Heat-conducting gasket, preparation method thereof and electronic component
Through silicon-free photosensitive colloid system and UV curing technology, the problems of poor filling and insufficient heat resistance of silicon-free thermal gaskets are solved, low volatility and high thermal conductivity are achieved, production process is simplified, and traditional thermal gaskets are avoided. Pollution and performance reduction.
Patent Information
- Application Number
- CN202411118660.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
The existing silicon-free thermal gaskets have poor filling properties and difficulty in operation, and lack of heat resistance, which cannot effectively solve the problems of contamination and performance reduction caused by the volatility of small molecules of silicone thermal gaskets.
Thermal gaskets are prepared by silicon-free photosensitive colloid system. By vacuum defoaming and UV curing, combined with active monomers, prepolymers and photoinitiators, thermal gaskets with high filling properties and good thermal conductivity are prepared, avoiding organic Small molecules of silicon volatilize and improve heat resistance.
The low volatility, good thermal conductivity and high heat resistance of thermal gaskets are achieved, the production process is simplified, the production efficiency is improved, and the pollution and performance reduction of traditional thermal gaskets are avoided.
Smart Images

Figure BDA0004994379250000121
Abstract
Description
Technical Field
[0001] The present application relates to the field of thermally conductive interface materials, and more specifically, to a thermally conductive gasket and a preparation method thereof, and an electronic component. Background Art
[0002] With the advancement of science and technology, all walks of life have developed rapidly, especially in the industrial, automotive and consumer electronics industries. Many electronic components are used in these industries. These electronic components will generate a lot of heat when working. If they cannot be dissipated in time and effectively, it may cause the performance of the components to deteriorate or even be damaged. Therefore, the role of thermal pads is to help these electronic components transfer heat quickly and evenly to ensure that they can operate stably and efficiently.
[0003] At present, most thermal pad materials on the market are based on silicone resin systems. However, with the continuous diversification and complexity of application scenarios, the shortcomings of silicone thermal pads have gradually emerged, that is, the volatilization problem of silicone small molecules. The volatilized silicone small molecules will cause pollution to equipment and products, reduce electrical performance, reduce the transmittance of optical equipment, and potentially threaten instruments and equipment. These problems will bring unnecessary trouble and losses to consumers. Silicone-free thermal pads were born in this context. The existing silicone-free thermal pads are prepared based on acrylic resin. Although the problem of volatilization of silicone small molecules in traditional thermal pads is avoided, new problems such as poor resin filling, high viscosity of the mixed material, difficult operation, and poor heat resistance of the silicone-free gaskets have emerged. Summary of the invention
[0004] The present application provides a material which has low volatility and good filling property for thermally conductive powder and good thermal conductivity.
[0005] The embodiment of the present application is implemented as follows:
[0006] In the first aspect, the present application provides a method for preparing a thermally conductive gasket, which comprises mixing raw materials including a UV curable composition and a thermally conductive powder to obtain a thermally conductive colloid, and sequentially performing vacuum degassing, calendering into sheets, and UV curing on the thermally conductive colloid to obtain a thermally conductive gasket. The UV curable composition comprises an active monomer, a prepolymer, and a photoinitiator.
[0007] In the above technical scheme, the preparation method of the thermally conductive gasket of the present application prepares a non-silicone thermally conductive gasket with a silicon-free photosensitive colloid system, firstly, the small molecules in the thermally conductive colloid are volatilized and the gas in the thermally conductive colloid is removed by vacuum degassing, thereby reducing or avoiding the influence of bubbles in the thermally conductive gasket on its thermal conductivity, and then UV curing treatment is performed after rolling into sheets to cure the raw materials into thermally conductive gaskets. Since there is no addition of silicone, the thermally conductive gasket still maintains a low oil yield in a long-term pressure and heat environment, and the thermally conductive gasket of the present application has good resin filling properties, and there is no problem of high viscosity of the mixed material and difficulty in operation, so that more thermally conductive powder can be filled to improve the thermal conductivity of the thermally conductive gasket. In addition, the UV curing time is short, and the thermally conductive colloid can be used for a long time after a one-time preparation under light-proof conditions, thereby greatly improving production efficiency.
[0008] In combination with the first aspect, in a first possible example of the first aspect of the present application, the raw materials include 4 to 18 parts by weight of a UV curable composition and 70 to 95 parts by weight of a thermally conductive powder.
