Mixed molten salt heat storage and heat transfer material and preparation method thereof
By using ionic liquid modified expanded graphite and modified carbon powder in molten salt heat transfer materials, a double-shell structure is formed, which solves the problems of molten salt leakage and low thermal conductivity at high temperatures, and achieves more efficient Heat storage and heat transfer properties.
Patent Information
- Application Number
- CN202411117412.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Molten salt heat storage and heat transfer materials are prone to leakage and corrosion at high temperatures, and have low thermal conductivity, which limits their large-scale application.
Ionic liquid modified expanded graphite is used as the inner shell material to coat the molten salt core body, and combined with modified carbon powder and composite modified boron nitride nanosheets to form a mixed molten salt heat storage and heat transfer material with a double-shell structure to improve heat conductivity Performance and prevent leakage.
It effectively prevents molten salt leakage, improves the thermal conductivity and specific heat capacity of heat storage and heat transfer materials, extends the service life and reduces the cost of use.
Smart Images

Figure CN119019995A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of physical heat transfer energy storage, and in particular to a mixed molten salt heat storage and heat transfer material and a preparation method thereof. Background Art
[0002] For a long time, people have been hoping to replace some fossil fuels with solar energy to reduce carbon emissions and protect the environment. An important way to utilize solar energy is to convert it into thermal energy, which is what we call solar thermal power generation. In this technology, the thermal energy from solar energy can be stored or transmitted to the power generation system to generate electricity, which constitutes a clean and efficient way to utilize solar energy and provides a potential solution to human energy needs in the future. Heat transfer and heat storage media are the main components of solar thermal power generation systems. Among various heat storage media, molten salts are considered to be ideal media for storing and transmitting thermal energy due to their wide operating temperature range, high thermal energy storage density, chemical stability and low melt viscosity. At present, nitrates, chlorides and carbonates are widely used molten salts. Among them, carbonates have the characteristics of low saturated vapor pressure and high working limit temperature, and are the heat storage materials for the next generation of thermal power plants. However, the inherent problems of molten salts such as easy leakage and corrosion of equipment after melting, small specific heat capacity and low thermal conductivity have greatly limited their large-scale application. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a method for preparing a mixed molten salt heat storage and heat transfer material, comprising the following steps:
[0004] Step (1) modifying expanded graphite with 1-butyl-3-methylimidazolium hexafluorophosphate ionic liquid to obtain ionic liquid modified expanded graphite;
[0005] Step (2) treating the molten salt mixture to prepare a molten salt core, and coating the molten salt core with ionic liquid modified expanded graphite as an inner shell material to obtain a core-shell molten salt composite sphere;
[0006] The molten salt mixture includes lithium carbonate, sodium carbonate, potassium carbonate and modified carbon powder;
[0007] The modified carbon powder is obtained by oxidizing the cathode product obtained by electrolysis of carbon dioxide in a molten carbonate electrolyte;
[0008] Step (3) adding urea to treat the hexagonal boron nitride nanosheets during the ball milling process to obtain highly exfoliated hexagonal boron nitride nanosheets;
[0009] Step (4) treating the highly exfoliated hexagonal boron nitride nanosheets with polydopamine to obtain modified boron nitride nanosheets; in-situ growing nanosilver on the modified boron nitride nanosheets to obtain silver-doped modified boron nitride nanosheets;
[0010] Step (5) treating the silver-doped modified boron nitride nanosheets with vinyltriethoxysilane to obtain composite modified boron nitride nanosheets;
[0011] Step (6) uses core-shell molten salt composite balls, composite modified boron nitride nanosheets, and styrene monomer as main raw materials to prepare a mixed molten salt heat storage and heat transfer material.
[0012] Preferably, in the step (1), the preparation method of the ionic liquid modified expanded graphite is as follows: the expanded graphite is mixed with 1-butyl-3-methylimidazolium hexafluorophosphate ionic liquid and ethanol, and ultrasonically dispersed at 30-40kHz for 100-150min, filtered and dried at 60-70°C to constant weight to obtain the ionic liquid modified expanded graphite; the mass ratio of the expanded graphite to the 1-butyl-3-methylimidazolium hexafluorophosphate ionic liquid and ethanol is 1:(0.8-1.1):(2-4);
[0013] In the above process, the ionic liquid is adsorbed on the surface of the expanded graphite through conjugated bonds and van der Waals forces to obtain ionic liquid modified expanded graphite. The thermal conductivity of the modified expanded graphite is improved and the surface energy is reduced.
[0014] Preferably, in step (2), the preparation method of the core-shell molten salt composite sphere is:
[0015] The molten salt mixture is mixed with ethanol, and after ultrasonic vibration treatment for 10-30 minutes, the resulting mixture is pressed into a spherical mold with a diameter of 10 mm at 18-22 MPa by cold isostatic pressing to obtain a spherical core material, and the spherical core material is sintered at 580-620° C. for 100-150 minutes to obtain a molten salt core body, wherein the mass ratio of the molten salt mixture to ethanol is 1:(0.1-0.15); the ionic liquid modified expanded graphite is mixed with an ethanol solution of 25-50wt% polyvinyl pyrrolidone to obtain an inner shell material, and the coating thickness is controlled to be 1.2-1.8mm to coat the inner shell material on the molten salt core body, and then cold isostatic pressing is performed at 18-22 MPa, and finally sintering in air at 430-470° C. for 100-150 minutes to obtain a core-shell molten salt composite ball; the mass ratio of the ionic liquid modified expanded graphite to the ethanol solution of polyvinyl pyrrolidone is 1:(0.1-0.2);
[0016] In the above process, polyvinyl pyrrolidone is dissolved in ethanol as a binder for the inner shell material, which can be removed in the subsequent sintering process. The surface energy of the expanded graphite modified by the ionic liquid is lower, which shows better hydrophobicity, further reducing the wettability with the molten salt, making it more difficult for the molten salt to penetrate into the expanded graphite shell, thereby avoiding the leakage of the molten salt. On the other hand, the hydrophobically modified expanded graphite can also prevent the core-shell molten salt composite ball from being wetted or dissolved by water during the subsequent treatment process.
