Ultrafine grain ruthenium-chromium alloy target material and preparation method thereof
Through ball milling and hydrogen heat treatment combined with discharge plasma sintering technology, ultrafine crystal ruthenium chromium alloy targets were prepared, solving the problems of grain refinement and high cost in the prior art, and achieving high density and pure targets with high density and phases preparation.
Patent Information
- Application Number
- CN202411106211.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art is difficult to process the grains of ruthenium chromium alloy targets through smelting casting and deformation, and the thermal isostatic sintering process is long and costly, so the control of the second phase Cr2Ru and Cr3Ru is not ideal, which affects the target material's agility. Density and phase purity.
Using ball mill mixing ruthenium powder and chromium powder, hydrogen heat treatment and low-pressure pre-pressing, combined with discharge plasma sintering (SPS) technology, ultrafine crystal ruthenium chromium alloy targets are prepared, and the grains are avoided abnormal length through two-stage cooling and low-pressure pre-pressing. Large, inhibiting the formation of the second phase.
It realizes the short production cycle and low cost preparation of ruthenium chromium alloy targets, with fine grain size, high density, pure physical phase, only Ru solid solution, no Cr2Ru or Cr3Ru second phase, which improves the performance and reliability of the target sex.
Smart Images

Figure CN119020627A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alloy target materials for magnetron sputtering, and in particular relates to an ultrafine-grained ruthenium-chromium alloy target material and a preparation method thereof. Background Art
[0002] Ruthenium-chromium alloy films have excellent chemical stability, thermal stability, high temperature strength, corrosion resistance, barrier properties, etc., and are widely used in integrated circuits and information storage. With the development of high-tech, the demand for products in these fields continues to expand, showing its good application prospects and attracting attention and development from countries around the world. For example, ruthenium-chromium alloy films are used in diffusion barrier layers in integrated circuits and non-magnetic intermediate layer materials in information storage magnetic recording, which can significantly improve the performance of products.
[0003] These ruthenium-chromium alloy films are usually deposited by sputtering ruthenium-chromium alloy targets of corresponding compositions using magnetron sputtering. Sputtering targets are the key raw materials for preparing thin films by magnetron sputtering, and their quality is one of the main factors determining the performance of thin films. Generally, the more uniform the target composition and the higher the density, the better the deposition efficiency and film uniformity during sputtering, and the better the service life and reliability of the target; in addition, the finer the target grains and the narrower the grain distribution, the higher the sputtering efficiency and the better the uniformity of film deposition. Therefore, the ideal ruthenium-chromium alloy target for magnetron sputtering should have the characteristics of high density, fine grains and pure phases. However, since ruthenium and chromium and their alloys are hard and brittle, it is difficult to refine the grains by smelting, casting and deformation processing, and the second phases Cr2Ru and Cr3Ru are often present in the ruthenium-chromium alloy prepared by the melt-casting process. At present, hot isostatic pressing sintering is commonly used at home and abroad to prepare ruthenium-chromium alloy targets, but the hot isostatic pressing sintering process is long, the sintering cost is high, and the control of the second phases Cr2Ru and Cr3Ru is not ideal. Summary of the invention
[0004] In view of the above-mentioned shortcomings of the prior art, the present invention provides an ultrafine-grained ruthenium-chromium alloy target and a preparation method thereof.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for preparing an ultrafine-grained ruthenium-chromium alloy target comprises the following steps:
[0007] (1) mixing metal ruthenium powder and chromium powder uniformly by ball milling to obtain mixed powder;
[0008] (2) heat treating the mixed powder in a hydrogen atmosphere;
[0009] (3) pre-pressing the heat-treated mixed powder;
[0010] (4) performing spark plasma sintering on the pre-pressed mixed powder to obtain a ruthenium-chromium alloy target blank;
[0011] (5) Grinding and polishing the ruthenium-chromium alloy target blank to obtain an ultrafine-grained ruthenium-chromium alloy target.
[0012] As a preferred embodiment of the present invention, the mass percentage of the metal ruthenium powder in the mixed powder is 40%-60%.
[0013] As a preferred embodiment of the present invention, in the step (1), the ball-to-material ratio of ball milling is 3:1 to 5:1, the ball milling mixing frequency is 5 to 8 Hz, and the time is 8 to 12 hours.
[0014] As a preferred embodiment of the present invention, the heat treatment temperature is 200-400° C. and the time is 1-3 hours.