[0009] In the above example, by making the raw materials include the above-mentioned parts by weight of the UV curable composition and the thermally conductive powder, the prepared thermally conductive gasket can have a better thermal conductive effect.
[0010] In combination with the first aspect, in a second possible example of the first aspect of the present application, the mass ratio of the above-mentioned active monomer, prepolymer and photoinitiator is 35-75:5-25:0.3-5;
[0011] Optionally, the active monomer includes any one or more of styrene, vinyl pyrrolidone, vinyl acetate, butyl acrylate, isooctyl acrylate, hydroxy (meth)acrylate, 1,4-butanediol acrylate, 1,6-hexanediol diacrylate, ethylene glycol dimethacrylate, tripropylene glycol diacrylate, neopentyl glycol diacrylate, pentaerythritol triacrylate, trimethylolpropane triacrylate and (3-ethoxy)trimethylolpropane triacrylate.
[0012] Optionally, the prepolymer includes any one or more of novolac epoxy acrylate, bisphenol A epoxy acrylate and epoxy soybean oil acrylate.
[0013] Optionally, the photoinitiator includes any one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, trimethylbenzoyl-diphenylphosphine oxide, benzophenone, 1-hydroxy-cyclohexyl-phenyl ketone and benzoin diethyl ether.
[0014] In combination with the first aspect, in a third possible example of the first aspect of the present application, the prepolymer includes bisphenol A epoxy acrylate.
[0015] In the above example, by selecting the prepolymer to include bisphenol A epoxy acrylate, the prepared thermally conductive pad can have better heat resistance.
[0016] In combination with the first aspect, in a fourth possible example of the first aspect of the present application, the thermally conductive powder includes any one or more of aluminum oxide, zinc oxide, aluminum nitride and boron nitride.
[0017] In the above example, the thermally conductive powder can be used to fill the network structure formed by the UV curing composition to improve the thermal conductivity of the thermally conductive gasket.
[0018] In combination with the first aspect, in a fifth possible example of the first aspect of the present application, the mixing includes placing the raw materials in a kneader and mixing them for 10 min to 200 min, and setting the stirring rate of the kneader to 10 r / min to 400 r / min.
[0019] In the above example, the above mixing method is conducive to preparing a thermally conductive colloid with uniform texture.
[0020] In combination with the first aspect, in a sixth possible example of the first aspect of the present application, the vacuum degassing includes vacuuming at a temperature of 100° C. to 150° C. for 1 h to 4 h.
[0021] In the above example, the preparation method of the thermally conductive gasket of the present application can more thoroughly remove the small molecular volatiles in the raw materials and reduce the oil yield of the thermally conductive gasket through vacuum degassing treatment at a higher temperature.
[0022] In combination with the first aspect, in a seventh possible example of the first aspect of the present application, the above-mentioned UV curing includes irradiating the front and back surfaces with ultraviolet light having a wavelength of 200nm to 450nm for 10s to 240s respectively.
[0023] In the above example, the curing time of the thermally conductive gasket of the present application is short, which is beneficial to improving production efficiency.
[0024] In a second aspect, the present application example provides a thermally conductive gasket, which is manufactured according to the above-mentioned method for manufacturing a thermally conductive gasket.
[0025] In the above technical solution, the thermally conductive gasket of the present application has a lower oil yield and better thermal conductivity.
[0026] In a third aspect, the present application example provides an electronic component comprising the above-mentioned thermal conductive gasket. DETAILED DESCRIPTION
[0027] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0028] The following is a detailed description of a thermally conductive pad and a preparation method thereof, and an electronic component according to an embodiment of the present application:
[0029] The present invention provides a method for preparing a thermally conductive pad, which comprises the following steps:
[0030] S1. Mixing
[0031] The raw materials including the UV curing composition and the thermal conductive powder are uniformly mixed to prepare a thermal conductive colloid.
[0032] The UV curable composition comprises active monomers, prepolymers and photoinitiators, and the mass ratio of the active monomers, prepolymers and photoinitiators is 35-75:5-25:0.3-5.
[0033] As an example, the mass ratio of the active monomer, the prepolymer and the photoinitiator may be 49:6:0.6.
[0034] In some embodiments, the reactive monomer includes any one or more of styrene, vinyl pyrrolidone, vinyl acetate, butyl acrylate, isooctyl acrylate, hydroxy (meth)acrylate, 1,4-butanediol acrylate, 1,6-hexanediol diacrylate, ethylene glycol dimethacrylate, tripropylene glycol diacrylate, neopentyl glycol diacrylate, pentaerythritol triacrylate, trimethylolpropane triacrylate, and (3-ethoxy)trimethylolpropane triacrylate.
