Anti-sloughing composition and broken joint body stratum wellbore reinforced water-based drilling fluid

By using anti-collapse composition and sealant synergistic efficiency in drilling of the fractured body formation, the prepared water-based drilling fluid solves the problem of poor stability of the well wall, and effectively seals and bonds the fractured body formation. , improves the performance of drilling fluid.

CN119020002AActive Publication Date: 2024-11-26CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310602884.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-11-26
Estimated Expiration
2043-05-26

AI Technical Summary

Technical Problem

In the drilling of existing drilling fluid, there are problems such as poor stability of the well wall, poor suspension and rock carrying performance, insufficient hydration inhibition performance of clay minerals and cementing capacity of crushed rocks in the cracked body formation, and it is difficult to effectively solve the instability of the well wall of the cracked body formation. problem.

Method used

Provided is a collapsing anti-collapse composition consisting of HTFT, modified asphalt anti-collapse anti-collapse agent GLA and C9 petroleum resin, and combined with polyamine inhibitor SMJA-1, sealing agent, tackifier TQ-1, lowering The wellbore of the crack-breaking body formation prepared by water loss agent, bentonite and water strengthens the water-based drilling fluid, and uses anti-collapse composition and sealing agent to synergize efficiency to improve the stability and strengthening performance of the well wall.

Benefits of technology

It significantly improves the stability and strengthening performance of the wellbore of the fractured fracture body formation, can effectively seal the cracks in the range of submicrons to 200 microns, enhance the cementitious force between broken rocks, maintain the stability of the well wall, and strong lithocarriage, which is suitable for breaking. Application in drilling of seam formations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004249628190000071
    Figure BDA0004249628190000071
  • Figure BDA0004249628190000072
    Figure BDA0004249628190000072
  • Figure BDA0004249628190000091
    Figure BDA0004249628190000091
Patent Text Reader

Abstract

The invention provides an anti-sloughing composition and a broken joint body stratum wellbore reinforced water-based drilling fluid. The anti-sloughing composition is prepared from a high-temperature-resistant anti-sloughing agent HTFT, a modified asphalt anti-sloughing agent GLA and C9 petroleum resin. The reinforced water-based drilling fluid for the wellbore in the broken joint body stratum has the following advantages that (1) the inhibition performance is high, and the filtrate loss reduction performance is good; (2) the plugging property is strong, the effective plugging range is wide, and cracks and pores in the range of submicron to 200 microns can be effectively plugged; (3) the cementing capacity is outstanding, the cementing force between broken rocks can be enhanced, and the borehole wall is kept stable; and (4) carrying lithology is strong, the high-shear effect of a drill bit water hole can be resisted, rock debris and falling blocks in a near-bit well section can be removed, and the method is applied to fracture body stratum drilling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of development of tight sandstone oil and gas reservoirs, and in particular relates to an anti-collapse composition and a fracture body stratum wellbore strengthening water-based drilling fluid. Background Art

[0002] The fault body is a large-scale network of fractured pore reservoirs that are controlled by faults and associated folds and are formed near faults (zones) by the superposition of matrix pores and faults and folds. The development of large-area matrix micropores and large-scale effective fracture communication are the main reasons for the formation of reservoirs. The fault body has poor stratum integrity, developed faults and crevices, and has characteristics such as abnormal sequence, formation fragmentation, and abnormal pressure. The exploration and development of tight sandstone targets the fault body, and the well deployment mode is "large faults must be relied on and small faults must be penetrated", which is more likely to lead to poor well wall stability, block falling, drilling tool stuck, frequent well leakage, and secondary well control risks. The prominent wellbore instability has become a fatal weakness, and the drilling project faces extreme challenges.

[0003] In order to solve the problem of wellbore instability in fault body formations, a variety of drilling fluid systems are currently used, such as potassium-based polysulfonate drilling fluid, composite salt strong inhibition polysulfonate anti-collapse drilling fluid and strong plugging oil-based drilling fluid, but none of them can effectively solve the problem of wellbore instability in fault body formations. Therefore, it is necessary to develop a water-based drilling fluid system suitable for fault body formations. Summary of the invention

[0004] The first aspect of the present invention provides an anti-slump composition, which comprises a high temperature resistant anti-slump agent HTFT, a modified asphalt anti-slump agent GLA and C 9 Petroleum resin.

[0005] According to a specific embodiment of the present invention, the anti-collapse composition comprises 10 to 20 parts by mass of the high temperature resistant anti-collapse agent HTFT, 10 to 20 parts by mass of the modified asphalt anti-collapse agent GLA and 10 to 25 parts by mass of the C 9 Petroleum resin.

[0006] According to a specific embodiment of the present invention, the C 9 The particle size of petroleum resin shall not exceed 80 mesh.

[0007] The second aspect of the present invention provides a water-based drilling fluid, which includes a polyamine inhibitor SMJA-1, a plugging agent, an anti-collapse composition, a viscosity increasing agent TQ-1, a fluid loss reducing agent, bentonite and water;

[0008] The anti-collapse composition is the anti-collapse composition described in the first aspect of the present invention.