[0015] As a preferred embodiment of the present invention, the pre-pressing pressure is 10-30 MPa, and the holding time is 20-40 min.
[0016] As a preferred embodiment of the present invention, the spark plasma sintering has a sintering temperature of 1150-1250° C., a pressure of 50-70 MPa, and a time of 10-30 min.
[0017] More preferably, the spark plasma sintering specifically includes the following operations: firstly applying a pressure of 20 to 40 MPa in the furnace, and then evacuating the furnace. -1 Pa, heat the temperature to 400-600℃ at a rate of 50-100℃ / min, and keep it warm for 5-10min; then evacuate the chamber, and when the vacuum degree reaches 10 -2 Pa, increase the temperature to 1150-1250°C at a heating rate of 50-100°C / min, and increase the pressure to 40-70MPa, and keep warm for 10-30min; after the insulation, cool the temperature to 800-600°C at a cooling rate of 50-200°C / min; then release the pressure and cool with the furnace to obtain an ultrafine-grained ruthenium-chromium alloy target blank.
[0018] The present invention also claims to protect the ultrafine-grained ruthenium-chromium alloy target prepared by the method for preparing the ultrafine-grained ruthenium-chromium alloy target.
[0019] As a preferred embodiment of the present invention, the ultrafine-grained ruthenium-chromium alloy target has a grain size of ≤1 μm, a uniform microstructure, and no abnormally grown grains.
[0020] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention realizes the short production cycle preparation of ruthenium-chromium alloy target by subjecting ruthenium powder and chromium powder to hydrogen heat treatment, low-pressure pre-pressing and SPS sintering treatment, with short sintering time and low cost, effectively refines the ruthenium-chromium alloy grains, and inhibits the formation of the second phases Cr2Ru and Cr3Ru, so that the phase of the ultrafine-grained ruthenium-chromium alloy target is pure, with only one phase of Ru solid solution and no Cr2Ru or Cr3Ru second phases. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a physical picture of the ultrafine-grained ruthenium-chromium alloy target prepared in Example 1.
[0022] Figure 2 This is a scanning electron microscope image of the fracture surface of the ultrafine-grained ruthenium-chromium alloy target prepared in Example 1.
[0023] Figure 3 This is the X-ray diffraction pattern of the fine-grained ruthenium-chromium alloy target prepared in Example 1. DETAILED DESCRIPTION
[0024] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0025] The method for preparing the ultrafine grained ruthenium-chromium alloy target comprises:
[0026] The present invention uses metal ruthenium powder and chromium powder with a purity of ≥99.9% and a particle size of ≤0.5μm as raw materials, weighs the raw material powder according to a ruthenium atom ratio of 40-60%, weighs zirconium oxide grinding balls according to a ball-to-material ratio of 3:1-5:1, and then places them in a resin ball mill; uses a planetary ball mill to mix for 8-12 hours, pauses for 10 minutes after each ball milling, and the ball milling frequency is 5-8Hz.
[0027] The mixed powder is placed in a tube furnace, hydrogen is passed at a flow rate of 10-15m3 / h, and after 5-10 minutes, the temperature is raised to 200-400°C at a rate of 5-10°C / min for heat treatment, and the heat treatment time is 1-3 hours; thereafter, the furnace is cooled to room temperature, and the hydrogen is turned off. The present invention adopts low-temperature calcination to remove adsorbed water vapor.
[0028] The heat-treated mixed powder is loaded into a high-strength graphite mold lined with ruthenium foil. Carbon paper is used as a partition between the ruthenium foil and the graphite mold. Low-pressure pre-pressing is performed by a hydraulic press. The pressing pressure is 10-30 MPa and the holding time is 20-40 minutes. Low-pressure pressing is conducive to the gas overflowing from the powder during spark plasma sintering, while taking into account the metallurgical bonding of the powder particles, thereby ensuring uniform density and small grain size; high-pressure pressing is not conducive to the overflow of gas during the sintering process, and higher strain will cause the powder particles to have undesirable phenomena such as preferential orientation and abnormal grain growth during the sintering process.