[0035] As an example, the reactive monomer may include styrene, vinyl pyrrolidone, vinyl acetate, butyl acrylate, isooctyl acrylate, hydroxy (meth)acrylate, 1,4-butanediol acrylate, 1,6-hexanediol diacrylate, ethylene glycol dimethacrylate, tripropylene glycol diacrylate, neopentyl glycol diacrylate, pentaerythritol triacrylate, trimethylolpropane triacrylate or (3-ethoxy)trimethylolpropane triacrylate alone, or may be a mixture of isooctyl acrylate, 1,6-hexanediol diacrylate and pentaerythritol triacrylate, or may be any combination of the above reactive monomers.
[0036] In some embodiments, the prepolymer includes any one or more of novolac epoxy acrylate, bisphenol A epoxy acrylate, and epoxy soybean oil acrylate.
[0037] Optionally, the prepolymer comprises bisphenol A epoxy acrylate.
[0038] By selecting the prepolymer to include bisphenol A epoxy acrylate, the prepared thermal conductive pad can have better heat resistance.
[0039] Optionally, the prepolymer is bisphenol A epoxy acrylate.
[0040] In some embodiments, the photoinitiator includes any one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, trimethylbenzoyl-diphenylphosphine oxide, benzophenone, 1-hydroxy-cyclohexyl-phenyl ketone, and benzoin diethyl ether.
[0041] It should be noted that different photoinitiators can be used to initiate polymerization of active monomers under ultraviolet light conditions of different wavelengths. For example, 2-hydroxy-2-methyl-1-phenyl-1-propanone can be used to initiate polymerization of active monomers under ultraviolet light conditions of 355nm wavelength, trimethylbenzoyl-diphenylphosphine oxide can be used to initiate polymerization of active monomers under ultraviolet light conditions of 368nm wavelength, benzophenone can be used to initiate polymerization of active monomers under ultraviolet light conditions of 255nm wavelength, 1-hydroxy-cyclohexyl-phenyl ketone can be used to initiate polymerization of active monomers under ultraviolet light conditions of 280nm wavelength, and benzoin diethyl ether can be used to initiate polymerization of active monomers under ultraviolet light conditions of 250nm wavelength.
[0042] In some embodiments, the thermally conductive powder includes any one or more of aluminum oxide, zinc oxide, aluminum nitride, and boron nitride.
[0043] As an example, the thermally conductive powder may include aluminum oxide, zinc oxide, aluminum nitride or boron nitride alone, or may include a mixture of aluminum oxide and zinc oxide, or may include a mixture of aluminum oxide and aluminum nitride, or may include a mixture of aluminum oxide and boron nitride, or may include a mixture of aluminum oxide, zinc oxide and aluminum nitride, or may include a mixture of zinc oxide, aluminum nitride and boron nitride, or may include a mixture of aluminum oxide, zinc oxide, aluminum nitride and boron nitride.
[0044] The thermally conductive powder can be used to fill the network structure formed by the UV curing composition to improve the thermal conductivity of the thermally conductive gasket.
[0045] In some embodiments, the raw materials include 4 parts by weight to 18 parts by weight of UV curable composition and 70 parts by weight to 95 parts by weight of thermal conductive powder.
[0046] As an example, the raw materials may include 4 parts by weight, 6 parts by weight, 8 parts by weight, 10 parts by weight, 12 parts by weight, 15 parts by weight or 18 parts by weight of UV curing composition and 70 parts by weight, 75 parts by weight, 80 parts by weight, 85 parts by weight, 90 parts by weight or 95 parts by weight of thermal conductive powder.
[0047] By making the raw materials include the above-mentioned UV curing composition and thermally conductive powder in parts by weight, the prepared thermally conductive pad can have a better thermal conductive effect.
[0048] In some embodiments, the mixing includes placing the raw materials in a kneader and mixing for 10 min to 200 min, and setting the stirring rate of the kneader to 10 r / min to 400 r / min.
[0049] As an example, the mixing time of the raw materials in the kneader can be 10 min, 20 min, 50 min, 80 min, 100 min, 120 min, 150 min, 180 min or 200 min; the stirring rate of the kneader can be 10 r / min, 20 r / min, 50 r / min, 80 r / min, 100 r / min, 150 r / min, 200 r / min, 250 r / min, 300 r / min, 350 r / min or 400 r / min.