[0017] Preferably, in step (2), the method for preparing the molten salt mixture comprises the following steps:
[0018] Step A1, lithium carbonate, sodium carbonate, and potassium carbonate are mixed in a mass ratio of (40-47): (30-33): (23-27), heated to 280-320 ° C and maintained for 20-28 hours to remove moisture from the carbonate, and then heated to 720-780 ° C at a heating rate of 3-5 ° C / min, and maintained for 5-6 hours to completely melt the molten salt to obtain a molten mixed molten salt; the molten mixed molten salt is cooled to 430-470 ° C and used as an electrolyte, a platinum-plated titanium plate is used as an anode, and a nickel sheet is used as a cathode, and in a carbon dioxide atmosphere, at 40-60 mA / cm 2 Electrolyze for 100-150 minutes, reverse the cathode with carbon deposited after the electrolysis to an anode, and oxidize for 15-30 minutes at a current of 0.4-0.6A. After the reaction is completed, remove the product on the anode, wash it with a 0.8-1.2 mol / L hydrochloric acid aqueous solution, dry it, and grind it to obtain modified carbon powder;
[0019] In the above process, carbon dioxide is captured during electrolysis to generate carbonate ions, and the carbonate ions are electrolyzed at the cathode to generate carbon. The anode produces oxygen as a by-product, and then the cathode is reversed to the anode. The carbon is in an oxygen-rich atmosphere, resulting in in-situ oxygen doping and the introduction of oxygen functional groups, thereby obtaining modified carbon powder rich in oxygen functional groups. The more oxygen functional groups on the surface of the modified carbon powder, the better the wettability with the molten carbonate, thereby improving the dispersion uniformity of the modified carbon powder in the molten salt.
[0020] Step A2, lithium carbonate, sodium carbonate and potassium carbonate are mixed, heated to 480-520°C at a heating rate of 3-5°C / min and maintained for 5-6h, then modified carbon powder is added, argon is introduced at a flow rate of 180-220mL / min, stirred and mixed in an argon atmosphere for 100-150min, cooled to room temperature, and ground to obtain a molten salt mixture; wherein the mass ratio of lithium carbonate, sodium carbonate, potassium carbonate and modified carbon powder is (40-47):(30-33):(23-27):(0.03-0.07);
[0021] In the above process, the well-dispersed modified carbon powder can form more uniform semi-solid layers and thermal conductive grids in the molten carbonate. The formation of the semi-solid layer can increase the specific heat capacity of the molten salt system, while the formation of the thermal conductive network improves the thermal conductivity of the molten salt and increases the thermal conductivity coefficient.
[0022] Furthermore, in step A1, the size of the platinum-plated titanium plate is 20 mm×20 mm×1 mm, the thickness of the platinum layer is 0.01 mm, and the size of the nickel sheet is 40 mm×30 mm×0.1 mm.
[0023] Preferably, in the step (3), the preparation method of the highly exfoliated hexagonal boron nitride nanosheets is as follows: the hexagonal boron nitride nanosheets are mixed with urea, ground at 400-500 r / min for 10-14 h, then heated to 530-570° C. at a heating rate of 3-5° C. / min and maintained for 3.5-4.5 h, cooled to room temperature, and ground to obtain highly exfoliated hexagonal boron nitride nanosheets; wherein the mass ratio of the hexagonal boron nitride nanosheets to the urea is 1:(8-10);
[0024] In the above process, boron nitride nanosheets are exfoliated and dispersed by ball milling, and urea is introduced during the ball milling process to aminize the unsaturated boron on the surface of the hexagonal boron nitride nanosheets to obtain amino-functionalized highly exfoliated hexagonal boron nitride nanosheets. The exfoliated boron nitride nanosheets are functionalized to reduce the aggregation of the nanosheets and improve the efficiency of subsequent treatment.
[0025] Preferably, in step (4), the preparation method of the silver-doped modified boron nitride nanosheets is:
[0026] The highly exfoliated hexagonal boron nitride nanosheets, Tris buffer and ethanol are mixed, ultrasonically treated for 20-40 minutes, and then dopamine hydrochloride is added, stirred and reacted at 23-28°C for 10-14 hours, filtered, and the filtered product is washed with ethanol to obtain modified boron nitride nanosheets, wherein the amount ratio of the highly exfoliated hexagonal boron nitride nanosheets, Tris buffer, ethanol and dopamine hydrochloride is (10-15) g: (250-500) mL: (80-200) mL: (4-6) g; 2 wt% N,N-dimethylformamide dispersion of modified boron nitride nanosheets is mixed with 2 wt% nitric acid; The invention discloses a method for preparing a silver-doped boron nitride nanosheet by mixing a mixed solution of N,N-dimethylformamide with silver nitrate, ultrasonically treating the mixture for 10-20 minutes, adding a 15 mg / mL sodium borohydride aqueous solution, heating the mixture to 55-65° C., and reacting the mixture for 5.5-6.5 hours at a stirring speed of 500-700 r / min. After the reaction is completed, the mixture is filtered, and the filtered product is washed with ethanol and then dried to obtain a silver-doped modified boron nitride nanosheet. The volume ratio of the N,N-dimethylformamide dispersion of the modified boron nitride nanosheet, the N,N-dimethylformamide of silver nitrate, and the sodium borohydride aqueous solution is (250-400):(50-80):(100-160).
