Method for accurately regulating and controlling components of remelted and recycled high-temperature alloy waste powder
Through the calculation and determination of the smelting process and feeding method under vacuum induction smelting conditions, the problem of precise control of the components of high-temperature alloy waste powder is solved, the low-cost preparation of high-temperature alloy powder and the improvement of resource utilization is achieved, and the high-temperature alloy powder is solved. High cost and low resource utilization.
Patent Information
- Application Number
- CN202411112200.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
AI Technical Summary
The low yield of fine powders of high-temperature alloys leads to high cost and low resource utilization, and the precise control of components during remelting and recycling, which affects the acquisition of high-performance printed parts for additive manufacturing.
Under vacuum induction smelting conditions, the smelting process and feeding method are calculated and determined, the vacuum degree and refining temperature are controlled, and the burning loss of elements is corrected. The method of adding feed ingots and filling sheets is used to achieve accurate control of the waste powder components of high-temperature alloys and improve smelting efficiency.
The precise control of the components of high-temperature alloy waste powder and the efficient utilization of resources are achieved, the cost of alloy powder preparation is reduced, the resource utilization is improved, and the low-cost preparation of alloy powders for additive manufacturing is promoted.
Smart Images

Figure CN119020620A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of powder metallurgy, and in particular relates to a method for accurately controlling the remelting and recovery of high-temperature alloy waste powder components. Background Art
[0002] With the development of additive manufacturing technology, the demand for superalloy fine powder (particle size range 15 ~ 53μm) is increasing day by day, mainly used in aerospace, automobile, energy and other fields. At present, the recovery rate of superalloy fine powder in the industry is about 40%, so nearly 60% of the coarse powder cannot be used, resulting in a serious backlog of waste powder, which is the main reason for the high cost of superalloy powder and low resource utilization. Therefore, it is particularly important to develop the recycling of superalloy waste powder.
[0003] For additive manufacturing, precise control of alloy powder composition is a prerequisite for obtaining high-performance printed parts, so precise control of the composition of remelting and recycling high-temperature alloy waste powder becomes the first problem to be solved. Due to the complex composition of high-temperature alloys and the variety of alloying elements, including easily burned elements (Al, Cr, etc.), refractory elements (Mo, W, etc.) and trace elements (C, B, etc.), the difficulty of precise control of the composition of high-temperature alloy powder is increased; secondly, during the smelting of alloy waste powder, due to the gaps between the powder filled in the crucible, it is impossible to melt by electromagnetic induction heat storage, which brings difficulties to the direct remelting of high-temperature alloy waste powder. At present, the recycling and reuse of alloy waste powder has been widely applied abroad, while China is in its infancy and there is a large gap with foreign countries. Therefore, it is urgent to carry out research on the recycling and utilization of alloy waste powder, reduce the cost of high-temperature alloy powder preparation, improve resource utilization, and promote the development of low-cost preparation technology of alloy powder for additive manufacturing. Summary of the invention
[0004] In order to solve the problem of recycling waste high-temperature alloy powder, the purpose of the present invention is to provide a method for accurately controlling the composition of remelting and recovering waste high-temperature alloy powder. This method not only solves the problem of accurately controlling the composition of waste high-temperature alloy powder recycling process and realizes the recycling of alloy powder, but also reduces the preparation cost of high-temperature alloy powder, which is of great significance to the development of alloy powder industry for additive manufacturing.
[0005] The technical solution adopted by the present invention is:
[0006] A method for accurately controlling the composition of waste high-temperature alloy powder by remelting and recycling, comprising the following steps:
[0007] Step 1: Under vacuum induction melting conditions, the melting process and charging method are determined by calculation, including:
[0008] Step 1.1: The vacuum degree of the melting process is controlled at 10Pa~10 -1 Pa;
[0009] Step 1.2, melting and refining temperature T r Controlled at T0+(50~120)℃, T0 is the melting point of the alloy;
[0010] Step 1.3, for volatile element Al, active elements (Y, Ti, Hf) or trace elements (V, Zr), after high-temperature refining, cool down to condensation film, then break the condensation film and add and stir evenly with electromagnetic stirring;
[0011] Step 1.4: The filling order for preparing the filler ingot is: Ni / Co→Cr→Mo, W, Ta→Ni / Co.
