Nano-emulsion energy storage medium as well as preparation method and application thereof

The high-concentration nanoemulsion of nanoparticles made of hot melt paraffin has solved the problem that drilling fluid is difficult to cool under high temperature conditions, and achieved rapid and effective cooling and improved stability of drilling fluid.

CN119019989APending Publication Date: 2024-11-26SINOPEC OILFIELD SERVICE CORPORATION +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310594973.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

It is difficult for existing drilling fluid to cool quickly and effectively under high temperature conditions, resulting in an increase in the underground temperature and affecting drilling efficiency and equipment stability. Traditional water and air cooling technologies have problems such as low efficiency and large equipment volume.

Method used

Paraffin is encapsulated into submicron particles by hot melting method, and nanoparticles are made by colloidal milling. It combines non-ionic surfactant to form a high concentration nanoemulsion, with high phase change latent heat and stability, and is used for rapid cooling of drilling fluid.

Benefits of technology

The rapid cooling of drilling fluid is achieved, the cooling efficiency and stability are improved, and the cooling amplitude can reach more than 20.0%, avoiding the problems of large equipment size and low efficiency in traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004246821430000021
    Figure BDA0004246821430000021
Patent Text Reader

Abstract

The invention provides a nano-emulsion energy storage medium as well as a preparation method and application thereof. The polyvinyl alcohol / paraffin composite core material comprises the following components in parts by mass: 80-120 parts of polyvinyl alcohol / paraffin composite core material; 3 to 6 parts by mass of a Span surfactant; 6 to 9 parts by mass of a Tween surfactant; 1-3 parts by mass of a benzyl quaternary ammonium salt surfactant; and 1-300 parts by mass of water. Paraffin is packaged into submicron particles with polyvinyl alcohol through a hot melting method, the submicron particles are ground into nano particles through a colloid mill, finally the nano particles are concentrated into high-concentration nano emulsion, the emulsion has high heat storage efficiency, and the purpose of rapidly reducing the temperature of the drilling fluid can be achieved by circulating a high-concentration energy storage material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of drilling fluid, and in particular relates to a nano-emulsion energy storage medium and a preparation method and application thereof. Background Art

[0002] At present, the global demand for energy is becoming more and more vigorous, especially in the oil and gas industry. In the process of oil and gas development, shallow development has been almost exhausted, and gradually moving towards deep layers. The temperature of the formation encountered by drilling is getting higher and higher, and the temperature of the underground circulating drilling fluid is also getting higher and higher. In this case, the temperature resistance of the drilling fluid has been increasingly challenged, especially various treatment agents may break the chain, side reactions, etc. at high temperatures, resulting in deterioration of the drilling fluid performance. At the same time, under current technical conditions, in order to improve the drilling efficiency during directional well and horizontal well drilling, it is generally necessary to assemble short sections such as rotary guide near the drill bit to achieve rapid drilling in the directional stage. However, since the main accessories in these instruments are precision electronic components, they may be overloaded or have reduced tolerance under high temperature conditions, causing instrument failure, resulting in immeasurable losses.

[0003] To this end, drilling engineers began to look for ways to reduce the underground temperature of drilling fluid. One method is to simply add newly formulated fluid to achieve the purpose of cooling. The second method is to add a certain amount of energy storage material to the drilling fluid, stimulate the energy storage under certain temperature conditions underground, and release the energy through a cooling device after returning to the ground, thereby achieving the purpose of cooling. However, these two methods require too high a content of components to be added to achieve better results. For example, energy storage materials generally need to be added to the drilling fluid at a rate of more than 30% to reduce the circulating temperature of the drilling fluid by 20°C, which will lead to an increase in the overall amount of drilling fluid and will also have a certain impact on the performance of the drilling fluid.

[0004] Another method is to cool the ground by preparing a cooling water circulation system and an air refrigeration system on the ground to cool the drilling fluid. However, due to the poor heat storage effect of water, a large heat exchange area is required to achieve a certain cooling effect, which leads to a large volume of the heat exchange coil and a long ground circulation time. For example, invention patent 200510038602.7 proposes a method for making microcapsules from phase change energy storage materials, using tetradecane or pentadecane as an organic phase change material, and using a mixture of natural gum and gum arabic to make an outer capsule to form a phase change material with a phase change temperature of 5 to 12°C. Tetradecane or pentadecane is easy to deform at high temperatures and absorbs relatively low heat. Another example is invention patent 201611184478.X discloses a composite phase change material and its preparation method. It includes an organic phase change material and an inorganic carrier, wherein the organic phase change material fills the pores of the inorganic carrier, the organic phase change material is polyethylene glycol, the inorganic carrier is expanded graphite, and the mass ratio of polyethylene glycol to the expanded graphite is 11.5:1. It is a solid phase change material, not a phase change fluid.