[0027] In the above process, dopamine self-polymerizes into polydopamine, and polydopamine is non-covalently bonded to highly exfoliated hexagonal boron nitride nanosheets through π-π stacking to obtain modified boron nitride nanosheets. More amino groups and hydroxyl groups are introduced on the surface of the boron nitride nanosheets, and more silver can be adsorbed during the growth of nanosilver particles, thereby increasing the growth and deposition amount of nanosilver of the boron nitride nanosheets. The presence of nanosilver can reduce the interfacial thermal resistance between the boron nitride nanosheets and significantly improve the thermal conductivity of the boron nitride nanosheets.
[0028] Preferably, in the step (5), the preparation method of the composite modified boron nitride nanosheets is as follows: silver-doped modified boron nitride nanosheets are dispersed in ethanol, ultrasonically dispersed for 100-150 minutes, then vinyl triethoxysilane is added, stirred for 10-20 minutes, and then ammonia water is added, stirred for reaction at room temperature for 7-9 hours, centrifuged, washed, and dried to obtain composite modified boron nitride nanosheets; wherein the amount ratio of silver-doped modified boron nitride nanosheets, ethanol, vinyl triethoxysilane, and ammonia water is (1-2) g: (250-500) mL: (5-10) mL: (5-10) mL;
[0029] In the above process, silanol formed after hydrolysis of vinyltriethoxysilane reacts with hydroxyl groups in the silver-doped modified boron nitride nanosheets, thereby introducing carbon-carbon double bonds on the surface of the silver-doped modified boron nitride nanosheets.
[0030] Preferably, in the step (6), the preparation method of the mixed molten salt heat storage and heat transfer material is as follows: core-shell molten salt composite balls, composite modified boron nitride nanosheets, water and potassium persulfate are mixed, and ultrasonicated to obtain an aqueous phase; styrene monomer and sodium dioctyl sulfosuccinate are mixed to obtain an oil phase; the aqueous phase is heated to 55-65°C, and the oil phase is added to the aqueous phase within 15-25 minutes to obtain a mixed solution; the mixed solution is mixed under stirring conditions of 500-600r / min for 100-150min, polymerized at 55-65°C for 11-13h, filtered, washed, and dried to obtain a mixed molten salt heat storage and heat transfer material; wherein the mass ratio of the core-shell molten salt composite balls, composite modified boron nitride nanosheets, water, potassium persulfate, styrene monomer and sodium dioctyl sulfosuccinate is (0.4-1.2):(1-2):(40-80):(0.1-0.5):(9-20):(1-2);
[0031] In the above process, under the initiation of potassium persulfate, the composite modified boron nitride nanosheets and styrene monomers are polymerized on the surface of the core-shell molten salt composite sphere, which improves the compatibility and dispersibility of the composite modified boron nitride nanosheets and styrene monomers, and forms an organic-inorganic hybrid outer shell. The organic-inorganic hybrid outer shell not only has excellent mechanical properties, which can make up for the insufficient mechanical properties of the expanded graphite inner shell, but also due to the excellent thermal conductivity of the composite modified boron nitride nanosheets, the thermal conductivity of the mixed molten salt heat storage and heat transfer material is further improved.
[0032] The mixed molten salt heat storage and heat transfer material is prepared by the method for preparing the mixed molten salt heat storage and heat transfer material.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] 1. The mixed molten salt heat storage and heat transfer material of the present invention has a mixed carbonate of lithium carbonate, sodium carbonate and potassium carbonate doped with modified carbon powder as a core, an ionic liquid modified expanded graphite as an inner shell, and an organic-inorganic hybrid material as an outer shell. The ionic liquid modified expanded graphite has a low wettability with carbonate, making it a very good carbonate packaging material, which can effectively prevent the leakage of liquid carbonate. The polystyrene shell of the composite modified boron nitride nanosheets encapsulates the carbonate in one step, while making up for the lack of mechanical properties of the expanded graphite material, preventing the heat storage and heat transfer material from being damaged during use. The mixed molten salt heat storage and heat transfer material with a double shell structure can not only solve the equipment corrosion problem caused by molten salt leakage, but also extend its own service life and reduce the use cost.
[0035] 2. The modified carbon powder in the present invention is rich in oxygen functional groups and has good wettability with molten carbonate. It can be well dispersed in carbonate molten salt, improving the specific heat capacity and thermal conductivity of the molten salt, thereby improving the heat storage performance of the mixed molten salt heat storage and heat transfer material.
[0036] 3. In the present invention, the synergy between the molten salt doped with modified carbon powder, the expanded graphite modified by ionic liquid and the composite modified boron nitride nanosheet / styrene organic-inorganic hybrid material makes the mixed molten salt heat storage and heat transfer material of the present invention have excellent thermal conductivity, thus solving the problem of low thermal conductivity of molten salt. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is a process flow chart of the preparation of the mixed molten salt heat storage and heat transfer material of the present invention. DETAILED DESCRIPTION
[0038] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0039] Example 1
[0040] This embodiment discloses a method for preparing a molten salt mixture, comprising the following steps:
[0041] Step A1, lithium carbonate, sodium carbonate, and potassium carbonate are mixed in a mass ratio of 43.5:31.5:25, heated to 300 ° C and maintained for 24 hours to remove moisture in the carbonate, and then heated to 750 ° C at a heating rate of 4 ° C / min, and maintained for 5.5 hours to completely melt the molten salt to obtain a molten mixed molten salt; the molten mixed molten salt is cooled to 450 ° C and used as an electrolyte, a platinum-coated titanium plate is used as an anode, and a nickel sheet is used as a cathode, and in a carbon dioxide atmosphere, at 50 mA / cm 2 The electrolysis was carried out for 120 minutes, wherein the size of the platinum-plated titanium plate was 20 mm × 20 mm × 1 mm, the thickness of the platinum layer was 0.01 mm, and the size of the nickel sheet was 40 mm × 30 mm × 0.1 mm; the cathode with carbon deposited after the electrolysis was reversed to an anode, and an oxidation treatment was carried out at a current of 0.5 A for 20 minutes. After the reaction was completed, the product on the anode was removed, washed with a 1 mol / L hydrochloric acid aqueous solution, dried, and ground to obtain modified carbon powder.