[0029] The graphite mold is wrapped with carbon felt, placed in a spark plasma sintering (SPS) furnace and subjected to a pressure of 20-40 MPa, and then evacuated. When the vacuum reaches 10 -1 Pa, heat the temperature to 400-600℃ at a rate of 50-100℃ / min and keep it at that temperature for 5-10min; then evacuate the chamber and when the vacuum degree reaches 10 -2 Pa, the temperature is raised to 1150-1250°C at a rate of 50-100°C / min, and the pressure is raised to 40-70MPa, and the temperature is kept for 10-30min; after the temperature is kept, the temperature is lowered to 800-600°C at a rate of 50-200°C / min; the pressure is then slowly released, and the target is cooled with the furnace to obtain an ultrafine grain ruthenium-chromium alloy target blank. The present invention adopts a two-stage cooling method, which can avoid the situation that the material is kept in a high temperature state for a long time due to the too slow cooling rate at a higher temperature, and the diffusion between Ru and Cr cannot be effectively inhibited, resulting in the appearance of the second phase, and also causing the grain size to become larger and the grains to grow abnormally.
[0030] Finally, the ruthenium-chromium alloy target material blank is ground and polished to obtain an ultrafine-grained ruthenium-chromium alloy target product.
[0031] Example 1
[0032] A method for preparing an ultrafine-grained ruthenium-chromium alloy target comprises the following steps:
[0033] (1) Using metal ruthenium powder and chromium powder with a purity of 99.9% and a particle size of ≤0.5 μm as raw materials, the powders are mixed according to the atomic ratio of metal ruthenium powder to chromium powder of 1:1; then, a planetary ball mill is used for ball milling and mixing, the grinding balls are made of zirconium oxide, the ball mill jar is made of resin, the ball-to-material ratio is 5:1, the ball milling mixing time is 12 hours, and the ball milling is paused for 10 minutes after every 1 hour, and the ball milling frequency is 5 Hz.
[0034] (2) Spread the mixed powder evenly in a crucible and place it in a quartz tube of a tube furnace at 10 m 3 / h flow of hydrogen for 5 minutes; then the temperature was raised to 300 ° C at a rate of 10 ° C / min, and kept at this temperature for 2 hours; thereafter, the furnace was cooled to room temperature, the hydrogen was turned off, and the mixed powder after heat treatment was taken out.
[0035] (3) First, a layer of carbon paper and then a layer of ruthenium foil are placed on the inner ring of the high-strength graphite mold; then, the heat-treated mixed powder is loaded into the high-strength graphite mold, and the upper and lower pressure heads in the graphite mold are slowly pressurized by a hydraulic press. When the pressing pressure reaches 20 MPa, the pressure is maintained for 30 minutes, and then the pressure is slowly unloaded.
[0036] (4) After low-pressure pre-pressing, the high-strength graphite mold is wrapped with carbon felt and fixed with graphite rope; the high-strength graphite mold is then placed in a spark plasma sintering (SPS) furnace and a pressure of 30 MPa is applied, and the sintering chamber is evacuated; when the vacuum degree of the sintering chamber reaches 10 -1 Pa, the temperature was raised to 600 °C at a rate of 100 °C / min and kept at that temperature for 5 min; thereafter, the sintering chamber was evacuated and when the vacuum degree reached 10 -2 Pa, the temperature is raised to 1150℃ at a heating rate of 100℃ / min for sintering, and the pressure is raised to 50MPa, and the sintering is kept warm for 20min; after the sintering and heat preservation is completed, the temperature is first lowered to 800℃ at a rate of 100℃ / min; then the furnace is cooled and the pressure is slowly unloaded to obtain an ultrafine-grained chromium alloy target blank, such as Figure 1 shown.
[0037] The ultrafine-grained ruthenium-chromium alloy target material blank is ground and polished to obtain an ultrafine-grained ruthenium-chromium alloy target finished product. Figure 2 From the scanning electron microscope image of the cross-section of the finished product of the ultrafine-grained ruthenium-chromium alloy target prepared in this example, it can be observed that the grains of the ruthenium-chromium alloy target are small and uniform, the grains are equiaxed, and there are no obvious hole defects. Figure 3 The X-ray diffraction pattern of the finished ultrafine-grained ruthenium-chromium alloy target prepared in this example shows that the ruthenium-chromium alloy target is pure in phase, without the second phases Cr2Ru and Cr3Ru. According to the test, the density of the finished ruthenium-chromium alloy target prepared in this example is 99.1%, and the average grain size is about 0.8μm.
[0038] Example 2
[0039] A method for preparing an ultrafine-grained ruthenium-chromium alloy target comprises the following steps:
[0040] Metal ruthenium powder and chromium powder with a purity of 99.9% and a particle size of ≤0.5μm are used as raw materials, and the powders are mixed according to the atomic ratio of metal ruthenium powder to chromium powder of 4:6; then zirconium oxide grinding balls and resin ball mills are used to mix the powders through a planetary ball mill, the ball-to-material ratio is 3:1, the ball milling mixing time is 8h, and the ball milling frequency is 8Hz after each hour of pausing for 10 minutes.