[0012] Step 2: Element burnout measurement: Inductively coupled plasma emission spectrometer was used to detect the composition of the initial and post-furnace alloy powders. The contents of different elements i were C io and C if , where C io is the waste powder content, C if is the content of waste powder remelting ingot, the difference between the two is ΔC i ′ is regarded as the burn-off amount of element i in the smelting process, which can be expressed as:
[0013] ΔC i ′=C if -C io ①
[0014] Considering that the element loss is related to the melting temperature, that is, as the temperature increases, the element loss increases, so the formula (3) is modified and can be expressed as:
[0015] ΔC im ′=AΔC i ′ ②
[0016] In the formula, the correction coefficient A=T r / T0;
[0017] Based on the initial component C io With target component C is , calculate the difference ΔC of each element content i ″, can be expressed as:
[0018] ΔC i =C is -C io ③
[0019] Step 3: Preparation of filler ingots: Based on the burnout amount ΔC obtained in step 2 i Difference between content and ΔC i ′, corresponding to the filling amount of each element ΔC i , which can be expressed as:
[0020] ΔC i =ΔC im ′+ΔC i ④
[0021] Assume that the mass of waste powder to be recycled and remelted is m, that is, the filling mass of each element is m i ′, can be expressed as:
[0022] m i ′=mΔC i ⑤
[0023] To synthesize the filler ingot, prepare the material according to the target composition (10% to 20%) m, and add the m of the element i to be filled. i ', that is, obtaining the filling material weight, smelting and synthesizing the filling material ingot and cutting it into filling pieces;
[0024] Step 4: Fill the waste powder and the prefabricated filling sheet in step 3. The filling sheet should be pre-placed in the waste powder to achieve the effect of powder fluxing and improving smelting efficiency;
[0025] Step 5. After completing the loading and presetting of the materials in step 4, put them into the vacuum induction furnace for smelting. The specific smelting process is: to prevent the powder from being extracted by the vacuum system, start the rough vacuum system, start the low vacuum system after 5 minutes, maintain a slow pumping speed, and when the vacuum is within 100Pa, apply a power of 5 to 10Kw, which is helpful to bake the waste powder and remove the moisture carried in the powder; when the vacuum is within 50Pa, apply a power of 15 to 25Kw; when the vacuum is within 10Pa, apply a power of 30 to 40Kw; when the vacuum enters within 1Pa, apply power of 40~50Kw until the powder is completely melted; at this time, start the high vacuum system to keep the vacuum degree at about 0.1Pa; wait for the melt to be clear, measure the melt temperature by contact thermocouple, wait for the temperature to reach T0+100℃, keep it for 5min for high-temperature refining, then cool down to condense the film, raise the temperature again to break the condensed film, measure the temperature to reach T0+50℃, keep it for 15min for low-temperature refining, and then obtain powder ingots or alloy powder according to process requirements.
[0026] Furthermore, in the above-mentioned method for accurately controlling the composition of remelting and recovering high-temperature alloy waste powder, the calculation method of step 1 is:
[0027] Under vacuum induction melting conditions, according to the Hertz-Knudsen-Langmuir equation, the theoretical maximum volatilization rate of alloying element i at the gas-liquid interface is given by:
[0028]
[0029] Where Vi is the volatilization rate of component i, Kg·m -2 ·s-1 ;γi is the activity coefficient of component i in the melt;χi is the molar fraction of component i; is the standard vapor pressure of pure element i, Pa; Mi is the molar mass of component i, g / mol; R is the ideal gas constant, J / (mol·K); T is the melt surface temperature, K;
[0030] According to formula ⑥, the theoretical volatilization rate of different elements and the standard vapor pressure of different components is proportional to each element. The saturated vapor pressure of a pure element is only a function of temperature and can be described by the Clausius-Clapeyron equation:
[0031]
[0032] According to formula ⑦ and the relevant parameters of different alloys in the thermodynamics handbook, the theoretical volatilization rate of each element in the high-temperature alloy melt at different temperatures can be calculated, and the volatility order of different elements at the same temperature can be obtained: Al>Cr>Co>Ni>Y>Ti>V>Hf>Zr>Mo>W>Ta.
