficial effects of the present invention: the epoxy adhesive of the present invention is prepared by mixing component A and component B, the auxiliary agent containing benzophenone structure, hindered phenol structure and hindered amine structure in component A has chemical reaction with the filler in component A, the modified filler and modified alicyclic amine in component B, and the modified filler in component B has chemical reaction with the auxiliary agent in component A and epoxy resin, therefore, the auxiliary agent and filler and modified filler of the present invention can be highly dispersed and stably present in the epoxy adhesive, fully exerting their functions, thereby giving the epoxy adhesive excellent and stable resistance to thermal oxidation aging and ultraviolet aging as well as impact resistance. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Example 1 The specific steps for preparing the additive in component A are as follows: S1. Under nitrogen protection, add 21.5 g of 2-hydroxy-4-acryloyloxybenzophenone, 2.4 mL of DBU and 180 mL of ethanol into a 500 mL three-necked flask, heat to 40 °C, stir to dissolve, and then slowly add 14.7 mL of 2,2,6,6-tetramethylpiperidinamine. After the addition is complete, heat to 60 °C and react for 48 hours. After the reaction is completed, distill under reduced pressure to obtain intermediate 1; S2, under nitrogen protection, 21.4 g of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, 5.5 mL of epichlorohydrin and 130 mL of DMF were added to a 250 mL three-necked flask, stirred evenly, and then 0.9 mL of anhydrous concentrated sulfuric acid was slowly added, reacted at room temperature for 4 h, most of the solvent was removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of benzene and ethyl acetate, and the volume ratio of benzene and ethyl acetate was 8:2), and the eluent was removed by reduced pressure distillation to obtain intermediate 2; S3, under nitrogen protection, add 25.5 g of intermediate 1, 23.4 g of intermediate 2, 12.5 mL of triethylamine and 200 mL of DMF into a 500 mL three-necked flask, mix and stir evenly, heat to 80° C., keep at 80° C. for reaction for 3 h, cool to room temperature, distill under reduced pressure, purify by column chromatography (the eluent is a mixed solvent of benzene and acetone, the volume ratio of benzene to acetone is 9:1), and remove the eluent by reduced pressure distillation to obtain intermediate 3; S4, under nitrogen protection, add 22.8g of intermediate 3, 8.2mL of 1,2-bistrimethoxysilylethane and 0.26g of tetraisopropyl titanate into a 500mL three-necked flask filled with 180mL of DMF, heat to 90°C and react for 24h, cool to room temperature after the reaction, distill under reduced pressure, wash with anhydrous ethanol 3 times, dry at 80°C for 6h, and purify by column chromatography (the eluent is a mixed solvent of chloroform and ether, and the volume ratio of chloroform to ether is 9:1), and finally remove the eluent by distillation under reduced pressure to obtain intermediate 4; S5. Under nitrogen protection, 21.5 g of intermediate 4, 1.5 g of propylene oxide and 0.17 g of tetraisopropyl titanate were added to a 500 mL three-necked flask containing 180 mL of DMF, and the temperature was raised to 100 ° C for reaction for 24 h. After the reaction, it was cooled to room temperature and distilled under reduced pressure. The mixture was washed with anhydrous ethanol for 3 times, dried at 80 ° C for 12 h, and purified by column chromatography (the eluent was a mixed solvent of benzene and ether, and the volume ratio of benzene and ether was 6:4). Finally, the eluent was removed by distillation under reduced pressure to obtain an auxiliary agent.
[0025] Example 2 The modified filler in component B is prepared in the following specific steps: 2 g of fumed silica, 24 g of silicon powder, 0.4 g of carbon black and 200 mL of deionized water were added to a 500 mL three-necked flask, and the pH value was adjusted to 5 with concentrated hydrochloric acid. The mixture was heated to 55 °C with stirring, and 1.32 g of coupling agent KH-540 was slowly added. After the addition was completed, the mixture was stirred for 10 h, cooled to room temperature, filtered, and washed with anhydrous ethanol for 3 times. After washing, the product was vacuum dried at 80 °C for 12 h to obtain a modified filler.
[0026] Example 3 The modified filler in component B is prepared in the following specific steps: 4 g of fumed silica, 30 g of silicon powder, 1 g of carbon black and 200 mL of deionized water were added to a 500 mL three-necked flask, and the pH value was adjusted to 5 with concentrated hydrochloric acid. The mixture was heated to 75 °C with stirring, and 1.75 g of coupling agent KH-540 was slowly added. After the addition was completed, the mixture was stirred for 10 h, cooled to room temperature, filtered, and washed with anhydrous ethanol for 4 times. After washing, the product was vacuum dried at 80 °C for 12 h to obtain a modified filler.
[0027] Example 4 The modified filler in component B is prepared in the following specific steps: 6 g of fumed silica, 36 g of silicon powder, 2 g of carbon black and 200 mL of deionized water were added to a 500 mL three-necked flask, and the pH value was adjusted to 5 with concentrated hydrochloric acid. The mixture was heated to 65 °C with stirring, and 2.2 g of coupling agent KH-540 was slowly added. After the addition was completed, the mixture was stirred for 10 h, cooled to room temperature, filtered, and washed with anhydrous ethanol for 5 times. After washing, the product was vacuum dried at 80 °C for 12 h to obtain a modified filler.