[0042] Step A2, mix lithium carbonate, sodium carbonate and potassium carbonate, heat to 500°C at a heating rate of 4°C / min and maintain for 5.5h, then add modified carbon powder, introduce argon at a flow rate of 200mL / min, stir and mix in an argon atmosphere for 120min, cool to room temperature, and grind to obtain a molten salt mixture; wherein the mass ratio of lithium carbonate, sodium carbonate, potassium carbonate and modified carbon powder is 43.5:31.5:25:0.05.
[0043] Example 2
[0044] This embodiment discloses a method for preparing a mixed molten salt heat storage and heat transfer material, comprising the following steps:
[0045] Step (1) Expanded graphite, 1-butyl-3-methylimidazolium hexafluorophosphate ionic liquid and ethanol are mixed in a mass ratio of 1:0.8:2, ultrasonically dispersed at 30 kHz for 100 minutes, filtered and dried at 60° C. to constant weight to obtain ionic liquid modified expanded graphite.
[0046] Step (2) mixing the molten salt mixture with ethanol in a mass ratio of 1:0.1, ultrasonically vibrating for 10 minutes, pressing the resulting mixture into a spherical mold with a diameter of 10 mm at 18 MPa by cold isostatic pressing to obtain a spherical core material, sintering the spherical core material at 580° C. for 100 minutes to obtain a molten salt core; mixing the ionic liquid modified expanded graphite with a 25wt% polyvinyl pyrrolidone ethanol solution in a mass ratio of 1:0.1 to obtain an inner shell material, controlling the coating thickness to 1.2 mm to coat the inner shell material on the molten salt core, then cold isostatically pressing at 18 MPa, and finally sintering in air at 430° C. for 100 minutes to obtain a core-shell molten salt composite ball.
[0047] Step (3) mixing hexagonal boron nitride nanosheets and urea in a mass ratio of 1:8, grinding at 400 r / min for 10 h, then heating to 530° C. at a heating rate of 3° C. / min and maintaining for 3.5 h, cooling to room temperature, and grinding to obtain highly exfoliated hexagonal boron nitride nanosheets.
[0048] Step (4) 10 g of highly exfoliated hexagonal boron nitride nanosheets, 250 mL of Tris buffer and 80 mL of ethanol are mixed, ultrasonically treated for 20 min, and then 4 g of dopamine hydrochloride is added, stirred and reacted at 23° C. for 10 h, filtered, and the filtered product is washed with ethanol to obtain modified boron nitride nanosheets; 250 mL of 2 wt% N,N-dimethylformamide dispersion of modified boron nitride nanosheets is mixed with 50 mL of 2 wt% silver nitrate N,N-dimethylformamide mixed solution, ultrasonically treated for 10 min, and then 100 mL of 15 mg / mL sodium borohydride aqueous solution is added, heated to 55° C., and reacted for 5.5 h under stirring conditions of 500 r / min. After the reaction is completed, filtered, the filtered product is washed with ethanol and then dried to obtain silver-doped modified boron nitride nanosheets.
[0049] Step (5) Disperse 1 g of silver-doped modified boron nitride nanosheets in 250 mL of ethanol, ultrasonically disperse for 100 min, then add 5 mL of vinyltriethoxysilane, stir for 10 min, then add 5 mL of ammonia water, stir and react at room temperature for 7 h, centrifuge, wash, and dry to obtain composite modified boron nitride nanosheets.
[0050] Step (6) 0.4 g of core-shell molten salt composite spheres, 1 g of composite modified boron nitride nanosheets, 40 g of water, and 0.1 g of potassium persulfate are mixed and ultrasonicated to obtain an aqueous phase; 9 g of styrene monomer and 1 g of sodium dioctyl sulfosuccinate surfactant are mixed to obtain an oil phase; the aqueous phase is heated to 55° C., and the oil phase is added to the aqueous phase within 15 min to obtain a mixed solution; the mixed solution is mixed at a stirring condition of 500 r / min for 100 min, polymerized at 55° C. for 11 h, filtered, washed, and dried to obtain a mixed molten salt heat storage and heat transfer material.
[0051] Example 3
[0052] This embodiment discloses a method for preparing a mixed molten salt heat storage and heat transfer material, comprising the following steps:
[0053] Step (1) Expanded graphite, 1-butyl-3-methylimidazolium hexafluorophosphate ionic liquid and ethanol are mixed in a mass ratio of 1:1.1:4, ultrasonically dispersed at 40 kHz for 150 minutes, filtered and dried at 70° C. to constant weight to obtain ionic liquid modified expanded graphite.