[0041] The mixed powder was spread evenly in a crucible and placed in a quartz tube of a tube furnace at 15 m 3 / h flow of hydrogen for 10 min; then the temperature was raised to 400 °C at a rate of 10 °C / min and kept at that temperature for 1 h; thereafter, the furnace was cooled to room temperature, the hydrogen was turned off, and the mixed powder after heat treatment was taken out.
[0042] First, a layer of carbon paper and then a layer of ruthenium foil are placed on the inner ring of the high-strength graphite mold; then, the heat-treated mixed powder is loaded into the high-strength graphite mold, and the upper and lower pressure heads in the graphite mold are slowly pressurized by a hydraulic press. When the pressing pressure reaches 10MPa, the pressure is maintained for 30 minutes, and then the pressure is slowly unloaded.
[0043] After low-pressure pre-pressing, the high-strength graphite mold is wrapped with carbon felt and fixed with graphite rope; then the high-strength graphite mold is placed in a spark plasma sintering (SPS) furnace and a pressure of 20 MPa is applied, and the sintering chamber is evacuated; when the vacuum degree of the sintering chamber reaches 10 -1 After the temperature drops below 10 Pa, the temperature is raised to 400 °C at a rate of 50 °C / min and kept at this temperature for 10 min. After that, the sintering chamber is evacuated. When the vacuum degree reaches 10 -2 Pa, and then heat the temperature to 1250℃ at a heating rate of 50℃ / min for sintering, and increase the pressure to 70MPa, and sinter and keep warm for 30min; after sintering and keeping warm, first cool the temperature to 600℃ at a cooling rate of 200℃ / min; then cool with the furnace and slowly unload the pressure to obtain an ultrafine-grained chromium alloy target blank.
[0044] The ultrafine grained ruthenium-chromium alloy target blank is ground and polished to obtain an ultrafine grained ruthenium-chromium alloy target product. According to the test, the density of the ruthenium-chromium alloy target product prepared in this example is 99.2%, the average grain size is about 0.9 μm, and the grains are equiaxed. The ruthenium-chromium alloy target prepared in this example is pure in phase, and no second phase Cr2Ru and Cr3Ru are produced.
[0045] Example 3
[0046] A method for preparing an ultrafine-grained ruthenium-chromium alloy target comprises the following steps:
[0047] (1) Using metal ruthenium powder and chromium powder with a purity of 99.9% and a particle size of ≤0.5 μm as raw materials, the powders are mixed according to the atomic ratio of metal ruthenium powder to chromium powder of 1:1; then, a planetary ball mill is used for ball milling and mixing, the grinding balls are made of zirconium oxide, the ball mill jar is made of resin, the ball-to-material ratio is 5:1, the ball milling mixing time is 12 hours, and the ball milling is paused for 10 minutes after every 1 hour, and the ball milling frequency is 5 Hz.
[0048] (2) Spread the mixed powder evenly in a crucible and place it in a quartz tube of a tube furnace at 10 m 3 / h flow of hydrogen for 5 minutes; then the temperature was raised to 300 ° C at a rate of 10 ° C / min, and kept at this temperature for 2 hours; thereafter, the furnace was cooled to room temperature, the hydrogen was turned off, and the mixed powder after heat treatment was taken out.
[0049] (3) First, a layer of carbon paper and then a layer of ruthenium foil are placed on the inner ring of the high-strength graphite mold; then, the heat-treated mixed powder is loaded into the high-strength graphite mold, and the upper and lower pressure heads in the graphite mold are slowly pressurized by a hydraulic press. When the pressing pressure reaches 20 MPa, the pressure is maintained for 30 minutes, and then the pressure is slowly unloaded.
[0050] (4) After low-pressure pre-pressing, the high-strength graphite mold is wrapped with carbon felt and fixed with graphite rope; the high-strength graphite mold is then placed in a spark plasma sintering (SPS) furnace and a pressure of 50 MPa is applied, and the sintering chamber is evacuated; when the vacuum degree of the sintering chamber reaches 10 -2 Pa, and then sintered at a heating rate of 100℃ / min to 1150℃, and raised the pressure to 50MPa, and sintered for 25min. After sintering and heat preservation, the temperature was first cooled to 800℃ at a rate of 100℃ / min, and then cooled with the furnace and the pressure was slowly unloaded to obtain an ultrafine-grained chromium alloy target blank.