[0033] Furthermore, in the above-mentioned method for accurately controlling the composition of waste high-temperature alloy powder by remelting, the process of smelting the filler material to synthesize the filler material ingot in step 3 is:
[0034] Step 3.1, loading the prepared metal elements into the crucible in the order of Ni / Co→Cr→Mo, W, Ta→Ni / Co;
[0035] Step 3.2: Use 45# steel mold tube, preheat the mold tube to 600±20℃, and keep it warm for 2h;
[0036] Step 3.3, use a vacuum induction furnace for smelting, the process is as follows: draw the vacuum degree to 40-50Pa, start to supply power at a low power of 8-12Kw, as the vacuum degree is drawn to 8-15Pa, increase the power to 20Kw, when the vacuum degree reaches 10 -1 Pa, the power is further increased to 30Kw, and the molten steel is completely melted and cleared; a contact thermocouple is used to measure the temperature, and when the temperature reaches T0+(80-120)℃, it is kept warm for 5 minutes, and then the temperature is reduced to condense the film, and then the power is increased to break the condensed film, and the volatile element Al, active elements (Y, Ti, Hf) or trace elements (V, Zr) are added to the melt, and electromagnetic stirring is used for 2 minutes, and then the power is turned off to measure the temperature. When the temperature is adjusted to T0+(40-60)℃, it is cast into the mold tube, and it is taken out of the furnace after standing for 5 minutes to obtain the supplementary ingot. After cooling to room temperature, it is polished and cut for use, and the cutting thickness of the sheet is not less than 10mm.
[0037] Furthermore, in the above-mentioned method for accurately controlling the composition of remelting and recovering waste high-temperature alloy powder, the preset principle of filling the sheet in step 4 is:
[0038] (1) The filling sheet is pre-placed in the core of the waste powder, that is, the area where the magnetic flux lines densely pass through;
[0039] (2) The filling pieces can be arranged in layers according to quantity, and the arrangement method includes but is not limited to
[0040] 1) From the bottom to the top 1 / 3 and 2 / 3 areas, multiple molten pools are obtained to improve melting efficiency;
[0041] 2) If the quantity is small, the filling piece can be placed in the center of the waste powder.
[0042] (3) When arranging the filling sheets in each layer, the filling sheets should cover the entire cross section to increase the area through which the magnetic flux lines pass, thereby achieving the purpose of rapid heating and melting to form a molten pool.
[0043] Furthermore, in the above-mentioned method for accurately controlling the composition of remelting and recovering high-temperature alloy waste powder, in step 5, the working pressure of the rough vacuum system is greater than 1330Pa, the working pressure of the low vacuum system is 1330Pa~0.13Pa, and the working pressure of the high vacuum system is less than 0.13Pa.
[0044] Further, in the above-mentioned method for accurately controlling the composition of waste high-temperature alloy powder by remelting, in step 5, the method for obtaining powder ingots or alloy powders is:
[0045] (1) The melt is directly poured into the mold tube, left to stand for 5 minutes, then taken out of the furnace and cooled to room temperature, and then polished and cut for use to obtain qualified powder ingots;
[0046] (2) Powdering is carried out according to the powder making process, the melt temperature is increased to T0+150~200℃, and the melt is poured into the tundish. The melt flows out from the guide tube. The atomizing gas pressure is 5~10Mpa. The melt is atomized under the action of high-pressure gas and the alloy powder is obtained by collection.