[0054] Step (2) The molten salt mixture is mixed with ethanol in a mass ratio of 1:0.15, and after ultrasonic vibration treatment for 30 minutes, the resulting mixture is pressed into a spherical mold with a diameter of 10 mm by cold isostatic pressing at 22 MPa to obtain a spherical core material, and the spherical core material is sintered at 620° C. for 150 minutes to obtain a molten salt core body; the ionic liquid modified expanded graphite is mixed with an ethanol solution of 50wt% polyvinyl pyrrolidone in a mass ratio of 1:0.2 to obtain an inner shell material, the inner shell material is coated on the molten salt core body with a coating thickness of 1.8 mm, and then cold isostatic pressing is performed at 22 MPa, and finally sintering in air at 470° C. for 150 minutes to obtain a core-shell molten salt composite ball.
[0055] Step (3) mixing hexagonal boron nitride nanosheets and urea in a mass ratio of 1:10, grinding at 500 r / min for 14 h, then heating to 570° C. at a heating rate of 5° C. / min and maintaining for 4.5 h, cooling to room temperature, and grinding to obtain highly exfoliated hexagonal boron nitride nanosheets.
[0056] Step (4) 15 g of highly exfoliated hexagonal boron nitride nanosheets, 500 mL of Tris buffer and 200 mL of ethanol are mixed, ultrasonically treated for 40 min, and then 6 g of dopamine hydrochloride is added, stirred and reacted at 28° C. for 14 h, filtered, and the filtered product is washed with ethanol to obtain modified boron nitride nanosheets; 400 mL of 2 wt% N,N-dimethylformamide dispersion of modified boron nitride nanosheets is mixed with 80 mL of 2 wt% silver nitrate N,N-dimethylformamide mixed solution, ultrasonically treated for 20 min, and then 160 mL of 15 mg / mL sodium borohydride aqueous solution is added, heated to 65° C., and reacted at a stirring condition of 700 r / min for 6.5 h. After the reaction is completed, filtered, the filtered product is washed with ethanol and then dried to obtain silver-doped modified boron nitride nanosheets.
[0057] Step (5) 2 g of silver-doped modified boron nitride nanosheets are dispersed in 500 mL of ethanol, ultrasonically dispersed for 150 min, and then 10 mL of vinyl triethoxysilane is added. After stirring for 20 min, 10 mL of ammonia water is added, and the reaction is stirred at room temperature for 9 h. The reaction is centrifuged, washed, and dried to obtain composite modified boron nitride nanosheets.
[0058] Step (6) 1.2 g of core-shell molten salt composite spheres, 2 g of composite modified boron nitride nanosheets, 80 g of water, and 0.5 g of potassium persulfate are mixed and ultrasonicated to obtain an aqueous phase; 20 g of styrene monomer and 2 g of sodium dioctyl sulfosuccinate surfactant are mixed to obtain an oil phase; the aqueous phase is heated to 65° C., and the oil phase is added to the aqueous phase within 25 min to obtain a mixed solution; the mixed solution is mixed at a stirring condition of 600 r / min for 150 min, polymerized at 65° C. for 13 h, filtered, washed, and dried to obtain a mixed molten salt heat storage and heat transfer material.
[0059] Example 4
[0060] This embodiment discloses a method for preparing a mixed molten salt heat storage and heat transfer material, comprising the following steps:
[0061] Step (1) Expanded graphite, 1-butyl-3-methylimidazolium hexafluorophosphate ionic liquid and ethanol are mixed in a mass ratio of 1:0.9:3, ultrasonically dispersed at 35 kHz for 120 minutes, filtered and dried at 65° C. to constant weight to obtain ionic liquid modified expanded graphite.
[0062] Step (2) The molten salt mixture is mixed with ethanol in a mass ratio of 1:0.12, and after ultrasonic vibration treatment for 20 minutes, the resulting mixture is pressed into a spherical mold with a diameter of 10 mm by cold isostatic pressing at 20 MPa to obtain a spherical core material, and the spherical core material is sintered at 600° C. for 120 minutes to obtain a molten salt core body; the ionic liquid modified expanded graphite and the ethanol solution of 35wt% polyvinyl pyrrolidone are mixed in a mass ratio of 1:0.15 to obtain an inner shell material, and the inner shell material is coated on the molten salt core body with a coating thickness of 1.5 mm, and then cold isostatic pressing is performed at 20 MPa, and finally sintering in air at 450° C. for 120 minutes to obtain a core-shell molten salt composite ball.
[0063] Step (3) mixing hexagonal boron nitride nanosheets and urea in a mass ratio of 1:9, grinding at 450 r / min for 12 h, then heating to 550° C. at a heating rate of 4° C. / min and maintaining for 4 h, cooling to room temperature, and grinding to obtain highly exfoliated hexagonal boron nitride nanosheets.
[0064] Step (4) 12.5 g of highly exfoliated hexagonal boron nitride nanosheets, 350 mL of Tris buffer and 140 mL of ethanol are mixed, ultrasonically treated for 30 min, and then 5 g of dopamine hydrochloride is added, stirred and reacted at 25° C. for 12 h, filtered, and the filtered product is washed with ethanol to obtain modified boron nitride nanosheets; 300 mL of 2 wt% N,N-dimethylformamide dispersion of modified boron nitride nanosheets is mixed with 65 mL of 2 wt% silver nitrate N,N-dimethylformamide mixed solution, ultrasonically treated for 15 min, and then 130 mL of 15 mg / mL sodium borohydride aqueous solution is added, heated to 60° C., and reacted for 6 h under stirring conditions of 600 r / min. After the reaction is completed, filtered, the filtered product is washed with ethanol and then dried to obtain silver-doped modified boron nitride nanosheets.
[0065] Step (5) 1.5 g of silver-doped modified boron nitride nanosheets are dispersed in 320 mL of ethanol, ultrasonically dispersed for 120 min, and then 8 mL of vinyl triethoxysilane is added. After stirring for 15 min, 7.5 mL of ammonia water is added, and the reaction is stirred at room temperature for 8 h. The reaction is centrifuged, washed, and dried to obtain composite modified boron nitride nanosheets.