[0005] Therefore, there is a need to seek a more efficient ground energy storage fluid to improve heat storage and heat exchange capabilities. Summary of the invention

[0006] The purpose of the present invention is to meet the demand for cooling the drilling fluid at the well site outlet and to solve the defect that the currently commonly used water cooling and air cooling technologies are difficult to cool quickly and effectively. The present invention mainly uses polyvinyl alcohol to encapsulate paraffin into submicron particles by a hot melt method, grinds it into nanoparticles using a colloid mill, and finally concentrates it into a high-concentration nanoemulsion. The emulsion has a high heat storage efficiency and can achieve the purpose of quickly reducing the temperature of the drilling fluid by circulating the high-concentration energy storage material.

[0007] In the first aspect, the present invention provides a nanoemulsion energy storage medium, the components of which include:

[0008]

[0009] As a specific embodiment of the present invention, the volume concentration of the nanoemulsion energy storage medium is 70% to 90%; the phase change latent heat is 201 J / g to 212 J / g, and the phase change temperature is 35° C. to 49° C.

[0010] As a specific embodiment of the present invention, the nanoemulsion energy storage medium is positively charged, +30mV to +60mV,

[0011] As a specific embodiment of the present invention, the particle size of the polyvinyl alcohol / paraffin composite core material is 200nm-400nm, wherein the particle size of the inner core paraffin is 150nm-300nm, and the thickness of the outer polyvinyl alcohol wall is 50nm-100nm.

[0012] As a specific embodiment of the present invention, the Span surfactant is a sorbitan fatty acid ester, a nonionic surfactant, preferably one of Span20, Span40, Span60, Span80, Span85 or a combination of any two thereof; and / or,

[0013] As a specific embodiment of the present invention, the Tween surfactant is polyoxyethylene sorbitan fatty acid ester, a non-ionic surfactant, preferably one of Tween 20, Tween 40, Tween 60, Tween 80, Tween 85 or a combination of any two thereof; and / or,

[0014] As a specific embodiment of the present invention, the benzyl quaternary ammonium salt surfactant is one or a combination of any two of dodecyl dimethyl benzyl ammonium chloride, tetradecyl dimethyl benzyl ammonium chloride, hexadecyl dimethyl benzyl ammonium chloride, octadecyl dimethyl benzyl ammonium chloride, dodecyl dimethyl benzyl ammonium bromide, tetradecyl dimethyl benzyl ammonium bromide, hexadecyl dimethyl benzyl ammonium bromide and octadecyl dimethyl benzyl ammonium bromide.

[0015] As a specific embodiment of the present invention, the preparation method of the polyvinyl alcohol / paraffin composite core material comprises: mixing polyvinyl alcohol and paraffin under high temperature conditions and granulating them.

[0016] As a specific embodiment of the present invention, the mixing conditions include: temperature of 150°C to 180°C, stirring speed of 1000rpm to 3000rpm, stirring time of 30min to 60min;

[0017] As a specific embodiment of the present invention, the granulation temperature is 80 to 100°C.

[0018] As a specific embodiment of the present invention, the molecular formula of the polyvinyl alcohol is [C2H4O]n, wherein n is the degree of polymerization, preferably n is 5000 to 7000;

[0019] As a specific embodiment of the present invention, the paraffin is a mixture of hydrocarbons with a carbon number ranging from 18 to 30, with a straight-chain alkane content exceeding 90%, preferably one of 52#, 54#, 56#, 58# or a combination of any two thereof.

[0020] In a second aspect, the present invention provides a method for preparing the nanoemulsion energy storage medium described in the first aspect, comprising the following steps:

[0021] S1: mixing and dispersing deionized water and polyvinyl alcohol / paraffin composite core material to obtain a first mixture;

[0022] S2: adding a Span surfactant to the first mixture obtained in step S1 and mixing to obtain a second mixture;

[0023] S3: adding Tween surfactant to the second mixture obtained in step S2 for emulsification reaction to obtain a third mixture;

[0024] S4: adding a benzyl quaternary ammonium salt surfactant to the third mixture obtained in step S3 to react to obtain a fourth mixture;

[0025] S5: Evaporating the fourth mixture obtained in step S4 to obtain a nanoemulsion energy storage medium.