[0050] The above mixing method is conducive to preparing a thermally conductive colloid with uniform texture.
[0051] S2. Preparation of thermal conductive pads
[0052] The thermal conductive colloid is sequentially subjected to vacuum degassing, calendering into sheets and UV curing to obtain a thermal conductive pad.
[0053] In some embodiments, vacuum degassing includes vacuuming at a temperature of 100° C. to 150° C. for 1 h to 4 h.
[0054] As an example, the temperature of vacuum degassing can be 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C or 150°C; the time of vacuum degassing can be 1h, 1.5h, 2h, 2.5h, 3h, 3.5h or 4h.
[0055] The preparation method of the thermally conductive gasket of the present application can more thoroughly remove small molecular volatiles in the raw materials and reduce the oil yield of the thermally conductive gasket through vacuum degassing treatment at a relatively high temperature.
[0056] In some embodiments, UV curing includes irradiating the front and back surfaces with ultraviolet light having a wavelength of 200 nm to 450 nm for 10 s to 240 s respectively.
[0057] As an example, the wavelength of ultraviolet light for UV curing can be 250nm, 255nm, 280nm, 355nm or 368nm; the duration of UV curing can be 10s, 20s, 30s, 50s, 80s, 100s, 150s, 200s or 240s.
[0058] The preparation method of the thermally conductive gasket of the present application prepares a non-silicone thermally conductive gasket with a silicon-free photosensitive colloid system. First, the small molecules in the thermally conductive colloid are volatilized and the gas in the thermally conductive colloid is removed by vacuum degassing, thereby reducing or avoiding the influence of bubbles in the thermally conductive gasket on its thermal conductivity. After rolling into sheets, UV curing treatment is performed to solidify the raw materials into thermally conductive gaskets. Since there is no addition of silicone, the thermally conductive gasket of the present application still maintains a low oil yield in a long-term pressure and heat environment. In addition, the thermally conductive gasket of the present application has good resin filling properties and does not have problems such as high viscosity of the mixed material and difficulty in operation, so that more thermally conductive powder can be filled to improve the thermal conductivity of the thermally conductive gasket. In addition, the UV curing time is short, and the thermally conductive colloid can be used for a long time after a one-time preparation under light-proof conditions, thereby greatly improving production efficiency.
[0059] The present application also provides a thermally conductive gasket, which is prepared according to the above-mentioned method for preparing the thermally conductive gasket.
[0060] The thermally conductive gasket of the present application has a lower oil yield and a better thermal conductive effect.
[0061] The present application also provides an electronic component, which includes the above-mentioned thermal conductive gasket.
[0062] A thermally conductive gasket and a preparation method thereof of the present application are further described in detail below in conjunction with embodiments.
[0063] Example 1
[0064] The present invention provides a method for preparing a thermally conductive pad, which comprises the following steps:
[0065] S1. Mixing
[0066] 25 parts by weight of isooctyl acrylate, 14 parts by weight of 1,6-hexanediol diacrylate, 10 parts by weight of pentaerythritol triacrylate, 6 parts by weight of bisphenol A epoxy acrylate, 0.6 parts by weight of 2-hydroxy-2-methyl-1-phenyl-1-propanone and 0.4 parts by weight of trimethylbenzoyl-diphenylphosphine oxide are added to a kneader, and the kneader is mixed at a stirring rate of 120 r / min for 30 minutes to obtain a first mixture, and then 900 parts by weight of aluminum oxide powder and 150 parts by weight of aluminum nitride powder are added to the kneader, and the kneader is mixed at a stirring rate of 120 r / min for 30 minutes to obtain a thermally conductive colloid.
[0067] S2. Preparation of thermal conductive pads
[0068] The thermal conductive colloid was poured out from the kneader, and the colloid was vacuumed at 120°C for 1 hour to achieve degassing, and then rolled into a sheet. Finally, ultraviolet light with a wavelength of 360nm was used to irradiate the front and back sides of the sheet thermal conductive colloid for 180s respectively to obtain a thermal conductive gasket.