[0066] Step (6) 0.8 g of core-shell molten salt composite spheres, 1.5 g of composite modified boron nitride nanosheets, 60 g of water, and 0.3 g of potassium persulfate are mixed and ultrasonicated to obtain an aqueous phase; 15 g of styrene monomer and 1.5 g of sodium dioctyl sulfosuccinate surfactant are mixed to obtain an oil phase; the aqueous phase is heated to 60° C., and the oil phase is added to the aqueous phase within 20 min to obtain a mixed solution; the mixed solution is mixed at a stirring condition of 550 r / min for 120 min, polymerized at 60° C. for 12 h, filtered, washed, and dried to obtain a mixed molten salt heat storage and heat transfer material.
[0067] Comparative Example 1
[0068] This comparative example discloses a method for preparing a molten salt mixture, comprising the following steps:
[0069] Step A1, lithium carbonate, sodium carbonate, and potassium carbonate are mixed in a mass ratio of 43.5:31.5:25, heated to 300 ° C and maintained for 24 hours to remove moisture in the carbonate, and then heated to 750 ° C at a heating rate of 4 ° C / min, and maintained for 5.5 hours to completely melt the molten salt to obtain a molten mixed molten salt; the molten mixed molten salt is cooled to 450 ° C and used as an electrolyte, a platinum-coated titanium plate is used as an anode, and a nickel sheet is used as a cathode, and in a carbon dioxide atmosphere, at 50 mA / cm 2The reaction was electrolyzed for 120 min, wherein the size of the platinum-coated titanium plate was 20 mm × 20 mm × 1 mm, the thickness of the platinum layer was 0.01 mm, and the size of the nickel sheet was 40 mm × 30 mm × 0.1 mm; after the reaction was completed, the product on the cathode was removed, washed with 1 mol / L hydrochloric acid aqueous solution, dried, and ground to obtain modified carbon powder.
[0070] Step A2, mix lithium carbonate, sodium carbonate and potassium carbonate, heat to 500°C at a heating rate of 4°C / min and maintain for 5.5h, then add modified carbon powder, introduce argon at a flow rate of 200mL / min, stir and mix in an argon atmosphere for 120min, cool to room temperature, and grind to obtain a molten salt mixture; wherein the mass ratio of lithium carbonate, sodium carbonate, potassium carbonate and modified carbon powder is 43.5:31.5:25:0.05.
[0071] Comparative Example 2
[0072] This comparative example discloses a method for preparing a molten salt mixture, comprising the following steps:
[0073] Lithium carbonate, sodium carbonate and potassium carbonate are mixed, heated to 500°C at a heating rate of 4°C / min and maintained for 5.5 hours, argon is introduced at a flow rate of 200 mL / min, stirred and mixed in an argon atmosphere for 120 minutes, cooled to room temperature, and ground to obtain a molten salt mixture; wherein the mass ratio of lithium carbonate, sodium carbonate and potassium carbonate is 43.5:31.5:25.
[0074] Comparative Example 3
[0075] Compared with Example 4, Comparative Example 3 uses the molten salt mixture prepared in Comparative Example 1, and other conditions remain unchanged.
[0076] Comparative Example 4
[0077] Compared with Example 4, Comparative Example 4 uses the molten salt mixture prepared in Comparative Example 2, and other conditions remain unchanged.
[0078] Comparative Example 5
[0079] Comparative Example 5 Compared with Example 4, in the process of preparing the core-shell molten salt composite spheres, expanded graphite is used instead of ionic liquid modified expanded graphite, and other conditions remain unchanged.
[0080] Comparative Example 6
[0081] Comparative Example 6 Compared with Example 4, in the process of preparing silver-doped modified boron nitride nanosheets, highly exfoliated hexagonal boron nitride nanosheets are used instead of modified boron nitride nanosheets in Comparative Example 6, and other conditions remain unchanged.
[0082] Comparative Example 7
[0083] Comparative Example 7 Compared with Example 4, in the process of preparing the composite modified boron nitride nanosheets, the modified boron nitride nanosheets were used instead of the silver-doped modified boron nitride nanosheets, and other conditions remained unchanged.
[0084] Comparative Example 8
[0085] Compared with Example 4, in Comparative Example 8, silver-doped modified boron nitride nanosheets are used instead of composite modified boron nitride nanosheets during the preparation of the mixed molten salt heat storage and heat transfer material, and other conditions remain unchanged.
[0086] Comparative Example 9
[0087] Comparative Example 9 Compared with Example 4, in Comparative Example 9, composite modified boron nitride nanosheets are added during the preparation of the mixed molten salt heat storage and heat transfer material, and other conditions remain unchanged.
[0088] Experimental example
[0089] 1. Specific heat capacity test: In a nitrogen atmosphere, the temperature was heated to 50-500°C at a heating rate of 10°C / min, and the specific heat capacity of the mixed molten salt heat storage and heat transfer materials of Examples 2-4 and Comparative Examples 3-4 was measured using a differential scanning calorimeter. The test results are shown in Table 1:
[0090] Table 1
[0091]
[0092] From the test results in Table 1, it can be seen that the specific heat capacity of the mixed molten salt heat storage and heat transfer material prepared in the embodiment of the present invention is as high as 3.85 J / (g·K), and has a good heat storage capacity. From the comparison between Comparative Example 3 and Comparative Example 4 and Example 4, it can be seen that the addition of carbon can significantly improve the specific heat capacity of the mixed molten salt heat storage and heat transfer material, and the modified carbon powder obtained by oxygen-enriched functional group treatment of carbon can better improve the specific heat capacity of the material.