[0028] Example 5 The epoxy adhesive is prepared in the following steps: Preparation of component A: 20 parts by weight of bisphenol A epoxy resin, 30 parts by weight of hydrogenated bisphenol A epoxy resin, 5 parts by weight of neopentyl glycol diglycidyl ether, 5 parts by weight of butyl glycidyl ether, 8 parts by weight of dibutyl phthalate, 5 parts by weight of fumed silica, 60 parts by weight of silicon powder, 5 parts by weight of titanium dioxide, 3 parts by weight of glass fiber, 1 part by weight of the auxiliary agent prepared in Example 1, and 0.1 part by weight of defoamer BYK-A530 were added into a stirring tank and mixed thoroughly for 1 hour to obtain component A; Preparation of component B: 25 parts of modified alicyclic amine IP43, 0.025 parts of methylimidazole, 0.025 parts of triethanolamine, and 66 parts of the modified filler prepared in Example 2 were added into a stirring tank and mixed thoroughly for 1 hour to prepare component B; Component A and component B are mixed and modulated at a mass ratio of 2.5:1 to obtain an epoxy adhesive.
[0029] Example 6 The epoxy adhesive is prepared in the following steps: Preparation of component A: 40 parts by weight of bisphenol A epoxy resin, 50 parts by weight of hydrogenated bisphenol A epoxy resin, 10 parts by weight of 1,4-butanediol diglycidyl ether, 10 parts by weight of phenyl glycidyl ether, 20 parts by weight of hydroxy-terminated liquid nitrile rubber, 15 parts by weight of fumed silica, 90 parts by weight of silica powder, 15 parts by weight of titanium dioxide, 10 parts by weight of glass fiber, 4 parts by weight of the additive prepared in Example 1, and 0.5 parts by weight of defoamer BYK-065 were added to a stirring tank and mixed thoroughly for 3 hours to obtain component A; Preparation of component B: 40 parts by weight of modified alicyclic amine IP43, 1 part of 2,4,6-tris(dimethylaminomethyl)phenol, 1 part of DBU, and 110 parts of the modified filler prepared in Example 3 were added into a stirred tank and mixed thoroughly for 3 hours to prepare component B; Component A and component B are mixed and modulated at a mass ratio of 3.5:1 to obtain an epoxy adhesive.
[0030] Example 7 The epoxy adhesive is prepared in the following steps: Preparation of component A: 38 parts of bisphenol A epoxy resin, 45 parts of hydrogenated bisphenol A epoxy resin, 10 parts of 1,2-cyclohexanediol diglycidyl ether, 9 parts of octyl glycidyl ether, 18 parts of polypropylene glycol diglycidyl ether, 14 parts of fumed silica, 85 parts of silicon powder, 13 parts of titanium dioxide, 8 parts of glass fiber, 3.8 parts of the additive prepared in Example 1, and 0.4 parts of defoamer BYK-A530 were added into a stirring tank and mixed thoroughly for 2 hours to prepare component A; Preparation of component B: 38 parts by weight of modified alicyclic amine IP98, 1.9 parts of triethylamine, and 105 parts of the modified filler prepared in Example 4 were added into a stirred tank and mixed thoroughly for 2 hours to prepare component B; Component A and component B are mixed and modulated in a mass ratio of 3:1 to obtain an epoxy adhesive.
[0031] Comparative Example 1 The specific steps for preparing the additive in component A are as follows: The remaining steps remain unchanged, and step S5 of Example 1 is removed to prepare the auxiliary agent.
[0032] Comparative Example 2 The epoxy adhesive is prepared in the following steps: The remaining steps remain unchanged, and the auxiliary agent in Example 7 is replaced by the auxiliary agent prepared in Comparative Example 1, thereby preparing an epoxy adhesive.
[0033] Comparative Example 3 The epoxy adhesive is prepared in the following steps: The remaining steps remained unchanged, except that the auxiliary agent in Example 7 was replaced by 1.2 parts of antioxidant 1010, 1.3 parts of ultraviolet absorber UV-531 and 1.3 parts of light stabilizer 744, thereby preparing an epoxy adhesive.
[0034] Comparative Example 4 The epoxy adhesive is prepared in the following steps: The remaining steps remain unchanged, and the auxiliary agent of Example 7 is removed to prepare the epoxy adhesive.