[0051] (5) The ultrafine-grained ruthenium-chromium alloy target blank is ground and polished to obtain an ultrafine-grained ruthenium-chromium alloy target product. According to the test, the density of the ruthenium-chromium alloy target product prepared in this example is 99.1%, the average grain size is about 0.83 μm, and the ruthenium-chromium alloy target is pure in phase, without the second phase Cr2Ru and Cr3Ru.
[0052] Comparative Example 1
[0053] A method for preparing an ultrafine-grained ruthenium-chromium alloy target comprises the following steps:
[0054] (1) Using metal ruthenium powder and chromium powder with a purity of 99.9% and a particle size of ≤0.5 μm as raw materials, the powders are mixed according to the atomic ratio of metal ruthenium powder to chromium powder of 1:1; then, a planetary ball mill is used for ball milling and mixing, the grinding balls are made of zirconium oxide, the ball mill jar is made of resin, the ball-to-material ratio is 5:1, the ball milling mixing time is 12 hours, and the ball milling is paused for 10 minutes after every 1 hour, and the ball milling frequency is 5 Hz.
[0055] (2) The uniformly mixed powder is loaded into an isostatic pressing mold of a polyurethane material, and the sealed mold is placed in an isostatic pressing device. The pressure is maintained at 250 MPa for 5 minutes, and the ruthenium-chromium mixed powder is cold isostatically pressed. After molding, the mold is demolded to obtain a ruthenium-chromium alloy blank.
[0056] (3) placing the ruthenium-chromium alloy blank in an alumina crucible in a hydrogen furnace, keeping the temperature at 1100° C. for 30 minutes in a hydrogen atmosphere, and cooling the blank with the furnace after the end of the keeping temperature to obtain a ruthenium-chromium alloy blank with improved purity.
[0057] (4) The ruthenium-chromium alloy blank treated with hydrogen is placed in a vacuum hot pressing device and heated in a vacuum for 10 -3 Pa, 1400℃ for 60min, then yttrium oxide ceramic indenter for in-situ die-free hot rolling slow deformation, the applied pressure is 30MPa, the deformation time is 30min, and the furnace is cooled after the insulation to obtain a 5mm thick, 200mm diameter, ruthenium-chromium alloy sputtering target with a density of 98%, an average grain size of about 19μm, an uneven microstructure, and abnormally grown grains. The ruthenium-chromium alloy target prepared in this comparative example produces second phases Cr2Ru and Cr3Ru.
[0058] Comparative Example 2
[0059] A method for preparing an ultrafine-grained ruthenium-chromium alloy target comprises the following steps:
[0060] (1) Using metal ruthenium powder and chromium powder with a purity of 99.9% and a particle size of ≤0.5 μm as raw materials, the powders are mixed according to the atomic ratio of metal ruthenium powder to chromium powder of 1:1; then, a planetary ball mill is used for ball milling and mixing, the grinding balls are made of zirconium oxide, the ball mill jar is made of resin, the ball-to-material ratio is 5:1, the ball milling mixing time is 12 hours, and the ball milling is paused for 10 minutes after every 1 hour, and the ball milling frequency is 5 Hz.
[0061] (2) The uniformly mixed powder is loaded into an isostatic pressing mold of a polyurethane material, and the sealed mold is placed in an isostatic pressing device. The pressure is maintained at 250 MPa for 5 minutes, and the ruthenium-chromium mixed powder is cold isostatically pressed. After molding, the mold is demolded to obtain a ruthenium-chromium alloy blank.
[0062] (3) Place the ruthenium-chromium alloy blank in an alumina crucible and place it in a hydrogen furnace at 10 m 3 / h flow of hydrogen for 5 minutes; then the temperature was raised to 300 ° C at a rate of 10 ° C / min, kept at this temperature for 2 hours, cooled with the furnace after the end of the heat preservation, and then the hydrogen was turned off to obtain a ruthenium-chromium alloy blank with improved purity.