[0093] 2. Thermal conductivity test: A laser thermal conductivity meter was used to test the thermal conductivity of the mixed molten salt heat storage and heat transfer materials of Examples 2-4 and Comparative Examples 3-9. The test results are shown in Table 2:
[0094] Table 1
[0095]
[0096] It can be seen from the test results of Table 2 that the mixed molten salt heat storage and heat transfer materials prepared in Examples 2-4 of the present invention have excellent thermal conductivity. From the comparison of Comparative Examples 3-4 and Example 4, it can be seen that after the modified carbon powder is functionalized with oxygen-enriched carbon powder, the improvement effect of the modified carbon powder on the thermal conductivity of the molten salt material can be improved; from Comparative Example 5, it can be seen that the expanded graphite is modified with ionic liquid, and the thermal conductivity of the mixed molten salt heat storage and heat transfer material is improved by improving the thermal conductivity of the expanded graphite; from the comparison of Comparative Examples 6-7 and Example 4, it can be seen that the growth and deposition of nanosilver improves the thermal conductivity of boron nitride nanosheets, thereby improving the thermal conductivity of the mixed molten salt heat storage and heat transfer material. Further, the use of polydopamine to modify the boron nitride nanosheets can increase The amount of nanosilver deposition is increased, thereby making the thermal conductivity of the boron nitride nanosheets better; from the comparison between Comparative Example 8 and Example 4, it can be seen that carbon-carbon double bonds are introduced on the surface of the silver-doped modified boron nitride nanosheets, so that the silver-doped modified boron nitride nanosheets are combined with the styrene monomer in the form of chemical bonds, thereby improving the dispersibility of the silver-doped modified boron nitride nanosheets in the shell, and therefore, it can also have a positive effect on the thermal conductivity of the mixed molten salt heat storage and heat transfer material; from the comparison between Comparative Example 9 and Example 4, it can be seen that the addition of the composite modified boron nitride nanosheets in the shell material significantly improves the thermal conductivity of the mixed molten salt heat storage and heat transfer material.
[0097] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a mixed molten salt heat storage and heat transfer material, characterized in that: The following steps are involved: Step (1) modifying expanded graphite with 1-butyl-3-methylimidazolium hexafluorophosphate ionic liquid to obtain ionic liquid modified expanded graphite; Step (2) treating the molten salt mixture to prepare a molten salt core, and coating the molten salt core with ionic liquid modified expanded graphite as an inner shell material to obtain a core-shell molten salt composite sphere; The molten salt mixture includes lithium carbonate, sodium carbonate, potassium carbonate and modified carbon powder; The modified carbon powder is obtained by oxidizing the cathode product obtained by electrolysis of carbon dioxide in a molten carbonate electrolyte; Step (3) adding urea to treat the hexagonal boron nitride nanosheets during the ball milling process to obtain highly exfoliated hexagonal boron nitride nanosheets; Step (4) treating the highly exfoliated hexagonal boron nitride nanosheets with polydopamine to obtain modified boron nitride nanosheets; in-situ growing nanosilver on the modified boron nitride nanosheets to obtain silver-doped modified boron nitride nanosheets; Step (5) treating the silver-doped modified boron nitride nanosheets with vinyltriethoxysilane to obtain composite modified boron nitride nanosheets; Step (6) uses core-shell molten salt composite balls, composite modified boron nitride nanosheets, and styrene monomer as main raw materials to prepare a mixed molten salt heat storage and heat transfer material.
2. The method for preparing the mixed molten salt heat storage and heat transfer material according to claim 1, characterized in that: In the step (1), the preparation method of the ionic liquid modified expanded graphite is as follows: the expanded graphite is mixed with 1-butyl-3-methylimidazolium hexafluorophosphate ionic liquid and ethanol, and ultrasonically dispersed at 30-40kHz for 100-150min, filtered and dried at 60-70°C to constant weight to obtain the ionic liquid modified expanded graphite; the mass ratio of the expanded graphite to the 1-butyl-3-methylimidazolium hexafluorophosphate ionic liquid and ethanol is 1:(0.8-1.1):(2-4).
3. The method for preparing the mixed molten salt heat storage and heat transfer material according to claim 1, characterized in that: In the step (2), the preparation method of the core-shell molten salt composite sphere is as follows: the molten salt mixture is mixed with ethanol, and after ultrasonic vibration treatment for 10-30 minutes, the obtained mixture is pressed into a spherical mold with a diameter of 10 mm by cold isostatic pressing at 18-22 MPa to obtain a spherical core material, and the spherical core material is sintered at 580-620°C for 100-150 minutes to obtain a molten salt core, wherein the mass ratio of the molten salt mixture to the ethanol is 1:(0.1-0.15); the ion Liquid modified expanded graphite is mixed with an ethanol solution of 25-50wt% polyvinyl pyrrolidone to obtain an inner shell material, the coating thickness is controlled to be 1.2-1.8mm, the inner shell material is coated on a molten salt core body, then cold isostatic pressing is performed at 18-22MPa, and finally sintering is performed in air at 430-470°C for 100-150min to obtain a core-shell molten salt composite ball; the mass ratio of the ionic liquid modified expanded graphite to the ethanol solution of polyvinyl pyrrolidone is 1:(0.1-0.2).