[0035] Performance Testing The epoxy adhesives prepared in Examples 5-7 and Comparative Examples 2-4 were tested for compressive strength, standard value of steel-to-steel tensile shear strength, resistance to long-term stress, resistance to wet and hot aging, and heat aging according to the Technical Specifications for Safety Appraisal of Engineering Structure Reinforcement Materials GB50728-2011; and the bonding time was tested according to the Epoxy Adhesive for Prefabricated Segment Assembly T / CECS10080-2020. The test results are shown in Table 1 below: Table 1 In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0036] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. Epoxy adhesive for bonding bridge segments, characterized in that: The invention is prepared by mixing component A and component B; the component A comprises the following raw materials by weight: 20-40 parts of bisphenol A epoxy resin, 30-50 parts of hydrogenated bisphenol A epoxy resin, 10-20 parts of diluent, 8-20 parts of toughening agent, 75-130 parts of filler, 1-4 parts of auxiliary agent, and 0.1-0.5 parts of defoamer; the component B comprises the following raw materials by weight: 25-40 parts of modified alicyclic amine, 0.05-2 parts of curing accelerator, and 66-110 parts of modified filler; Wherein, the auxiliary agent is prepared by the following steps: S1. Add 2-hydroxy-4-acryloyloxybenzophenone, DBU and ethanol into a flask under nitrogen protection, heat to 40°C with stirring, add 2,2,6,6-tetramethylpiperidinamine, react at 60°C for 48h, and after the reaction is completed, distill under reduced pressure to obtain intermediate 1; S2, under nitrogen protection, 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, epichlorohydrin and DMF were added to a flask, and concentrated sulfuric acid was added after stirring. The mixture was reacted at room temperature for 4 h, and then rotary evaporated, purified by column chromatography, and distilled under reduced pressure to obtain intermediate 2; S3, under nitrogen protection, add intermediate 1, intermediate 2, triethylamine and DMF into a flask, stir, react at 80°C for 3h, distill under reduced pressure, purify by column chromatography, and distill under reduced pressure to obtain intermediate 3; S4, under nitrogen protection, add intermediate 3, 1,2-bistrimethoxysilylethane and tetraisopropyl titanate into a flask containing DMF, react at 90°C for 24h, cool, distill under reduced pressure, wash, dry, purify by column chromatography, and distill under reduced pressure to obtain intermediate 4; S5. Under nitrogen protection, add intermediate 4, propylene oxide and tetraisopropyl titanate into a flask containing DMF, react at 100° C. for 24 h, cool, distill under reduced pressure, wash, dry, purify by column chromatography, and distill under reduced pressure to obtain an auxiliary agent.
2. The epoxy adhesive for bonding bridge segments according to claim 1, characterized in that: The modified filler is prepared by the following steps: Add inorganic filler and deionized water into a flask, adjust the pH value to 5, heat to 55-75°C, add coupling agent KH-540, stir for 10 hours, cool, filter, wash and dry to obtain a modified filler.
3. The epoxy adhesive for bonding bridge segments according to claim 1, characterized in that: The amount ratio of 2,2,6,6-tetramethylpiperidinamine, 2-hydroxy-4-acryloxybenzophenone, DBU and ethanol in step S1 is 14.7mL:21.5g:2.4mL:180mL; the amount ratio of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, epichlorohydrin, anhydrous concentrated sulfuric acid and DMF in step S2 is 21.4g:5.5mL:0.9mL:130mL; the intermediate 1 in step S3, The amount ratio of intermediate 2, triethylamine and DMF is 25.5g:23.4g:12.5mL:200mL; the amount ratio of intermediate 3, 1,2-bistrimethoxysilylethane, tetraisopropyl titanate and DMF in step S4 is 22.8g:8.2mL:0.26g:180mL; the amount ratio of intermediate 4, glycidol, tetraisopropyl titanate and DMF in step S5 is 21.5g:1.5g:0.17g:180mL.
4. The epoxy adhesive for bonding bridge segments according to claim 2, characterized in that: The inorganic filler is a mixture of fumed silica, silicon powder and carbon black in a mass ratio of (1-3):(12-18):(0.2-1); the mass ratio of the modified filler to the coupling agent KH-540 is 20:
1.
5. The epoxy adhesive for bonding bridge segments according to claim 1, characterized in that: The mass ratio of component A to component B is (2.5-3.5):
1.
6. The epoxy adhesive for bonding bridge segments according to claim 1, characterized in that: The diluent is one or more of ethylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,2-cyclohexanediol diglycidyl ether, butyl glycidyl ether, phenyl glycidyl ether and octyl glycidyl ether.
7. The epoxy adhesive for bonding bridge segments according to claim 1, characterized in that: The toughening agent is one or more of dibutyl phthalate, dioctyl phthalate, hydroxyl-terminated liquid nitrile rubber, carboxyl-terminated nitrile rubber, and polypropylene glycol diglycidyl ether.
8. The epoxy adhesive for bonding bridge segments according to claim 1, characterized in that: The filler is a mixture of fumed silica, silicon powder, titanium dioxide and glass fiber in a mass ratio of (1-3):(12-18):(1-3):(1-2).
9. The epoxy adhesive for bonding bridge segments according to claim 1, characterized in that: The defoaming agent is one or both of BYK-A530 and BYK-065.
10. The epoxy adhesive for bonding bridge segments according to claim 1, characterized in that: The curing accelerator is one or more of 2,4,6-tris(dimethylaminomethyl)phenol, triethylamine, methylimidazole, triethanolamine and DBU.