[0026] As a specific embodiment of the present invention, in step S1, the mixing conditions include: temperature of 80°C to 90°C, stirring rate of 1000rpm to 3000rpm, stirring time of 50min to 80min; the mass ratio of deionized water to polyvinyl alcohol / paraffin composite core material is (3-8):1.

[0027] As a specific embodiment of the present invention, in step S2, the mixing conditions include: temperature of 80°C to 90°C, stirring rate of 1000rpm to 3000rpm, stirring time of 20min to 30min; the amount of the Span surfactant added is 2.5-7.5% of the total mass of the polyvinyl alcohol / paraffin composite core material.

[0028] As a specific embodiment of the present invention, in step S3, the mixing conditions include: temperature of 80°C to 90°C, stirring rate of 15000rpm to 20000rpm, reaction time of 60min to 90min; the amount of Tween surfactant added is 5-11.25% of the total mass of the polyvinyl alcohol / paraffin composite core material.

[0029] As a specific embodiment of the present invention, in step S4, the mixing conditions include: temperature of 80°C to 90°C, stirring rate of 15000rpm to 20000rpm, stirring time of 60min to 90min; the amount of the benzyl quaternary ammonium salt surfactant added is 0.83-3.75% of the total mass of the polyvinyl alcohol / paraffin composite core material;

[0030] As a specific implementation of the present invention, in the step S5, the evaporation conditions include: the evaporation temperature is 60° C. to 80° C., and the evaporation to a volume concentration of 70% to 90%.

[0031] As a specific embodiment of the present invention, the Span surfactant is a sorbitan fatty acid ester, a non-ionic surfactant, preferably one of Span20, Span40, Span60, Span80, Span85 or a combination of any two thereof.

[0032] As a specific embodiment of the present invention, the Tween surfactant is polyoxyethylene sorbitan fatty acid ester, a non-ionic surfactant, preferably one of Tween 20, Tween 40, Tween 60, Tween 80, Tween 85 or a combination of any two thereof.

[0033] As a specific embodiment of the present invention, the benzyl quaternary ammonium salt surfactant is one or a combination of any two of dodecyl dimethyl benzyl ammonium chloride, tetradecyl dimethyl benzyl ammonium chloride, hexadecyl dimethyl benzyl ammonium chloride, octadecyl dimethyl benzyl ammonium chloride, dodecyl dimethyl benzyl ammonium bromide, tetradecyl dimethyl benzyl ammonium bromide, hexadecyl dimethyl benzyl ammonium bromide and octadecyl dimethyl benzyl ammonium bromide.

[0034] As a specific embodiment of the present invention, the nanoemulsion energy storage medium obtained by the present invention has strong Ostwald ripening stability, and the particle size change rate after standing for half a year is less than 2.5%.

[0035] The above raw materials in the present invention can be prepared in-house or commercially available, and the present invention is not particularly limited thereto.

[0036] In a third aspect, the present invention provides an application of the nanoemulsion energy storage medium described in the first aspect or the nanoemulsion energy storage medium prepared by the preparation method described in the second aspect in the field of rapid cooling of drilling fluid surface.

[0037] As a specific embodiment of the present invention, the nanoemulsion energy storage medium needs to be preheated and pre-stirred before being used in the drilling fluid field, with the temperature raised to 60°C to 80°C, the stirring speed being 100rpm to 300rpm, and the stirring time being 5min to 20min.

[0038] As a specific embodiment of the present invention, the nanoemulsion energy storage medium is directly pumped into the circulating cooling pipeline at the drilling fluid site, and a condenser is connected to the rear end of the circulating pipeline. The cooling medium of the condenser is Freon. After heat exchange, the core material of the droplets in the highly concentrated nanoemulsion energy storage medium restores the internal crystal state, and continues to circulate several times to achieve the purpose of rapid cooling of the drilling fluid ground.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] 1. The present invention uses polyvinyl alcohol to encapsulate paraffin into submicron particles through a hot-melt method to form a composite energy storage core with a high phase change potential (>200 J / g).

[0041] 2. Use a colloid mill to grind it into nanoparticles, use a composite non-ionic surfactant to emulsify it, use a rigid benzyl cationic quaternary ammonium salt surfactant to stabilize the emulsion, and finally concentrate it into a high-concentration nanoemulsion. The emulsion has excellent stability, uniform heat storage, and high heat storage efficiency. DETAILED DESCRIPTION

[0042] The present invention will be further described below in conjunction with specific embodiments, but they do not constitute any limitation to the present invention.