[0069] Example 2
[0070] The present invention provides a method for preparing a thermally conductive pad, which comprises the following steps:
[0071] S1. Mixing
[0072] 25 parts by weight of butyl methacrylate, 14 parts by weight of 1,6-hexanediol diacrylate, 10 parts by weight of trimethylolpropane triacrylate, 0.6 parts by weight of bisphenol A epoxy acrylate, 0.06 parts by weight of 2-hydroxy-2-methyl-1-phenyl-1-propanone and 0.04 parts by weight of trimethylbenzoyl-diphenylphosphine oxide were added to a kneader, and the kneader was mixed at a stirring rate of 120 r / min for 30 minutes to obtain a first mixture, and then 900 parts by weight of aluminum oxide powder and 150 parts by weight of aluminum nitride powder were added to the kneader, and the kneader was mixed at a stirring rate of 120 r / min for 30 minutes to obtain a thermally conductive colloid.
[0073] S2. Preparation of thermal conductive pads
[0074] The thermal conductive colloid was poured out from the kneader, and the colloid was vacuumed at 120°C for 1 hour to achieve degassing, and then rolled into a sheet. Finally, ultraviolet light with a wavelength of 360nm was used to irradiate the front and back sides of the sheet thermal conductive colloid for 180s respectively to obtain a thermal conductive gasket.
[0075] Example 3
[0076] The present invention provides a method for preparing a thermally conductive pad, which comprises the following steps:
[0077] S1. Mixing
[0078] 25 parts by weight of isooctyl acrylate, 14 parts by weight of 1,6-hexanediol diacrylate, 10 parts by weight of pentaerythritol triacrylate, 6 parts by weight of novolac epoxy acrylate, 0.6 parts by weight of 2-hydroxy-2-methyl-1-phenyl-1-propanone and 0.4 parts by weight of trimethylbenzoyl-diphenylphosphine oxide were added into a kneader, and the kneader was mixed at a stirring rate of 120 r / min for 30 minutes to obtain a first mixture, and then 900 parts by weight of aluminum oxide powder and 150 parts by weight of aluminum nitride powder were added into the kneader, and the kneader was mixed at a stirring rate of 120 r / min for 30 minutes to obtain a thermally conductive colloid.
[0079] S2. Preparation of thermal conductive pads
[0080] The thermal conductive colloid was poured out from the kneader, and the colloid was vacuumed at 120°C for 1 hour to achieve degassing, and then rolled into a sheet. Finally, ultraviolet light with a wavelength of 360nm was used to irradiate the front and back sides of the sheet thermal conductive colloid for 180s respectively to obtain a thermal conductive gasket.
[0081] Example 4
[0082] The present invention provides a method for preparing a thermally conductive pad, which comprises the following steps:
[0083] S1. Mixing
[0084] 25 parts by weight of isooctyl acrylate, 14 parts by weight of 1,6-hexanediol diacrylate, 10 parts by weight of pentaerythritol triacrylate, 6 parts by weight of bisphenol A epoxy acrylate, 0.6 parts by weight of 2-hydroxy-2-methyl-1-phenyl-1-propanone and 0.4 parts by weight of trimethylbenzoyl-diphenylphosphine oxide are added to a kneader, and the kneader is mixed at a stirring rate of 120 r / min for 30 minutes to obtain a first mixture, and then 900 parts by weight of aluminum oxide powder, 50 parts by weight of boron nitride powder and 100 parts by weight of aluminum nitride are added to the kneader, and the kneader is mixed at a stirring rate of 120 r / min for 30 minutes to obtain a thermally conductive colloid.
[0085] S2. Preparation of thermal conductive pads
[0086] The thermal conductive colloid was poured out from the kneader, and the colloid was vacuumed at 120°C for 1 hour to achieve degassing, and then rolled into a sheet. Finally, ultraviolet light with a wavelength of 360nm was used to irradiate the front and back sides of the sheet thermal conductive colloid for 180s respectively to obtain a thermal conductive gasket.
[0087] Example 5
[0088] The present invention provides a method for preparing a thermally conductive pad, which comprises the following steps:
[0089] S1. Mixing
[0090] 25 parts by weight of isooctyl acrylate, 14 parts by weight of 1,6-hexanediol diacrylate, 10 parts by weight of pentaerythritol triacrylate, 6 parts by weight of bisphenol A epoxy acrylate, 0.6 parts by weight of 2-hydroxy-2-methyl-1-phenyl-1-propanone and 0.4 parts by weight of trimethylbenzoyl-diphenylphosphine oxide are added to a kneader, and the kneader is mixed at a stirring rate of 120 r / min for 30 minutes to obtain a first mixture, and then 900 parts by weight of aluminum oxide powder and 150 parts by weight of aluminum nitride powder are added to the kneader, and the kneader is mixed at a stirring rate of 120 r / min for 30 minutes to obtain a thermally conductive colloid.