[0009] According to a specific embodiment of the present invention, the water-based drilling fluid comprises 5 to 20 parts by mass of the polyamine inhibitor SMJA-1, 50 to 100 parts by mass of the plugging agent, 35 to 60 parts by mass of the anti-collapse composition, 10 to 20 parts by mass of the viscosity enhancer TQ-1, 50 to 80 parts by mass of the fluid loss additive, 30 to 60 parts by mass of the bentonite and 1000 parts by mass of water;

[0010] Preferably, the water-based drilling fluid comprises 5 to 20 parts by mass of the polyamine inhibitor SMJA-1, 50 to 100 parts by mass of the plugging agent, 35 to 60 parts by mass of the anti-collapse composition, 10 to 15 parts by mass of the viscosity enhancer TQ-1, 50 to 80 parts by mass of the fluid loss additive, 60 parts by mass of the bentonite and 1000 parts by mass of water.

[0011] According to a specific embodiment of the present invention, the plugging agent includes nano plugging agent NP-1, film-forming plugging agent FDM-1, ultrafine calcium carbonate and asphalt; and / or

[0012] The fluid loss reducing agent comprises polyanionic cellulose, sulfonated phenolic resin and lignite resin SPNH for drilling fluid.

[0013] According to a specific embodiment of the present invention, the plugging agent includes 5 to 10 parts by mass of the nano plugging agent NP-1, 5 to 20 parts by mass of the film-forming plugging agent FDM-1, 20 to 50 parts by mass of the ultrafine calcium carbonate and 10 to 30 parts by mass of the asphalt;

[0014] and / or

[0015] The fluid loss reducer comprises 10 to 20 parts by mass of the polyanionic cellulose, 20 to 40 parts by mass of the sulfonated phenolic resin and 20 to 40 parts by mass of the lignite resin SPNH for drilling fluid;

[0016] Preferably, the plugging agent comprises 5 to 10 parts by mass of the nano plugging agent NP-1, 5 to 20 parts by mass of the film-forming plugging agent FDM-1, 25 to 50 parts by mass of the ultrafine calcium carbonate and 15 to 20 parts by mass of the asphalt;

[0017] and / or

[0018] The fluid loss additive comprises 10 to 20 parts by mass of the polyanionic cellulose, 20 to 25 parts by mass of the sulfonated phenolic resin and 20 to 35 parts by mass of the lignite resin SPNH for drilling fluid.

[0019] According to a specific embodiment of the present invention, the median particle size of the nano plugging agent NP-1 is 200 to 500 nm; and / or

[0020] The ultrafine calcium carbonate includes ultrafine calcium carbonate with an average particle size of 2500 mesh and ultrafine calcium carbonate with an average particle size of 1200 mesh; and / or

[0021] The average particle size of the asphalt is 7 to 100 μm;

[0022] Preferably, the ultrafine calcium carbonate comprises 10 to 25 parts by mass of ultrafine calcium carbonate having an average particle size of 2500 mesh and 10 to 30 parts by mass of ultrafine calcium carbonate having an average particle size of 1200 mesh; and / or

[0023] The average particle size of the asphalt is 6 to 80 μm;

[0024] Preferably, the ultrafine calcium carbonate comprises 15 to 25 parts by mass of ultrafine calcium carbonate having an average particle size of 2500 mesh and 10 to 25 parts by mass of ultrafine calcium carbonate having an average particle size of 1200 mesh; and / or

[0025] The sulfonated phenolic resin is sulfonated phenolic resin SMP-1.

[0026] According to a specific embodiment of the present invention, it is characterized in that the water-based drilling fluid also includes sodium carbonate and a lubricant;

[0027] Preferably, the amount of the sodium carbonate is 20 parts by mass; and / or the amount of the lubricant is 10 parts by mass;

[0028] Preferably, the water-based drilling fluid further comprises a weighting agent; and / or

[0029] The weighting agent is barite; and / or

[0030] The density of the water-based drilling fluid is 1.2 g / cm 3 Up to 2g / cm 3 ;

[0031] Preferably, the lubricant is SRH-101.

[0032] According to a specific embodiment of the present invention, the water-based drilling fluid is prepared by the following method:

[0033] 1) mixing water and the bentonite, pre-hydrating, to obtain a base slurry;

[0034] 2) The polyamine inhibitor SMJA-1, the plugging agent, the anti-collapse composition, the viscosity increasing agent TQ-1 and the fluid loss reducing agent are mixed to obtain the water-based drilling fluid.

[0035] According to a specific embodiment of the present invention, in step 1), water, sodium carbonate and bentonite are mixed and then prehydrated; and / or

[0036] In step 2), the polyamine inhibitor SMJA-1, the plugging agent, the anti-collapse composition, the viscosity increasing agent TQ-1, the fluid loss additive and the lubricant are mixed, and then a weighting agent is added and mixed to obtain the water-based drilling fluid;

[0037] Preferably, the temperature of the water is 60°C; and / or the duration of the prehydration is 24 hours;

[0038] Preferably, in step 1), the mixture is stirred and mixed at a speed of 600 r / min; and / or

[0039] In step 2), the mixture is stirred and mixed at a rotation speed of 5000 r / min.

[0040] The application of the anti-collapse composition according to the first aspect of the present invention and the water-based drilling fluid according to the second aspect of the present invention in the development of tight sandstone oil and gas reservoirs, especially in drilling in fractured strata.