[0043] Example 1

[0044] This embodiment provides a nanoemulsion energy storage medium and a preparation method thereof, the specific details of which are as follows:

[0045] Preparation of polyvinyl alcohol / paraffin composite core material:

[0046] 1) Add 1000g polyvinyl alcohol ([C2H4O] number average molecular weight is 5000) into a closed autoclave, raise the system temperature to 150°C, adjust the stirring speed to 1000rpm, slowly add 300g 52# paraffin wax, add it over 25min, and stir and disperse it at high speed for 30min;

[0047] 2) After the reaction is completed, the mixture is transferred to an extrusion drying granulator while still hot (temperature>80°C), and the granular material with a particle size of 0.1mm to 0.3mm is finally obtained, which is the polyvinyl alcohol / paraffin composite core material.

[0048] Preparation of highly concentrated nanoemulsion energy storage medium:

[0049] 1) Add 4000 g of deionized water and 800 g of polyvinyl alcohol / paraffin composite core material to a colloid mill, raise the temperature of the colloid mill to 80° C., and disperse at a speed of 1000 rpm for 50 min;

[0050] 2) Add 30 g of Span20 into the above reactor at one time and continue to disperse for 20 minutes;

[0051] 3) Rapidly increase the stirring speed of the above reactor to 15000 rpm, then slowly add 60 g of Tween 20 within 25 min, and continue the emulsification reaction until the emulsion returns a uniform blue light. The reaction is completed within 60 min;

[0052] 4) Add 10 g of dodecyl dimethyl benzyl ammonium chloride to the above reactor and continue the reaction for 60 min;

[0053] 5) After the reaction is completed, the system is transferred to a high-temperature rotary evaporator in batches, and the water is rotary evaporated at 60°C for 20 minutes. The obtained thick blue fluid is the highly concentrated nano energy storage material.

[0054] Example 2

[0055] This embodiment provides a nanoemulsion energy storage medium and a preparation method thereof, the specific details of which are as follows:

[0056] Preparation of polyvinyl alcohol / paraffin composite core material:

[0057] 1) Add 1250g of polyvinyl alcohol ([C2H4O] number average molecular weight is 6000) into a closed autoclave, raise the system temperature to 160°C, adjust the stirring speed to 2000rpm, slowly add 400g of 54# paraffin wax, add it over 30 minutes, and stir and disperse it at high speed for 40 minutes;

[0058] 2) After the reaction is completed, the mixture is transferred to an extrusion drying granulator while still hot (temperature>80°C), and the granular material with a particle size of 0.1mm to 0.3mm is finally obtained, which is the polyvinyl alcohol / paraffin composite core material.

[0059] Preparation of highly concentrated nanoemulsion energy storage medium:

[0060] 1) Add 5000 g of deionized water and 1000 g of polyvinyl alcohol / paraffin composite core material to a colloid mill, raise the temperature of the colloid mill to 90° C., and disperse at a speed of 2000 rpm for 60 min;

[0061] 2) Add 40 g of Span40 into the above reactor at one time and continue to disperse for 30 minutes;

[0062] 3) Rapidly increase the stirring speed of the reactor to 18000 rpm, then slowly add 70 g of Tween 40 within 35 min, and continue the emulsification reaction until the emulsion returns a uniform blue light. The reaction is completed within 70 min;

[0063] 4) Add 20 g of tetradecyl dimethyl benzyl ammonium chloride into the above reactor and continue the reaction for 70 min;

[0064] 5) After the reaction is completed, the system is transferred to a high-temperature rotary evaporator in batches, and the water is rotary evaporated at 70°C for 30 minutes. The obtained thick blue fluid is the highly concentrated nano energy storage material.

[0065] Example 3

[0066] This embodiment provides a nanoemulsion energy storage medium and a preparation method thereof, the specific details of which are as follows:

[0067] Preparation of polyvinyl alcohol / paraffin composite core material:

[0068] 1) Add 1500g of polyvinyl alcohol ([C2H4O] number average molecular weight is 7000) into a closed autoclave, raise the system temperature to 170°C, adjust the stirring speed to 3000rpm, slowly add 500g of 56# paraffin wax, add it over 30min, and stir and disperse it at high speed for 50min;

[0069] 2) After the reaction is completed, the mixture is transferred to an extrusion drying granulator while still hot (temperature>80°C), and the granular material with a particle size of 0.1mm to 0.3mm is finally obtained, which is the polyvinyl alcohol / paraffin composite core material.