[0047] Advantages and beneficial effects of the present invention:
[0048] The advantage of the present invention is that the volatility characteristics of different elements are determined by combining thermodynamic calculations, and a waste powder remelting and recycling process method is formulated based on this. At the same time, by comparing the initial and post-furnace powder components with the target components, as well as element burn-out correction, the addition amounts of different elements are obtained to ensure accurate control of the alloy composition; in addition, by reasonably placing the filler ingots in the waste powder, multiple molten pools are obtained to improve the smelting efficiency. Based on the above inventions and creations, the waste powder can be flexibly controlled according to the set target composition, solving the problem of accurate control of the remelting and recycling waste powder composition, not only allowing the alloy waste powder to be recycled, but also improving resource utilization, and realizing low-cost preparation of high-temperature alloy powder. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 A schematic diagram of loading waste powder and filling sheets;
[0050] Figure 2 for Figure 1 AA top view. DETAILED DESCRIPTION
[0051] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings and examples of the specification. The following examples are used to illustrate the present invention but cannot be used to limit the scope of the present invention.
[0052] Example 1
[0053] The Co-Cr-Al-Y alloy waste powder is used as the research object. The alloy melting point T0 is 1390℃, the weight of the waste powder is 50kg, and the refining temperature is T r The temperature is 1510℃. The initial waste powder, remelted powder and target composition are shown in Table 1.
[0054] Table 1 Co-Cr-Al-Y composition and filling information
[0055]
[0056]
[0057] According to the requirements, filler ingots are melted. According to the calculation results, 8.79 kg of ingredients are needed to process 50 kg of powder. The prepared metal elements are loaded into the crucible according to Co→Cr→Co; 45# steel mold tube is used, and the mold tube is kept at 600℃ for 2 hours; during the smelting process, the vacuum degree is pumped to 48pa, and the power is transmitted at a low power of 10Kw. As the vacuum degree is pumped to 9Pa, the power is increased to 20Kw. When the vacuum degree enters 0.1Pa, the power is further increased to 30Kw, and the molten steel is completely melted and cleared; contact thermocouples are used to measure the temperature. When the temperature reaches 1510℃, it is kept warm for 5 minutes, then the temperature is lowered to condense the film, and the power is increased to break the condensed film, Al and Y are added to the melt, electromagnetic stirring is used for 2 minutes, and then the power is turned off to measure the temperature. When the temperature is adjusted to about 1440℃, it is cast into the mold tube, and it is taken out of the furnace after standing for 5 minutes. After cooling to room temperature, it is polished and cut for use. The thickness of the sheet cutting is 30mm.
[0058] In the early stage of smelting, the waste powder is loaded into the crucible. At the same time, the filling pieces are pre-placed in the waste powder core, 1 / 3 and 2 / 3 from top to bottom, such as Figure 1 , Figure 2 shown.
[0059] After completing the material filling and presetting, start the rough vacuum system, start the low vacuum system after 5 minutes, maintain a slow pumping speed, when the vacuum is within 100Pa, apply a power of 8Kw to bake the waste powder; when the vacuum is within 40Pa, apply a power of 20Kw; when the vacuum is within 10Pa, apply a power of 35Kw; when the vacuum is within 1Pa, apply a power of 45Kw until the powder is completely melted; at this time, start the high vacuum system to keep the vacuum degree at 0.1Pa; wait for the melt to be clear, measure the melt temperature by contact thermocouple, wait for the temperature to reach 1510℃, keep it for 5min for high temperature refining, then cool down to condense the film, raise the temperature again to break the condensed film, measure the temperature to reach 1440℃, keep it for 15min for low temperature refining, pour it into the mold tube, let it stand for 5min, take it out of the furnace and cool it to room temperature, grind and cut it for use, and take samples of the ingot for chemical analysis. As shown in Table 2, the composition of the alloy ingot is qualified.