[0041] The high temperature resistant anti-collapse agent HTFT of the present invention is purchased from Beijing Sanhe Runjing Technology Co., Ltd., and has a temperature resistance of 160°C;

[0042] The modified asphalt anti-collapse agent GLA described in the present invention is purchased from Beijing Sanhe Runjing Technology Co., Ltd. and has a temperature resistance of 180°C;

[0043] The C of the present invention 9 Petroleum resin: C with a softening point of 140°C purchased from Jinan Dahui Chemical Technology Co., Ltd. 9 The petroleum resin particles were crushed by a pulverizer and passed through an 80-mesh sieve to obtain C 9 Petroleum resin particles;

[0044] The bentonite described in the present invention: bentonite for drilling fluid, purchased from Xinjiang Zhongfei Xiazijie Bentonite Co., Ltd.;

[0045] The polyamine inhibitor SMJA-1 described in the present invention was purchased from Jiujiang Lanzhuo New Material Technology Co., Ltd.

[0046] The nano plugging agent NP-1 described in the present invention is purchased from Shak (Tianjin) Petroleum Technology Service Co., Ltd., with a D50 of 200 to 500 nm;

[0047] The film-forming plugging agent FDM-1 for drilling fluid of the present invention was purchased from Chengdu Xiyou Huawei Technology Co., Ltd.;

[0048] The lignite resin SPNH for drilling fluid of the present invention is purchased from Chengdu Chuanfeng Chemical Engineering Co., Ltd.;

[0049] The tackifier TQ-1 described in the present invention: purchased from Hongda Chemical Manufacturing Co., Ltd.;

[0050] The lubricant SRH-101 described in the present invention was purchased from Tianjin Samit Chemical Co., Ltd.

[0051] Beneficial effects of the present invention:

[0052] Aiming at the problems of poor well wall stability, poor suspension and rock carrying performance, insufficient clay mineral hydration inhibition performance and insufficient broken rock cementation capacity in the existing drilling fluid system used for drilling in fractured formations, the present invention provides an anti-collapse composition and a fractured formation wellbore reinforced water-based drilling fluid. The anti-collapse composition comprises a high temperature resistant anti-collapse agent HTFT, a modified asphalt anti-collapse agent GLA and C 9The water-based drilling fluid for strengthening the wellbore of the fractured formation provided by the present invention mainly comprises a polyamine inhibitor SMJA-1, a plugging agent, the anti-collapse composition, a tackifier TQ-1, a fluid loss reducer, bentonite and water, and secondly comprises sodium carbonate, a lubricant and a weighting agent, wherein the plugging agent comprises a nano plugging agent NP-1, a film-forming plugging agent FDM-1, ultrafine calcium carbonate with an average particle size of 2500 mesh, ultrafine calcium carbonate with an average particle size of 1200 mesh and asphalt. In the fractured formation wellbore strengthening water-based drilling fluid, the anti-collapse composition and the plugging agent are synergistically enhanced, which is beneficial to improving the wellbore stability improvement performance and wellbore strengthening performance of the fractured formation wellbore strengthening water-based drilling fluid: the high-temperature and high-pressure filtration loss (150°C, 3.5MPa) of the fractured formation wellbore strengthening water-based drilling fluid after hot rolling aging in a roller heating furnace at 150°C for 24 hours is 27.9 to 35.7mL; the fractures of 50μm, 100μm, and 200μm blocked by the fractured formation wellbore strengthening water-based drilling fluid only leak during the pressure stabilization stage when the pressure reaches 3MPa to 3.5MPa, and they are successfully blocked before that. For cracks in the range of submicron to 200μm, the leakage rate is 27.9 to 35.7mL. The fractures have a strong plugging ability; in the hot rolling test conducted after the fracture body formation wellbore strengthened water-based drilling fluid was hot-rolled and aged in a roller heating furnace at 150°C for 24 hours, the first rolling recovery rate of the Xujiahe outcrop core in the fracture body formation wellbore strengthened water-based drilling fluid was 95.18% to 98.53%; further, the second rolling recovery rate of the Xujiahe outcrop core in clean water after the first rolling recovery was still 87.29% to 95.11%; the rock samples soaked in the fracture body formation wellbore strengthened water-based drilling fluid have higher compressive strength and smaller penetration, specifically, the compressive strength is 190.522 to 205.133 KPa, and the penetration is 3.162 to 3.588 mm. In summary, the fractured body formation wellbore reinforced water-based drilling fluid provided by the present invention has the following advantages: ① strong inhibition and good filtration loss reduction performance; ② strong plugging ability and a wide effective plugging range, which can effectively plug cracks and pores in the range of submicron to 200 microns; ③ outstanding bonding ability, which can enhance the bonding force between broken rocks and maintain the stability of the well wall; ④ strong rock carrying ability, which can resist the high shear effect of the drill bit water hole, ensure the removal of cuttings and fallen blocks in the well section near the drill bit, and is suitable for application in fractured body formation drilling. DETAILED DESCRIPTION

[0053] The present invention will be further described below in conjunction with examples, but the examples of the present invention are only exemplary descriptions, and the implementation methods do not constitute limitations of the present invention under any circumstances.