[0070] Preparation of highly concentrated nanoemulsion energy storage medium:

[0071] 1) Add 6000 g of deionized water and 1200 g of polyvinyl alcohol / paraffin composite core material to the colloid mill in sequence, raise the temperature of the colloid mill to 90° C., and disperse at a speed of 3000 rpm for 70 min;

[0072] 2) Add 50 g of Span60 into the above reactor at one time and continue to disperse for 30 minutes;

[0073] 3) Rapidly increase the stirring speed of the reactor to 20,000 rpm, then slowly add 80 g of Tween 60 within 50 min, and continue the emulsification reaction until the emulsion returns a uniform blue light. The reaction is completed within 80 min;

[0074] 4) Add 20 g of hexadecyl dimethyl benzyl ammonium chloride into the above reactor and continue the reaction for 80 min;

[0075] 5) After the reaction is completed, the system is transferred to a high-temperature rotary evaporator in batches, and the water is rotary evaporated at 80°C for 30 minutes. The obtained thick blue fluid is the highly concentrated nano energy storage material.

[0076] Example 4

[0077] This embodiment provides a nanoemulsion energy storage medium and a preparation method thereof, the specific details of which are as follows:

[0078] Preparation of polyvinyl alcohol / paraffin composite core material:

[0079] 1) Add 1500g of polyvinyl alcohol ([C2H4O] number average molecular weight is 5000) into a closed autoclave, raise the system temperature to 180°C, adjust the stirring speed to 3000rpm, slowly add 500g of 58# paraffin wax, add it over 30 minutes, and stir and disperse it at high speed for 60 minutes;

[0080] 2) After the reaction is completed, the mixture is transferred to an extrusion drying granulator while still hot (temperature>80°C), and the granular material with a particle size of 0.1mm to 0.3mm is finally obtained, which is the polyvinyl alcohol / paraffin composite core material.

[0081] Preparation of highly concentrated nanoemulsion energy storage medium:

[0082] 1) Add 6000 g of deionized water and 1200 g of polyvinyl alcohol / paraffin composite core material to a colloid mill, raise the temperature of the colloid mill to 90° C., and disperse at a speed of 3000 rpm for 80 min;

[0083] 2) Add 60 g of Span80 into the above reactor at one time and continue to disperse for 30 minutes;

[0084] 3) Rapidly increase the stirring speed of the reactor to 20,000 rpm, then slowly add 90 g of Tween 80 within 50 min, and continue the emulsification reaction until the emulsion returns a uniform blue light. The reaction is completed within 90 min;

[0085] 4) Add 30 g of octadecyl dimethyl benzyl ammonium chloride into the above reactor and continue the reaction for 90 min;

[0086] 5) After the reaction is completed, the system is transferred to a high-temperature rotary evaporator in batches, and the water is rotary evaporated at 80°C for 30 minutes. The obtained thick blue fluid is the highly concentrated nano energy storage material.

[0087] Example 5

[0088] This embodiment provides a nanoemulsion energy storage medium and a preparation method thereof, the specific details of which are as follows:

[0089] Preparation of polyvinyl alcohol / paraffin composite core material:

[0090] 1) Add 1500g of polyvinyl alcohol ([C2H4O] number average molecular weight is 6000) into a closed autoclave, raise the system temperature to 180°C, adjust the stirring speed to 3000rpm, slowly add 500g of 52# paraffin wax, add it over 30 minutes, and stir and disperse it at high speed for 60 minutes;

[0091] 2) After the reaction is completed, the mixture is transferred to an extrusion drying granulator while still hot (temperature>80°C), and the granular material with a particle size of 0.1mm to 0.3mm is finally obtained, which is the polyvinyl alcohol / paraffin composite core material.