[0091] S2. Preparation of thermal conductive pads
[0092] The thermal conductive colloid was poured out from the kneader, and the colloid was vacuumed at 25°C for 1 hour to achieve degassing, and then rolled into a sheet. Finally, ultraviolet light with a wavelength of 360nm was used to irradiate the front and back sides of the sheet of thermal conductive colloid for 180s each to obtain a thermal conductive pad.
[0093] Comparative Example 1
[0094] The comparative example of the present application provides a method for preparing a thermally conductive gasket, which comprises the following steps:
[0095] S1. Mixing
[0096] 58 parts by weight of vinyl silicone oil, 6 parts by weight of hydrogenated silicone oil, 910 parts by weight of alumina powder, 100 parts by weight of aluminum nitride powder, 2 parts by weight of silane coupling agent, 1 part by weight of platinum catalyst and 0.1 part by weight of inhibitor were added into a kneader, and the kneader was mixed at a stirring rate of 150 r / min for 30 minutes to obtain a thermally conductive colloid.
[0097] S2. Preparation of thermal conductive pads
[0098] The thermally conductive colloid was poured out from the kneader, and the colloid was vacuumed at 25°C for 1 hour to achieve degassing, then rolled into sheets, and finally baked at 125°C for 15 minutes to obtain a thermally conductive gasket.
[0099] Comparative Example 2
[0100] The comparative example of the present application provides a method for preparing a thermally conductive gasket, which comprises the following steps:
[0101] S1. Mixing
[0102] 50 parts by weight of acrylic resin, 2 parts by weight of isocyanate, 11 parts by weight of dioctyl terephthalate, 800 parts by weight of alumina thermal conductive powder, 40 parts by weight of zinc oxide powder, 40 parts by weight of aluminum nitride powder and 40 parts by weight of boron nitride powder were added to a kneader, and the kneader mixed at a stirring rate of 300 r / min for 10 minutes to obtain a first mixture, and then 0.2 parts by weight of an organic tin catalyst was added to the kneader, and the kneader mixed at a stirring rate of 300 r / min for 10 minutes to obtain a thermally conductive colloid.
[0103] S2. Preparation of thermal conductive pads
[0104] The thermal conductive colloid was poured out from the kneader, and the colloid was vacuumed at 25°C for 1 hour to achieve degassing, then rolled into sheets, and finally baked at 125°C for 20 minutes to obtain a thermal conductive gasket.
[0105] Comparative Example 3
[0106] The comparative example of the present application provides a method for preparing a thermally conductive gasket, which comprises the following steps:
[0107] S1. Mixing
[0108] 50 parts by weight of acrylic resin, 2 parts by weight of isocyanate, 11 parts by weight of dioctyl terephthalate, 800 parts by weight of alumina thermal conductive powder, 40 parts by weight of zinc oxide powder, 40 parts by weight of aluminum nitride powder and 100 parts by weight of boron nitride powder were added to a kneader, and the kneader mixed at a stirring rate of 300 r / min for 10 minutes to obtain a first mixture, and then 0.02 parts by weight of an organic tin catalyst was added to the kneader, and the kneader mixed at a stirring rate of 300 r / min for 10 minutes to obtain a thermally conductive colloid.
[0109] S2. Preparation of thermal conductive pads
[0110] The thermal conductive colloid was poured out from the kneader, and the colloid was vacuumed at 25°C for 1 hour to achieve degassing, then rolled into sheets, and finally baked at 125°C for 20 minutes to obtain a thermal conductive gasket.
[0111] Test Example 1
[0112] The thermal conductivity, volatility and heat resistance of the thermally conductive gaskets prepared in Examples 1 to 5 and Comparative Examples 1 to 3 were measured. The results are shown in Table 1.
[0113] The test method is as follows:
[0114] 1. Thermal conductivity
[0115] The test was performed according to ASTM D5470.
[0116] 2. Volatility rate
[0117] The samples were baked at 150°C for 72 h, and the weight loss of the samples was measured.
[0118] 3. Heat resistance
[0119] The samples were baked at 150°C for 168 hours, and the hardness difference before and after the test samples was verified.