[0054] The polyanionic cellulose used in Examples 1 to 3 was purchased from Sichuan Mai Te Wei New Materials Co., Ltd.

[0055] Example 1

[0056] The anti-collapse composition used in this embodiment includes 20g of high temperature resistant anti-collapse agent HTFT, 15g of modified asphalt anti-collapse agent GLA and 10g of C 9 Petroleum resin particles;

[0057] Preparation of fracture formation wellbore strengthening water-based drilling fluid:

[0058] Step 1: Take 1000g water, raise the water temperature to 60℃, add 60g drilling fluid bentonite under stirring at 600r / min, stir for 30min, then add 20g Na 2 CO 3 Continue stirring for 30 minutes, and prehydrate at room temperature and pressure for 24 hours to obtain a base slurry;

[0059] Step 2: Add 20 g of polyamine inhibitor SMJA-1 while stirring at a speed of 5000 r / min, and continue stirring for 30 minutes after the addition is completed;

[0060] Step 3: Add 10g of nano plugging agent NP-1, 10g of drilling fluid film-forming plugging agent FDM-1, 20g of ultrafine calcium carbonate with an average particle size of 2500 mesh, 20g of ultrafine calcium carbonate with an average particle size of 1200 mesh, and 20g of asphalt with an average particle size of 6 to 80 μm while stirring at a speed of 5000 r / min, and continue stirring for 30 minutes after the addition is completed;

[0061] Step 4: Add 45 g of the anti-collapse composition while stirring at a speed of 5000 r / min, and continue stirring for 30 minutes after the addition is completed;

[0062] Step 5: add 10 g of polyanionic cellulose, 20 g of sulfonated phenolic resin SMP-1, and 20 g of lignite resin SPNH for drilling fluid at a speed of 5000 r / min while stirring, and continue stirring for 30 min after the addition is completed;

[0063] Step 6: Add 10g of tackifier TQ-1 and 10g of lubricant SRH-101 while stirring at a speed of 5000r / min, and continue stirring for 30min after the addition is completed;

[0064] Step 7: Add barite to adjust the system density to 1.5g / cm 3 , and obtain a fractured formation wellbore reinforced water-based drilling fluid with a pH of 9.

[0065] Example 2

[0066] The anti-collapse composition used in this embodiment includes 15g of high temperature resistant anti-collapse agent HTFT, 20g of modified asphalt anti-collapse agent GLA and 25g of C 9 Petroleum resin particles;

[0067] Preparation of fracture formation wellbore strengthening water-based drilling fluid:

[0068] Step 1: Take 1000g water, raise the water temperature to 60℃, add 60g drilling fluid bentonite under stirring at 600r / min, stir for 30min, then add 20g Na 2 CO 3 Continue stirring for 30 minutes, and prehydrate at room temperature and pressure for 24 hours to obtain a base slurry;

[0069] Step 2: Add 5 g of polyamine inhibitor SMJA-1 while stirring at a speed of 5000 r / min, and continue stirring for 30 minutes after the addition is completed;

[0070] Step 3: Add 5g of nano plugging agent NP-1, 5g of drilling fluid film plugging agent FDM-1, 15g of ultrafine calcium carbonate with an average particle size of 2500 mesh, 10g of ultrafine calcium carbonate with an average particle size of 1200 mesh, and 15g of asphalt with an average particle size of 6 to 80 μm while stirring at a speed of 5000 r / min, and continue stirring for 30 minutes after the addition is completed;

[0071] Step 4: Add 60 g of the anti-collapse composition while stirring at a speed of 5000 r / min, and continue stirring for 30 minutes after the addition is completed;

[0072] Step 5: Add 20 g of polyanionic cellulose, 25 g of sulfonated phenolic resin SMP-1, and 35 g of lignite resin SPNH for drilling fluid at a speed of 5000 r / min while stirring, and continue stirring for 30 min after the addition is completed;

[0073] Step 6: Add 15g of tackifier TQ-1 and 10g of lubricant SRH-101 while stirring at a speed of 5000r / min, and continue stirring for 30min after the addition is completed;

[0074] Step 7: Add barite to adjust the system density to 1.5g / cm 3 , and obtain a fractured formation wellbore reinforced water-based drilling fluid with a pH of 9.

[0075] Example 3

[0076] The anti-collapse composition used in this embodiment includes 10g of high temperature resistant anti-collapse agent HTFT, 10g of modified asphalt anti-collapse agent GLA and 15g of C 9 Petroleum resin particles;

[0077] Preparation of fracture formation wellbore strengthening water-based drilling fluid:

[0078] Step 1: Take 1000g water, raise the water temperature to 60℃, add 60g drilling fluid bentonite under stirring at 600r / min, stir for 30min, then add 20g Na 2 CO 3 Continue stirring for 30 minutes, and prehydrate at room temperature and pressure for 24 hours to obtain a base slurry;

[0079] Step 2: Add 15 g of polyamine inhibitor SMJA-1 while stirring at a speed of 5000 r / min, and continue stirring for 30 minutes after the addition is completed;