[0092] Preparation of highly concentrated nanoemulsion energy storage medium:

[0093] 1) Add 6000 g of deionized water and 1200 g of polyvinyl alcohol / paraffin composite core material to a colloid mill, raise the temperature of the colloid mill to 90° C., and disperse at a speed of 3000 rpm for 80 min;

[0094] 2) Add 60g of Span85 into the above reactor at one time and continue to disperse for 30 minutes;

[0095] 3) Rapidly increase the stirring speed of the reactor to 20,000 rpm, then slowly add 90 g of Tween 85 within 50 min, and continue the emulsification reaction until the emulsion returns a uniform blue light. The reaction is completed within 90 min;

[0096] 4) Add 30 g of dodecyl dimethyl benzyl ammonium bromide into the above reactor and continue the reaction for 90 min;

[0097] 5) After the reaction is completed, the system is transferred to a high-temperature rotary evaporator in batches, and the water is rotary evaporated at 80°C for 30 minutes. The obtained thick blue fluid is the highly concentrated nano energy storage material.

[0098] Example 6

[0099] This embodiment provides a nanoemulsion energy storage medium and a preparation method thereof, the specific details of which are as follows:

[0100] Preparation of polyvinyl alcohol / paraffin composite core material:

[0101] 1) Add 1500g of polyvinyl alcohol ([C2H4O] number average molecular weight is 7000) into a closed autoclave, raise the system temperature to 180°C, adjust the stirring speed to 3000rpm, slowly add 500g of 54# paraffin wax, add it over 30 minutes, and stir and disperse it at high speed for 60 minutes;

[0102] 2) After the reaction is completed, the mixture is transferred to an extrusion drying granulator while still hot (temperature>80°C), and the granular material with a particle size of 0.1mm to 0.3mm is finally obtained, which is the polyvinyl alcohol / paraffin composite core material.

[0103] Preparation of highly concentrated nanoemulsion energy storage medium:

[0104] 1) Add 6000 g of deionized water and 1200 g of polyvinyl alcohol / paraffin composite core material to a colloid mill, raise the temperature of the colloid mill to 90° C., and disperse at a speed of 3000 rpm for 80 min;

[0105] 2) Add 60g of Span20 into the above reactor at one time and continue to disperse for 30 minutes;

[0106] 3) Rapidly increase the stirring speed of the reactor to 20,000 rpm, then slowly add 90 g of Tween 20 within 50 min, and continue the emulsification reaction until the emulsion returns a uniform blue light. The reaction is completed within 90 min;

[0107] 4) Add 30 g of hexadecyl dimethyl benzyl ammonium bromide into the above reactor and continue the reaction for 90 min;

[0108] 5) After the reaction is completed, the system is transferred to a high-temperature rotary evaporator in batches, and the water is rotary evaporated at 80°C for 30 minutes. The obtained thick blue fluid is the highly concentrated nano energy storage material.

[0109] Example 7

[0110] This embodiment provides a nanoemulsion energy storage medium and a preparation method thereof, the specific details of which are as follows:

[0111] Preparation of polyvinyl alcohol / paraffin composite core material:

[0112] 1) Add 1500g of polyvinyl alcohol ([C2H4O] number average molecular weight is 6000) into a closed autoclave, raise the system temperature to 180°C, adjust the stirring speed to 3000rpm, slowly add 500g of 56# paraffin wax, add it over 30 minutes, and stir and disperse it at high speed for 60 minutes;

[0113] 2) After the reaction is completed, the mixture is transferred to an extrusion drying granulator while still hot (temperature>80°C), and the granular material with a particle size of 0.1mm to 0.3mm is finally obtained, which is the polyvinyl alcohol / paraffin composite core material.

[0114] Preparation of highly concentrated nanoemulsion energy storage medium:

[0115] 1) Add 6000 g of deionized water and 1200 g of polyvinyl alcohol / paraffin composite core material to a colloid mill, raise the temperature of the colloid mill to 90° C., and disperse at a speed of 3000 rpm for 80 min;

[0116] 2) Add 60 g of Span60 into the above reactor at one time and continue to disperse for 30 minutes;

[0117] 3) Rapidly increase the stirring speed of the reactor to 20,000 rpm, then slowly add 90 g of Tween 60 within 50 min, and continue the emulsification reaction until the emulsion returns a uniform blue light. The reaction is completed within 90 min;

[0118] 4) Add 30 g of octadecyl dimethyl benzyl ammonium bromide into the above reactor and continue the reaction for 90 min;

[0119] 5) After the reaction is completed, the system is transferred to a high-temperature rotary evaporator in batches, and the water is rotary evaporated at 80°C for 30 minutes. The obtained thick blue fluid is the highly concentrated nano energy storage material.