[0063] (4) The high-strength graphite mold is wrapped with carbon felt and fixed with graphite rope; the high-strength graphite mold is then placed in a spark plasma sintering (SPS) furnace and a pressure of 30 MPa is applied, and the sintering chamber is evacuated; when the vacuum degree of the sintering chamber reaches 10 -1 Pa, the temperature was raised to 600 °C at a rate of 100 °C / min and kept at that temperature for 5 min; thereafter, the sintering chamber was evacuated and when the vacuum degree reached 10 -2 Pa, the temperature is raised to 1150℃ at a heating rate of 100℃ / min for sintering, and the pressure is raised to 50MPa, and the sintering is kept warm for 20min; after the sintering and heat preservation is completed, the temperature is first lowered to 800℃ at a rate of 100℃ / min; then the furnace is cooled and the pressure is slowly unloaded to obtain an ultrafine-grained chromium alloy target blank.
[0064] The ultrafine grained ruthenium-chromium alloy target blank is ground and polished to obtain an ultrafine grained ruthenium-chromium alloy target finished product. According to the test, the density of the ruthenium-chromium alloy target finished product prepared in this example is 96%, the average grain size is about 0.8 μm, and there are micropores inside the target. The ruthenium-chromium alloy target prepared in this comparative example does not produce the second phase Cr2Ru and Cr3Ru.
[0065] In Comparative Example 2, the mixed powder is first pressed under high pressure to form a ruthenium-chromium alloy blank. During the subsequent heat treatment process, it is difficult for hydrogen to contact the interior of the blank and take effect, and the residual gas inside the blank is difficult to overflow and form micropores during the subsequent sintering process. In addition, the higher strain in the pre-pressing will cause the powder particles to have preferential orientation, abnormal grain growth and other undesirable phenomena during the sintering process, resulting in uneven microstructure of the ruthenium-chromium alloy target and difficulty in achieving grain refinement.
[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing an ultrafine-grained ruthenium-chromium alloy target, characterized in that: The steps include: (1) mixing metal ruthenium powder and chromium powder uniformly by ball milling to obtain mixed powder; (2) heat treating the mixed powder in a hydrogen atmosphere; (3) pre-pressing the heat-treated mixed powder; (4) performing spark plasma sintering on the pre-pressed mixed powder to obtain a ruthenium-chromium alloy target blank; (5) Grinding and polishing the ruthenium-chromium alloy target blank to obtain an ultrafine-grained ruthenium-chromium alloy target.
2. The method for preparing an ultrafine-grained ruthenium-chromium alloy target according to claim 1, characterized in that: The mass percentage of the metal ruthenium powder in the mixed powder is 40%-60%.
3. The method for preparing an ultrafine-grained ruthenium-chromium alloy target according to claim 1, characterized in that: In the step (1), the ball-to-material ratio of the ball mill is 3:1 to 5:1, the ball mill mixing frequency is 5 to 8 Hz, and the time is 8 to 12 hours.
4. The method for preparing an ultrafine-grained ruthenium-chromium alloy target according to claim 1, characterized in that: The heat treatment temperature is 200-400° C. and the time is 1-3 hours.
5. The method for preparing an ultrafine-grained ruthenium-chromium alloy target according to claim 1, characterized in that: The pre-pressing pressure is 10-30 MPa, and the holding time is 20-40 min.
6. The method for preparing an ultrafine-grained ruthenium-chromium alloy target according to claim 1, characterized in that: The spark plasma sintering has a sintering temperature of 1150-1250° C., a pressure of 50-70 MPa, and a time of 10-30 min.
7. The method for preparing an ultrafine-grained ruthenium-chromium alloy target according to claim 1, characterized in that: The spark plasma sintering specifically includes the following operations: firstly, applying a pressure of 20-40 MPa in the furnace, and then evacuating the furnace. -1 Pa, heat the temperature to 400-600℃ at a rate of 50-100℃ / min, and keep it warm for 5-10min; then evacuate the chamber, and when the vacuum degree reaches 10 -2 Pa, increase the temperature to 1150-1250°C at a heating rate of 50-100°C / min, and increase the pressure to 40-70MPa, and keep warm for 10-30min; after the insulation, cool the temperature to 800-600°C at a cooling rate of 50-200°C / min; then release the pressure and cool with the furnace to obtain an ultrafine-grained ruthenium-chromium alloy target blank.
8. An ultrafine-grained ruthenium-chromium alloy target prepared by the method for preparing an ultrafine-grained ruthenium-chromium alloy target as claimed in claim 1.
9. The ultrafine-grained ruthenium-chromium alloy target according to claim 8, characterized in that: The grain size of the ultrafine-grained ruthenium-chromium alloy target material is ≤1 μm.
Citation Information
Cited By
Alloy powder and method for producing the same
CN122703006A