[0080] Step 3: Add 10g of nano plugging agent NP-1, 20g of drilling fluid film-forming plugging agent FDM-1, 25g of ultrafine calcium carbonate with an average particle size of 2500 mesh, 25g of ultrafine calcium carbonate with an average particle size of 1200 mesh, and 20g of asphalt with an average particle size of 6 to 80 μm while stirring at a speed of 5000 r / min, and continue stirring for 30 minutes after the addition is completed;

[0081] Step 4: Add 35 g of the anti-collapse composition while stirring at a speed of 5000 r / min, and continue stirring for 30 minutes after the addition is completed;

[0082] Step 5: Add 15 g of polyanionic cellulose PAC, 20 g of sulfonated phenolic resin SMP-1, and 25 g of lignite resin SPNH for drilling fluid at a speed of 5000 r / min while stirring, and continue stirring for 30 min after the addition is completed;

[0083] Step 6: Add 15g of tackifier TQ-1 and 10g of lubricant SRH-101 while stirring at a speed of 5000r / min, and continue stirring for 30min after the addition is completed;

[0084] Step 7: Add barite to adjust the system density to 1.5g / cm 3 , and obtain a fractured formation wellbore reinforced water-based drilling fluid with a pH of 9.

[0085] Experimental evaluation

[0086] 1. Evaluation of basic properties of water-based drilling fluid for fracture formation wellbore strengthening and determination of rolling recovery rate

[0087] The high-temperature and high-pressure filtration meter GGS42-2A of Kence Instrument (Shanghai) Co., Ltd. and the ZNN-D6B six-speed rotary viscometer of the special instrument factory of Qingdao Hisense Optical Communication Co., Ltd. were used to measure the high-temperature and high-pressure filtration loss and rheological properties of the water-based drilling fluid for strengthening the fracture formation wellbore. The XGRL-2 digital roller heating furnace of the special instrument factory of Qingdao Hisense Optical Communication Co., Ltd. and the LHG-2 aging tank of Kence Instrument (Shanghai) Co., Ltd. were used to measure the rolling recovery rate. The specific steps are as follows:

[0088] 1) Determination of high temperature and high pressure filtration loss of water-based drilling fluid in fracture formation wellbore:

[0089] a. Add the fracture body formation wellbore strengthening water-based drilling fluid into the aging tank, and then place the aging tank in a roller heating furnace heated to 150°C for 24 hours to obtain the fracture body formation wellbore strengthening water-based drilling fluid after aging;

[0090] b. The aged drilling fluid obtained in step a is cooled to 60°C, and then added to a high-temperature and high-pressure filtration meter GGS42-2A with a temperature set at 150°C and a pressure difference set at 3.5MPa to measure the high-temperature and high-pressure filtration loss of the fracture body formation wellbore strengthened water-based drilling fluid after aging;

[0091] 2) Determination of basic properties such as rheology:

[0092] ⅰ. Add the fracture body formation wellbore strengthening water-based drilling fluid into the aging tank, and then place the aging tank in a roller heating furnace heated to 150°C for 24 hours to obtain the aged fracture body formation wellbore strengthening water-based drilling fluid;

[0093] ⅱ. The aged fracture body obtained in step ⅰ was cooled to 60 ℃, and the basic parameters such as the rheological properties of the aged fracture body wellbore water-based drilling fluid were determined at 60 ℃ using a six-speed rotary viscometer ZNN-D6B;

[0094] 3) Determination of rolling recovery rate:

[0095] A. Use a 6-10 mesh sieve to sieve the Xujiahe outcrop core, dry it at 105℃ for 4h, and obtain the experimental rock chips, which are placed in a desiccator for later use;

[0096] B. Pour 350mL of fracture formation wellbore strengthening water-based drilling fluid into the aging tank, then add 50g of rock cuttings while stirring to evenly disperse the rock cuttings in the fracture formation wellbore strengthening water-based drilling fluid, and immediately put the aging tank into a roller heating furnace heated to 150℃ for 24 hours;

[0097] C. After the hot rolling is completed, immediately pour the hot-rolled fracture formation wellbore reinforced water-based drilling fluid carrying rock chips in the aging tank into a 40-mesh (0.425mm) sieve, put it into a water tank and rinse it repeatedly with water until the rinsed water is clear (if the rock chips are clumped together, gently separate them to disperse them into particles). Collect the hot-rolled rock chips and put them in a 105℃ oven to dry for 4 hours. Place them in a dryer to cool to room temperature and weigh them. Calculate the single rolling recovery rate R according to formula (1): 1 ;

[0098]

[0099] Among them, R 1 is the one-time rolling recovery rate, %;

[0100] m 1 The mass of the rock cuttings after drying after one rolling recovery, g;

[0101] m is the initial mass of cuttings, g.