[0120] Test Case

[0121] (1) Phase transition temperature test: The DSC curve is obtained by measuring the heating curve and the cooling curve. According to the regulations of the ICTA Standardization Committee, the upward DSC curve is an exothermic peak and the downward DSC curve is an endothermic peak. The intersection of the extension line of the front baseline and the tangent line at the maximum slope of the peak front is the melting point. The crystallization peak of melting and recrystallization is taken as the characteristic peak for analysis to obtain the phase transition temperature, phase transition latent heat and other thermophysical parameters.

[0122] (2) Cooling efficiency test: Hot water (90°C, pipe diameter 10 cm, displacement 30 L / s) is passed through the pipes used. The condenser is arranged in a winding manner. Different fluids are passed through the pipes to test the temperature difference between the inlet and outlet of the pipes. The cooling efficiency is obtained by dividing the temperature difference by the initial temperature.

[0123] This test example tests the phase change temperature and cooling efficiency of the nanoemulsion energy storage medium of Examples 1-7, and compares them with conventional water cooling and air cooling. The results are shown in Table 1.

[0124] Table 1 Phase transition temperature and cooling efficiency of different systems

[0125] Test fluid Phase transition temperature, °C Cooling efficiency, % Example 1 26 22.1 Example 2 28 24.5 Example 3 32 25.7 Example 4 35 27.6 Example 5 29 24.8 Example 6 26 22.4 Example 7 27 23.9 Water Cooling — 12.5 Air Cooling — 6.9

[0126] From the results in Table 1, it can be seen that the cooling effects of conventional water cooling and air cooling are both lower than 15.0%, while the use of energy storage medium can greatly improve the cooling effect of the system, and the cooling efficiency is increased to a certain extent, and the cooling range is above 20.0%.

[0127] In summary, the nanoemulsion energy storage medium of the present invention uses polyvinyl alcohol to encapsulate paraffin into submicron particles by a hot-melt method to form a composite energy storage core with high phase change potential (>200 J / g); a colloid mill is used to grind it into nanoparticles, and a composite non-ionic surfactant is used for emulsification, and a benzyl cationic quaternary ammonium salt surfactant with strong rigidity is used to stabilize the emulsion, and finally concentrated into a high-concentration nanoemulsion, the emulsion has excellent stability, uniform heat storage, and high heat storage efficiency.

[0128] Any numerical value mentioned in the present invention, if there is only an interval of two units between any minimum value and any maximum value, includes all values ​​from the minimum value to the maximum value each time increasing by one unit. For example, if the amount of a component, or the value of a process variable such as temperature, pressure, time, etc. is declared to be 50-90, in this specification it means that 51-89, 52-88... and 69-71 and 70-71 are specifically listed. For non-integer values, 0.1, 0.01, 0.001 or 0.0001 can be appropriately considered as a unit. These are just some specially specified examples. In this application, in a similar manner, all possible combinations of numerical values ​​between the listed minimum and maximum values ​​are considered to have been disclosed.

[0129] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.

Claims

1. A nanoemulsion energy storage medium, characterized in that: Its components include: 80-120 parts by weight of polyvinyl alcohol / paraffin composite core material; 3-6 parts by weight of Span surfactant; 6-9 parts by weight of Tween surfactant; 1-3 parts by weight of benzyl quaternary ammonium salt surfactant; Water 1-300 parts by mass.

2. The nanoemulsion energy storage medium according to claim 1, characterized in that: The nanoemulsion energy storage medium has a volume concentration of 70% to 90%, a phase change latent heat of 201 J / g to 212 J / g, and a phase change temperature of 35°C to 49°C. The nanoemulsion energy storage medium is positively charged, +30mV to +60mV.

3. The nanoemulsion energy storage medium according to claim 1 or 2, characterized in that: The particle size of the polyvinyl alcohol / paraffin composite core material is 200nm-400nm, wherein the particle size of the inner core paraffin is 150nm-300nm, and the thickness of the outer polyvinyl alcohol wall is 50nm-100nm.

4. The nanoemulsion energy storage medium according to any one of claims 1 to 3, characterized in that: The Span surfactant is a sorbitan fatty acid ester, preferably one of Span20, Span40, Span60, Span80, Span85 or a combination of any two thereof; and / or, The Tween surfactant is polyoxyethylene sorbitan fatty acid ester, preferably one of Tween 20, Tween 40, Tween 60, Tween 80, Tween 85 or a combination of any two thereof; and / or, The benzyl quaternary ammonium salt surfactant is one or a combination of any two of dodecyl dimethyl benzyl ammonium chloride, tetradecyl dimethyl benzyl ammonium chloride, hexadecyl dimethyl benzyl ammonium chloride, octadecyl dimethyl benzyl ammonium chloride, dodecyl dimethyl benzyl ammonium bromide, tetradecyl dimethyl benzyl ammonium bromide, hexadecyl dimethyl benzyl ammonium bromide and octadecyl dimethyl benzyl ammonium bromide.