4. The method for preparing the mixed molten salt heat storage and heat transfer material according to claim 1, characterized in that: In the step (2), the method for preparing the molten salt mixture comprises the following steps: Step A1, lithium carbonate, sodium carbonate, and potassium carbonate are mixed in a mass ratio of (40-47): (30-33): (23-27), heated to 280-320 ° C and maintained for 20-28 hours to remove moisture from the carbonate, and then heated to 720-780 ° C at a heating rate of 3-5 ° C / min, and maintained for 5-6 hours to obtain a molten mixed molten salt; the molten mixed molten salt is cooled to 430-470 ° C and used as an electrolyte, a platinum-coated titanium plate is used as an anode, and a nickel sheet is used as a cathode, and in a carbon dioxide atmosphere, at 40-60 mA / cm 2 Electrolyze for 100-150 minutes, reverse the cathode with carbon deposited after the electrolysis to an anode, and oxidize for 15-30 minutes at a current of 0.4-0.6A. After the reaction is completed, remove the product on the anode, wash it with a 0.8-1.2 mol / L hydrochloric acid aqueous solution, dry it, and grind it to obtain modified carbon powder; Step A2, mix lithium carbonate, sodium carbonate and potassium carbonate, heat to 480-520°C at a heating rate of 3-5°C / min and maintain for 5-6h, then add modified carbon powder, introduce argon at a flow rate of 180-220mL / min, stir and mix in an argon atmosphere for 100-150min, cool to room temperature, and grind to obtain a molten salt mixture; wherein the mass ratio of lithium carbonate, sodium carbonate, potassium carbonate and modified carbon powder is (40-47):(30-33):(23-27):(0.03-0.07).
5. The method for preparing the mixed molten salt heat storage and heat transfer material according to claim 4, characterized in that: In the step A1, the size of the platinum-plated titanium plate is 20 mm×20 mm×1 mm, the thickness of the platinum layer is 0.01 mm, and the size of the nickel sheet is 40 mm×30 mm×0.1 mm.
6. The method for preparing the mixed molten salt heat storage and heat transfer material according to claim 1, characterized in that: In the step (3), the preparation method of the highly exfoliated hexagonal boron nitride nanosheets is as follows: the hexagonal boron nitride nanosheets are mixed with urea, ground at 400-500 r / min for 10-14 h, then heated to 530-570°C at a heating rate of 3-5°C / min and maintained for 3.5-4.5 h, cooled to room temperature, and ground to obtain highly exfoliated hexagonal boron nitride nanosheets; wherein the mass ratio of the hexagonal boron nitride nanosheets to the urea is 1:(8-10).
7. The method for preparing the mixed molten salt heat storage and heat transfer material according to claim 1, characterized in that: In the step (4), the preparation method of the silver-doped modified boron nitride nanosheets is as follows: highly exfoliated hexagonal boron nitride nanosheets, Tris buffer, and ethanol are mixed, ultrasonically treated for 20-40 minutes, dopamine hydrochloride is added, stirred and reacted at 23-28°C for 10-14 hours, filtered, and the filtered product is washed with ethanol to obtain modified boron nitride nanosheets, wherein the amount ratio of highly exfoliated hexagonal boron nitride nanosheets, Tris buffer, ethanol, and dopamine hydrochloride is (10-15) g: (250-500) mL: (80-200) mL: (4-6) g; 2 wt% of N,N-dihydrogen peroxide of the modified boron nitride nanosheets is added to the mixture. A methylformamide dispersion is mixed with a 2wt% silver nitrate N,N-dimethylformamide mixed solution, subjected to ultrasonic treatment for 10-20 minutes, and then a 15 mg / mL sodium borohydride aqueous solution is added, heated to 55-65° C., and reacted for 5.5-6.5 hours under a stirring condition of 500-700 r / min. After the reaction is completed, the mixture is filtered, and the filtered product is washed with ethanol and then dried to obtain silver-doped modified boron nitride nanosheets; wherein the volume ratio of the modified boron nitride nanosheet N,N-dimethylformamide dispersion, silver nitrate N,N-dimethylformamide, and sodium borohydride aqueous solution is (250-400):(50-80):(100-160).
8. The method for preparing the mixed molten salt heat storage and heat transfer material according to claim 1, characterized in that: In the step (5), the preparation method of the composite modified boron nitride nanosheets is as follows: silver-doped modified boron nitride nanosheets are dispersed in ethanol, ultrasonically dispersed for 100-150 minutes, then vinyl triethoxysilane is added, stirred for 10-20 minutes, and then ammonia water is added, stirred for reaction at room temperature for 7-9 hours, centrifuged, washed, and dried to obtain composite modified boron nitride nanosheets; wherein the amount ratio of silver-doped modified boron nitride nanosheets, ethanol, vinyl triethoxysilane, and ammonia water is (1-2) g: (250-500) mL: (5-10) mL: (5-10) mL.
9. The method for preparing the mixed molten salt heat storage and heat transfer material according to claim 1, characterized in that: In the step (6), the preparation method of the mixed molten salt heat storage and heat transfer material is as follows: core-shell molten salt composite balls, composite modified boron nitride nanosheets, water, and potassium persulfate are mixed, and ultrasonicated to obtain an aqueous phase; styrene monomer and sodium dioctyl sulfosuccinate are mixed to obtain an oil phase; the aqueous phase is heated to 55-65°C, and the oil phase is added to the aqueous phase within 15-25 minutes to obtain a mixed solution; the mixed solution is mixed under stirring conditions of 500-600 r / min for 100-150 minutes, polymerized at 55-65°C for 11-13 hours, filtered, washed, and dried to obtain a mixed molten salt heat storage and heat transfer material; wherein the mass ratios of the core-shell molten salt composite balls, composite modified boron nitride nanosheets, water, potassium persulfate, styrene monomer, and sodium dioctyl sulfosuccinate are (0.4-1.2):(1-2):(40-80):(0.1-0.5):(9-20):(1-2).
10. A mixed molten salt heat storage and heat transfer material prepared by the method according to any one of claims 1 to 9.