[0102] D. The dried rock chips obtained after the first hot rolling in step C are passed through a 40-mesh sieve and weighed. They are dispersed into an aging tank filled with water according to the mass volume ratio of 350 mL of water for every 50 g of the dried rock chips after the first hot rolling. The aging tank is immediately placed in a roller heating furnace heated to 150°C for hot rolling for 16 hours. After the hot rolling is completed, the hot-rolled fracture formation wellbore reinforced water-based drilling fluid carrying rock chips in the aging tank is immediately poured into a 40-mesh (0.425 mm) sieve, placed in a water tank and repeatedly rinsed with water until the rinsed water is clear (if the rock chips are clumped together, gently separate them to disperse the rock chips into particles). The rock chips after the second hot rolling are collected and placed in an oven at 105°C for drying for 4 hours. They are placed in a dryer to cool to room temperature and weighed. The secondary rolling recovery rate R is calculated according to formula (2): 2 ;

[0103]

[0104] Among them, R 2 is the secondary rolling recovery rate, %;

[0105] m 2 is the mass of the secondary rolling recovery cuttings after drying, g;

[0106] m 3 It is the mass of the residue after the rolling recovery cuttings are dried and passed through a 40-mesh sieve, g.

[0107] According to the above method, the basic properties such as high temperature and high pressure filtration loss, rheology and rolling recovery rate of the fracture formation wellbore enhanced water-based drilling fluid prepared in Examples 1 to 3 were measured respectively. The specific results are shown in Table 1.

[0108] Table 1. Basic properties and rolling recovery rate of water-based drilling fluid for fracture formation wellbore strengthening

[0109] index Example 1 Example 2 Example 3 <![CDATA[Φ 600 ]]> 112 107 115 <![CDATA[Φ 300 ]]> 79 75 80 Plastic viscosity (PV) / mPa.s 30 34 30 Dynamic shear force (YP) / Pa 21 24 22 <![CDATA[Initial shear force (G 1 ) / Pa]]> 4 3 4 <![CDATA[Final shear force (G 2 ) / Pa]]> 9 9 10 <![CDATA[High Temperature High Pressure Fluid Loss (HTHP) 150℃ / mL]]> 29.3 35.7 27.9 One-time rolling recovery rate / % 98.53 95.18 98.21 Secondary rolling recovery rate / % 95.11 87.29 94.19

[0110] From the data in Table 1, it can be seen that the fracture body formation wellbore strengthening water-based drilling fluid prepared in Examples 1 to 3 has good rheological energy and other basic properties. The high-temperature and high-pressure filtration loss (150°C, 3.5MPa) after hot rolling aging in a roller heating furnace at 150°C for 24 hours is 27.9 to 35.7mL, and the anti-filtration performance is good; in the hot rolling experiment after the fracture body formation wellbore strengthening water-based drilling fluid prepared in Examples 1 to 3 was hot rolled in a roller heating furnace at 150°C for 24 hours, the Xujiahe outcrop core The primary rolling recovery rate in the fractured formation wellbore reinforced water-based drilling fluid is 95.18% to 98.53%; further, the secondary rolling recovery rate of the Xujiahe outcrop core in clean water after the primary rolling recovery is still 87.29% to 95.11%, indicating that the fractured formation wellbore reinforced water-based drilling fluid prepared in Examples 1 to 3 can effectively enhance the stability of the core surface, the anti-collapse composition and the plugging agent therein synergistically enhance the effectiveness, and the fractured formation wellbore reinforced water-based drilling fluid has good wellbore stability improvement performance.

[0111] 2. Evaluation of the plugging performance of water-based drilling fluid in fracture formation wellbore

[0112] The plugging performance of the fracture body formation wellbore reinforced water-based drilling fluid prepared in Examples 1 to 3 on fractures of different widths is measured, and the specific steps are as follows:

[0113] The 3D printer used in this experiment is the DesktopXLPlus 3D printer from EnvisionTEC, Germany.

[0114] (1) Preparation of cores with different fracture widths: rock samples made of polyphthalamide (PPA) were selected and cores with fracture widths of 50 μm, 100 μm, and 200 μm were prepared using a 3D printer;

[0115] (2) Plugging strength measurement: The prepared core with a specific fracture width was fixed in a core holder. Then, the fracture body formation wellbore reinforced water-based drilling fluid was added to the core holder. The core holder was pressurized at room temperature (specifically, starting from 0.5 MPa, pressurized by 0.5 MPa every 5 minutes, and then stabilized for 5 minutes after pressurization to 4 MPa). The cumulative leakage was observed and recorded before pressurization for 5 minutes. The specific results are shown in Table 2.

[0116] Table 2. Plugging performance of water-based drilling fluid in fracture formation wellbore

[0117]

[0118]

[0119]

[0120] Combined with the data and notes in Table 2, it can be seen that when the reinforced water-based drilling fluid for the fractured formation wellbore prepared in Example 1 is used to plug 50μm cracks, 100μm cracks, and 200μm cracks, leakage only occurs in the steady pressure stage when the pressure reaches 3MPa, 3.5MPa, and 3.5MPa respectively; when the reinforced water-based drilling fluid for the fractured formation wellbore prepared in Example 2 and Example 3 is used to plug 50μm cracks, 100μm cracks, and 200μm cracks, leakage only occurs in the steady pressure stage when the pressure reaches 3MPa. It can be seen that the reinforced water-based drilling fluid for the fractured formation wellbore prepared in Examples 1 to 3 only leaked during the pressure stabilization stage when the pressure reached 3MPa to 3.5MPa, and was successfully blocked before that. This shows that the reinforced water-based drilling fluid for the fractured formation wellbore prepared in Examples 1 to 3 can effectively block cracks of 50μm, 100μm, and 200μm, and has a strong blocking ability for cracks in the submicron to 200 micron range.