[0120] Table 1 Parameters of thermally conductive pads obtained in Examples 1 to 5 and Comparative Examples 1 to 3
[0121]
[0122] It can be seen from Examples 1 to 5 that the thermally conductive pad prepared in the present application has a good thermal conductivity and a low volatility.
[0123] From the comparison between Example 1 and Example 3, it can be seen that when the prepolymer includes bisphenol A epoxy acrylate, the prepared thermally conductive gasket has better heat resistance.
[0124] By comparing Example 1 and Example 5, it can be seen that when the temperature of vacuum degassing is 100°C to 150°C, not only can the small molecular volatiles in the raw materials be removed more thoroughly and the volatility of the thermally conductive gasket be reduced, but also the thermal conductivity of the thermally conductive gasket can be improved.
[0125] From the comparison between Examples 1 to 5 and Comparative Example 1, it can be seen that compared with the silicone resin system, the thermally conductive pad prepared by the preparation method of the present application has a lower volatility.
[0126] From the comparison between Examples 1 to 5 and Comparative Example 2, it can be seen that compared with the acrylic resin matrix system, the thermally conductive gasket prepared by the preparation method of the present application has a better thermal conductive effect.
[0127] From the comparison between Examples 1 to 5 and Comparative Example 3, it can be seen that if a relatively large amount of thermal conductive monomer is added to the acrylic resin matrix system, the thermal conductive powder cannot be mixed uniformly.
[0128] The above description is only a specific embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A method for preparing a thermally conductive gasket, characterized in that: The preparation method of the thermally conductive gasket comprises: mixing raw materials including a UV curable composition and a thermally conductive powder to obtain a thermally conductive colloid, and sequentially performing vacuum degassing, calendering into sheets and UV curing on the thermally conductive colloid to obtain a thermally conductive gasket; The UV curable composition includes active monomers, prepolymers and photoinitiators.
2. The method for preparing a thermally conductive gasket according to claim 1, characterized in that: The raw materials include 4 to 18 parts by weight of the UV curing composition and 70 to 95 parts by weight of the thermal conductive powder.
3. The method for preparing a thermally conductive pad according to claim 1, characterized in that: The mass ratio of the active monomer, the prepolymer and the photoinitiator is 35-75:5-25:0.3-5; Optionally, the active monomer includes any one or more of styrene, vinyl pyrrolidone, vinyl acetate, butyl acrylate, isooctyl acrylate, hydroxy (meth)acrylate, 1,4-butanediol acrylate, 1,6-hexanediol diacrylate, ethylene glycol dimethacrylate, tripropylene glycol diacrylate, neopentyl glycol diacrylate, pentaerythritol triacrylate, trimethylolpropane triacrylate and (3-ethoxy)trimethylolpropane triacrylate; Optionally, the prepolymer includes any one or more of novolac epoxy acrylate, bisphenol A epoxy acrylate and epoxy soybean oil acrylate; Optionally, the photoinitiator includes any one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, trimethylbenzoyl-diphenylphosphine oxide, benzophenone, 1-hydroxy-cyclohexyl-phenyl ketone and benzoin diethyl ether.
4. The method for preparing a thermally conductive pad according to claim 3, characterized in that: The prepolymer includes bisphenol A epoxy acrylate.
5. The method for preparing a thermally conductive pad according to claim 1, characterized in that: The thermally conductive powder includes any one or more of aluminum oxide, zinc oxide, aluminum nitride and boron nitride.
6. The method for preparing a thermally conductive pad according to claim 1, characterized in that: The mixing comprises placing the raw materials in a kneader and mixing them for 10 min to 200 min, and setting the stirring rate of the kneader to 10 r / min to 400 r / min.
7. The method for preparing a thermally conductive gasket according to claim 1, characterized in that: The vacuum degassing comprises vacuuming at a temperature of 100° C. to 150° C. for 1 hour to 4 hours.
8. The method for preparing a thermally conductive gasket according to claim 1, characterized in that: The UV curing includes irradiating the front and back surfaces with ultraviolet light having a wavelength of 200nm to 450nm for 10s to 240s respectively.
9. A thermally conductive gasket, characterized in that: The thermally conductive gasket is prepared according to the method for preparing a thermally conductive gasket according to any one of claims 1 to 8.
10. An electronic component, characterized in that: The electronic component comprises the thermally conductive pad according to claim 9.
Citation Information
Cited By
Low-dielectric heat-conducting gasket and preparation method thereof
CN119505070A