5. The nanoemulsion energy storage medium according to any one of claims 1 to 4, characterized in that: The preparation method of the polyvinyl alcohol / paraffin composite core material comprises: mixing polyvinyl alcohol and paraffin under high temperature conditions and granulating them; Preferably, the mixing conditions include: a temperature of 150°C to 180°C, a stirring speed of 1000 rpm to 3000 rpm, a stirring time of 30 min to 60 min; and a granulation temperature of 80 to 100°C.

6. The nanoemulsion energy storage medium according to claim 5, characterized in that: The molecular formula of the polyvinyl alcohol is [C2H4O]n, wherein n is the degree of polymerization, preferably n is 5000 to 7000; The paraffin wax is a mixture of hydrocarbons with a carbon number ranging from 18 to 30, with a straight-chain alkane content exceeding 90%, preferably one of 52#, 54#, 56#, 58# or a combination of any two thereof.

7. A method for preparing the nanoemulsion energy storage medium according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1: mixing and dispersing deionized water and polyvinyl alcohol / paraffin composite core material to obtain a first mixture; S2: adding a Span surfactant to the first mixture obtained in step S1 and mixing to obtain a second mixture; S3: adding Tween surfactant to the second mixture obtained in step S2 for emulsification reaction to obtain a third mixture; S4: adding a benzyl quaternary ammonium salt surfactant to the third mixture obtained in step S3 to react to obtain a fourth mixture; S5: Evaporating the fourth mixture obtained in step S4 to obtain a nanoemulsion energy storage medium.

8. The preparation method according to claim 7, characterized in that: In the step S1, the mixing conditions include: a temperature of 80°C to 90°C, a stirring rate of 1000rpm to 3000rpm, and a stirring time of 50min to 80min; a mass ratio of the deionized water to the polyvinyl alcohol / paraffin composite core material of (3-8): 1; And / or, in step S2, the mixing conditions include: temperature of 80°C to 90°C, stirring rate of 1000rpm to 3000rpm, stirring time of 20min to 30min; the amount of the Span surfactant added is 2.5-7.5% of the total mass of the polyvinyl alcohol / paraffin composite core material; And / or, in step S3, the mixing conditions include: temperature of 80°C to 90°C, stirring rate of 15000rpm to 20000rpm, reaction time of 60min to 90min; the amount of Tween surfactant added is 5-11.25% of the total mass of the polyvinyl alcohol / paraffin composite core material; And / or, in step S4, the mixing conditions include: temperature of 80°C to 90°C, stirring rate of 15000rpm to 20000rpm, stirring time of 60min to 90min; the amount of the benzyl quaternary ammonium salt surfactant added is 0.83-3.75% of the total mass of the polyvinyl alcohol / paraffin composite core material; And / or, in the step S5, the evaporation conditions include: the evaporation temperature is 60° C. to 80° C., and the evaporation to a volume concentration of 70% to 90%.

9. The preparation method according to claim 7 or 8, characterized in that: The Span surfactant is a sorbitan fatty acid ester, preferably one of Span20, Span40, Span60, Span80, Span85 or a combination of any two thereof; and / or, The Tween surfactant is polyoxyethylene sorbitan fatty acid ester, preferably one of Tween 20, Tween 40, Tween 60, Tween 80, Tween 85 or a combination of any two thereof; and / or, The benzyl quaternary ammonium salt surfactant is one or a combination of any two of dodecyl dimethyl benzyl ammonium chloride, tetradecyl dimethyl benzyl ammonium chloride, hexadecyl dimethyl benzyl ammonium chloride, octadecyl dimethyl benzyl ammonium chloride, dodecyl dimethyl benzyl ammonium bromide, tetradecyl dimethyl benzyl ammonium bromide, hexadecyl dimethyl benzyl ammonium bromide and octadecyl dimethyl benzyl ammonium bromide.

10. Use of the nanoemulsion energy storage medium according to any one of claims 1 to 6 or the nanoemulsion energy storage medium prepared by the preparation method according to any one of claims 7 to 9 in the field of rapid cooling of drilling fluid surface.