[0121] 3. Evaluation of the wellbore strengthening performance of water-based drilling fluid for wellbore strengthening in fractured formations

[0122] The rock samples of the Xujiahe Group II core material were immersed in conventional anti-collapse fault body formation wellbore strengthening water-based drilling fluid and the fault body formation wellbore strengthening water-based drilling fluid prepared in Examples 1 to 3, respectively. The compressive strength was measured using a microporous electro-hydraulic servo concrete pressure testing machine produced by Shanghai Sansi Metrology Instrument Manufacturing Co., Ltd., and the penetration was measured using an intelligent needle penetration tester RP-2801B produced by Hebi Ruipu Instrument Co., Ltd., to evaluate the wellbore strengthening performance of the fault body formation wellbore strengthening water-based drilling fluid.

[0123] The specific method is as follows:

[0124] The conventional anti-collapse fracture formation wellbore strengthening water-based drilling fluid used in this experiment includes 60g bentonite for drilling fluid, 40g soda ash, 4g quicklime, 5g polyamine inhibitor SMJA-1, 8g polyanionic cellulose, 20g sulfonated phenolic resin SMP-1, 20g lignite resin SPNH for drilling fluid, 1g zwitterionic polymer coating agent FA367, 40g lubricant SRH-101 and 1000mL water;

[0125] Among them, the zwitterionic polymer coating agent FA367 is a high molecular weight linear polymer containing cationic, anionic and nonionic groups, purchased from Puyang Meijing Chemical Materials Co., Ltd.;

[0126] The core sample making machine used in this experiment: RHA-27640 core sample making machine, purchased from Beijing Runhengao Instrument Equipment Co., Ltd.;

[0127] The microporous electro-hydraulic servo concrete pressure testing machine used in this experiment was purchased from Shanghai Sansi Measuring Instrument Manufacturing Co., Ltd.

[0128] The needle penetration tester used in this experiment: Intelligent needle penetration tester RP-2801B, purchased from Hebi Ruipu Instrument Co., Ltd.

[0129] ① Rock sample preparation: The cores of the second group of Xujiahe were crushed by a rock crusher and passed through 300 mesh, 240 mesh and 80 mesh sieves respectively to obtain core particles with particle sizes of 300 mesh, 240 mesh and 80 mesh; then the core particles of 300 mesh, 240 mesh and 80 mesh were mixed evenly in a mass ratio of 3:3:4 and put into a core sample preparation machine, and the temperature was set to 100°C and the pressure was set to 50MPa to prepare cylindrical rock samples with a length of 5cm and a diameter of 2.54cm; several rock samples of the same specifications were prepared according to the above method for standby use;

[0130] ② Control group: The prepared rock samples were immersed in conventional anti-collapse water-based drilling fluid for 12 hours, and the water on the surface of the rock samples was absorbed with absorbent paper after being taken out. The compressive strength was measured with a microporous electro-hydraulic servo concrete pressure testing machine at room temperature and normal pressure, and the penetration was measured with a needle penetration tester;

[0131] ③ Experimental group: Take 3 prepared rock samples and immerse them in the fracture formation wellbore reinforced water-based drilling fluid prepared in Examples 1 to 3 for 12 hours, then take them out, dry the water on the surface of the rock samples with absorbent paper, and then measure the compressive strength with a microporous electro-hydraulic servo concrete pressure testing machine at room temperature and normal pressure, and measure the penetration with a penetration tester.

[0132] See Table 3 for specific results.

[0133] Table 3. Wellbore strengthening performance of water-based drilling fluid for wellbore strengthening in fractured formations

[0134] Serial number Compressive strength / KPa Needle penetration / mm Control group 131.522 17.201 Example 1 201.377 3.162 Example 2 190.522 3.588 Example 3 205.133 3.211

[0135] Table 3 shows that the rock samples in the experimental group after being soaked in the fracture formation wellbore strengthening water-based drilling fluid prepared in Examples 1 to 3 have higher compressive strength and smaller penetration, with specific compressive strength of 190.522 to 205.133 KPa and penetration of 3.162 to 3.588 mm; while the rock samples of the same specifications in the control group after being soaked in the conventional anti-collapse fracture formation wellbore strengthening water-based drilling fluid have lower compressive strength and higher penetration, with specific compressive strength of only 131.522 KPa and penetration of up to 17.201 mm. The compressive strength of the rock samples in the experimental group after being soaked in the water-based drilling fluid for strengthening the fractured formation prepared in Examples 1 to 3 was 1.45 to 1.56 times that of the control group, while the penetration of the rock samples of the same specifications in the control group after being soaked in the conventional anti-collapse water-based drilling fluid for strengthening the fractured formation was 4.79 to 5.44 times that of the rock samples in the experimental group, which proves that the water-based drilling fluid for strengthening the fractured formation prepared in Examples 1 to 3 can effectively enhance the strength of the rock samples compared with the conventional anti-collapse water-based drilling fluid for strengthening the fractured formation. This shows that the anti-collapse composition and the plugging agent in the water-based drilling fluid for strengthening the fractured formation prepared in Examples 1 to 3 work synergistically, which helps to enhance the wellbore strengthening ability of the water-based drilling fluid for strengthening the fractured formation.