[0060] Table 2 Alloy ingot composition
[0061]
[0062]
Claims
1. A method for accurately controlling the composition of waste high-temperature alloy powder by remelting, characterized in that: The following steps are involved: Step 1: Under vacuum induction melting conditions, the melting process and charging method are determined by calculation, including: Step 1.1: The vacuum degree of the melting process is controlled at 10Pa~10 -1 Pa; Step 1.2, melting and refining temperature T r Controlled at T0+(50~120)℃, T0 is the melting point of the alloy; Step 1.3, for volatile elements Al, active elements Y, Ti, Hf or trace elements V, Zr, after high-temperature refining, cool down to a condensed film, then break the condensed film and add and stir evenly with electromagnetic stirring; Step 1.4: The filling order of the filling ingot preparation is: Ni / Co→Cr→Mo, W, Ta→Ni / Co; Step 2: Element burnout measurement: Inductively coupled plasma emission spectrometer was used to detect the composition of the initial and post-furnace alloy powders. The contents of different elements i were C io and C if , where C io is the waste powder content, C if is the content of waste powder remelting ingot, the difference between the two is ΔC i ′ is regarded as the burn-off amount of element i in the smelting process, which can be expressed as: ΔC i ′=C if -C io ① Considering that the element loss is related to the melting temperature, that is, as the temperature increases, the element loss increases, so the formula (3) is modified and can be expressed as: ΔC im ′=AΔC i ′ ② In the formula, the correction coefficient A=T r / T0; Based on the initial component C io With target component C is , calculate the difference ΔC of each element content i ″, can be expressed as: ΔC i ″=C is -C io ③ Step 3: Preparation of filler ingots: Based on the burnout amount ΔC obtained in step 2 i Difference between content and ΔC i ′, corresponding to the filling amount of each element ΔC i , which can be expressed as: ΔC i =ΔC im ′+ΔC i ″ ④ Assume that the mass of waste powder to be recycled and remelted is m, that is, the filling mass of each element is m i ′, can be expressed as: m i ′=mΔC i ⑤ To synthesize the filler ingot, prepare the material according to the target composition (10% to 20%) m, and add the m of the element i to be filled. i ', that is, obtaining the filling material weight, smelting and synthesizing the filling material ingot and cutting it into filling pieces; Step 4: Fill the waste powder and the prefabricated filling sheet in step 3. The filling sheet should be pre-placed in the waste powder to achieve the effect of powder fluxing and improving smelting efficiency; Step 5. After completing the loading and presetting of the materials in step 4, put them into the vacuum induction furnace for smelting. The specific smelting process is: to prevent the powder from being extracted by the vacuum system, start the rough vacuum system, start the low vacuum system after 5 minutes, maintain a slow pumping speed, and when the vacuum is within 100Pa, apply a power of 5 to 10Kw, which is helpful to bake the waste powder and remove the moisture carried in the powder; when the vacuum is within 50Pa, apply a power of 15 to 25Kw; when the vacuum is within 10Pa, apply a power of 30 to 40Kw; when the vacuum enters within 1Pa, apply power of 40~50Kw until the powder is completely melted; at this time, start the high vacuum system to keep the vacuum degree at about 0.1Pa; wait for the melt to be clear, measure the melt temperature by contact thermocouple, wait for the temperature to reach T0+100℃, keep it for 5min for high-temperature refining, then cool down to condense the film, raise the temperature again to break the condensed film, measure the temperature to reach T0+50℃, keep it for 15min for low-temperature refining, and then obtain powder ingots or alloy powder according to process requirements.
2. The method for accurately controlling the composition of waste high-temperature alloy powder by remelting according to claim 1 is characterized in that: The calculation method for step 1 is: Under vacuum induction melting conditions, according to the Hertz-Knudsen-Langmuir equation, the theoretical maximum volatilization rate of alloying element i at the gas-liquid interface is given by: Where Vi is the volatilization rate of component i, Kg·m -2 ·s -1 ;γi is the activity coefficient of component i in the melt;χi is the molar fraction of component i; is the standard vapor pressure of pure element i, Pa; Mi is the molar mass of component i, g / mol; R is the ideal gas constant, J / (mol·K); T is the melt surface temperature, K; According to formula ⑥, the theoretical volatilization rate of different elements and the standard vapor pressure of different components is proportional to each element. The saturated vapor pressure of a pure element is only a function of temperature and can be described by the Clausius-Clapeyron equation: According to formula ⑦ and the relevant parameters of different alloys in the thermodynamics handbook, the theoretical volatilization rate of each element in the high-temperature alloy melt at different temperatures can be calculated, and the volatility order of different elements at the same temperature can be obtained: Al>Cr>Co>Ni>Y>Ti>V>Hf>Zr>Mo>W>Ta.