[0136] Based on the above experimental results, it can be seen that the fracture body formation wellbore reinforced water-based drilling fluid prepared in Examples 1 to 3 has the following advantages: ① strong inhibition and good filtration loss reduction performance; ② strong plugging ability and a wide effective plugging range, which can effectively plug cracks and pores in the range of submicron to 200 microns; ③ outstanding bonding ability, which can enhance the bonding force between broken rocks and maintain the stability of the well wall; ④ strong rock carrying ability, which can resist the high shear effect of the drill bit water hole, ensure the removal of cuttings and fallen blocks in the near-drill bit well section, and is suitable for application in fracture body formation drilling.

[0137] Although the present invention has been described with reference to specific embodiments, it will be appreciated by those skilled in the art that various changes may be made without departing from the true spirit and scope of the present invention. In addition, various changes may be made to the subject matter, spirit and scope of the present invention to adapt to specific situations, materials, material anti-collapse compositions and methods. All of these changes are included within the scope of the claims of the present invention.

Claims

1. An anti-collapse composition comprising a high temperature resistant anti-collapse agent HTFT, a modified asphalt anti-collapse agent GLA and a C9 petroleum resin.

2. The anti-collapse composition according to claim 1, characterized in that: The anti-collapse composition comprises 10 to 20 parts by mass of the high temperature resistant anti-collapse agent HTFT, 10 to 20 parts by mass of the modified asphalt anti-collapse agent GLA and 10 to 25 parts by mass of the C9 petroleum resin.

3. The anti-collapse composition according to claim 1 or 2, characterized in that: The particle size of the C9 petroleum resin is not greater than 80 meshes.

4. A water-based drilling fluid comprising a polyamine inhibitor SMJA-1, a plugging agent, an anti-collapse composition, a tackifier TQ-1, a fluid loss additive, bentonite and water; The anti-collapse composition is the anti-collapse composition according to any one of claims 1 to 3.

5. The water-based drilling fluid according to claim 4, characterized in that: The water-based drilling fluid comprises 5 to 20 parts by mass of the polyamine inhibitor SMJA-1, 50 to 100 parts by mass of the plugging agent, 35 to 60 parts by mass of the anti-collapse composition, 10 to 20 parts by mass of the viscosity enhancer TQ-1, 50 to 80 parts by mass of the fluid loss reducer, 30 to 60 parts by mass of the bentonite and 1000 parts by mass of water.

6. The water-based drilling fluid according to claim 4 or 5, characterized in that: The plugging agent includes nano plugging agent NP-1, film-forming plugging agent FDM-1, ultrafine calcium carbonate and asphalt; and / or The fluid loss reducing agent comprises polyanionic cellulose, sulfonated phenolic resin and lignite resin SPNH for drilling fluid.

7. The water-based drilling fluid according to claim 6, characterized in that: The plugging agent comprises 5 to 10 parts by mass of the nano plugging agent NP-1, 5 to 20 parts by mass of the film-forming plugging agent FDM-1, 20 to 50 parts by mass of the ultrafine calcium carbonate and 10 to 30 parts by mass of the asphalt; and / or The fluid loss additive comprises 10 to 20 parts by mass of the polyanionic cellulose, 20 to 40 parts by mass of the sulfonated phenolic resin and 20 to 40 parts by mass of the lignite resin SPNH for drilling fluid.

8. The water-based drilling fluid according to claim 6 or 7, characterized in that: The median particle size of the nano plugging agent NP-1 is 200 to 500 nm; and / or The ultrafine calcium carbonate includes ultrafine calcium carbonate with an average particle size of 2500 meshes and ultrafine calcium carbonate with an average particle size of 1200 meshes; and / or The average particle size of the asphalt is 7 to 100 μm; Preferably, the ultrafine calcium carbonate comprises 10 to 25 parts by mass of ultrafine calcium carbonate having an average particle size of 2500 meshes and 10 to 30 parts by mass of ultrafine calcium carbonate having an average particle size of 1200 meshes.

9. The water-based drilling fluid according to any one of claims 4 to 8, characterized in that: The water-based drilling fluid also includes sodium carbonate and a lubricant; Preferably, the amount of the sodium carbonate is 20 parts by mass; and / or the amount of the lubricant is 10 parts by mass; Preferably, the water-based drilling fluid further comprises a weighting agent; and / or The weighting agent is barite; and / or The density of the water-based drilling fluid is 1.2 g / cm 3 Up to 2g / cm 3 .

10. Use of the anti-collapse composition according to any one of claims 1 to 3 and the water-based drilling fluid according to any one of claims 4 to 9 in the development of tight sandstone oil and gas reservoirs, especially in drilling in fractured formations.

Citation Information

Patent Citations

  • Elastic micro-sphere anti-collapse drilling fluid

    CN105713583A

  • High-plugging-performance drilling fluid composition and preparation method and application thereof

    CN110205104A

  • Anti-collapse drilling fluid for coal seams, and preparation method thereof

    CN111117579A

  • Anti-sloughing drilling fluid as well as preparation method and application thereof

    CN113637464A