3. The method for accurately controlling the composition of waste high-temperature alloy powder by remelting according to claim 1 is characterized in that: The process of melting the filler material to synthesize the filler material ingot in step 3 is as follows: Step 3.1, loading the prepared metal elements into the crucible in the order of Ni / Co→Cr→Mo, W, Ta→Ni / Co; Step 3.2: Use 45# steel mold tube, preheat the mold tube to 600±20℃, and keep it warm for 2h; Step 3.3, use a vacuum induction furnace for smelting, the process is as follows: draw the vacuum degree to 40-50Pa, start to supply power at a low power of 8-12Kw, as the vacuum degree is drawn to 8-15Pa, increase the power to 20Kw, when the vacuum degree reaches 10 -1 Pa, the power is further increased to 30Kw, and the steel liquid is completely melted and cleared; a contact thermocouple is used to measure the temperature, and when the temperature reaches T0+(80-120)℃, it is kept warm for 5 minutes, and then the temperature is reduced to condense the film, and then the power is increased to break the condensed film, and the volatile element Al, active elements Y, Ti, Hf or trace elements V, Zr are added to the melt, and electromagnetic stirring is used for 2 minutes, and then the power is turned off to measure the temperature. When the temperature is adjusted to T0+(40-60)℃, it is cast into the mold tube, and it is taken out of the furnace after standing for 5 minutes to obtain the supplementary ingot. After cooling to room temperature, it is polished and cut for use, and the cutting thickness of the sheet is not less than 10mm.
4. The method for accurately controlling the composition of waste high-temperature alloy powder by remelting according to claim 1 is characterized in that: The preset principle for filling the sheet in step 4 is: (1) The filling sheet is pre-placed in the core of the waste powder, that is, the area where the magnetic flux lines densely pass through; (2) The filling pieces can be arranged in layers according to quantity, and the arrangement method includes but is not limited to 1) From the bottom to the top 1 / 3 and 2 / 3 areas, multiple molten pools are obtained to improve melting efficiency; 2) If the quantity is small, the filling piece can be placed in the center of the waste powder. (3) When arranging the filling sheets in each layer, the filling sheets should cover the entire cross section to increase the area through which the magnetic flux lines pass, thereby achieving the purpose of rapid heating and melting to form a molten pool.
5. The method for accurately controlling the composition of waste high-temperature alloy powder by remelting according to claim 1 is characterized in that: In step 5, the working pressure of the rough vacuum system is greater than 1330Pa, the working pressure of the low vacuum system is 1330Pa to 0.13Pa, and the working pressure of the high vacuum system is less than 0.13Pa.
6. The method for accurately controlling the composition of waste high-temperature alloy powder by remelting according to claim 1 is characterized in that: In step 5, the method for obtaining powder ingots or alloy powders is: (1) The melt is directly poured into the mold tube, left to stand for 5 minutes, then taken out of the furnace and cooled to room temperature, and then polished and cut for use to obtain qualified powder ingots; (2) Powdering is carried out according to the powder making process, the melt temperature is increased to T0+150~200℃, and the melt is poured into the tundish. The melt flows out from the guide tube. The atomizing gas pressure is 5~10Mpa. The melt is atomized under the action of high-pressure gas and the alloy powder is obtained by collection.
Citation Information
Cited By
Method for controlling carbon content of nickel-based high-temperature alloy powder prepared from coarse powder return scrap
CN121467712A
Method for controlling carbon content in nickel-based superalloy powder produced from coarse powder return