Novel high-thermal-conductivity diamond / tungsten composite material and preparation method thereof
Through the discharge plasma sintering process of nickel-plated diamond and tungsten powder, the problem of degradation of tungsten material under high thermal load is solved, the density and thermal conductivity of diamond/tungsten composite materials are improved, and more efficient heat removal is achieved.
Patent Information
- Application Number
- CN202410999906.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-26
AI Technical Summary
Pure tungsten, as a thermally conductive material, is prone to recrystallization and melting under high thermal load conditions, resulting in a decline in material performance. The poor interface bond between diamond and tungsten material leads to a lower density and thermal conductivity of composite materials.
Nickel-plated diamond and tungsten powder are mixed in a specific proportion, and the nickel coating is deposited by magnetron sputtering and discharge plasma sintering is used to prepare high-thermal conduction diamond/tungsten composite materials to improve the interface bonding state and avoid the generation of low-thermal conduction compounds.
The density and thermal conductivity of the composite material are improved, the problem of lack of active force between powder particles is overcome, and the thermal conductivity of the material is enhanced.
Smart Images

Figure CN119020630A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of composite materials, and in particular to a novel high thermal conductivity diamond / tungsten composite material and a preparation method thereof. Background Art
[0002] Tungsten has the advantages of high melting point, high thermal conductivity, high sputtering threshold, low hydrogen retention, etc. It is considered to be one of the most promising plasma-facing (PFM) candidate materials for future nuclear fusion devices. In addition, tungsten and tungsten alloys meet the requirements of aerospace materials and are also widely used in key components such as engine thermal insulation materials in the aerospace field. The current problem is that pure tungsten, as a thermal conductive material, will undergo recrystallization and melting under high heat load conditions, resulting in a decrease in material performance. By increasing the thermal conductivity of tungsten materials and quickly removing heat, the damage to material performance caused by heat load can be reduced.
[0003] Diamond is the material with the highest thermal conductivity in nature, with a thermal conductivity of 1600-2000W / m -1 ·K -1 By adding a low-density, low-expansion diamond reinforcement phase to metal heat dissipation materials (such as silver, aluminum and copper), the thermal conductivity of the matrix can be greatly improved. The preparation of diamond-doped tungsten composite materials is expected to achieve a significant increase in the thermal conductivity of tungsten materials and improve the rapid heat transfer ability of tungsten materials under high heat loads.
[0004] However, due to the large differences in the physical properties of diamond and tungsten materials, the use of traditional forming methods results in poor interface bonding between diamond and tungsten substrate, and brittle and low thermal conductivity tungsten carbon compounds are easily formed at the interface, which are easily broken under stress, leading to defects such as pores in the interface of the composite material, reducing the thermal conductivity of the composite material, resulting in low density and thermal conductivity of the prepared composite material. Summary of the invention
[0005] The main purpose of the present invention is to provide a novel high thermal conductivity diamond / tungsten composite material with higher density and thermal conductivity and a preparation method thereof.
[0006] To achieve the above-mentioned purpose, the present invention provides a novel high thermal conductivity diamond / tungsten composite material, which is sintered by raw materials including nickel-plated diamond and tungsten powder; the nickel-plated diamond is obtained by depositing a nickel coating on the surface of diamond particles with a particle size of 200 to 400 μm, and the particle size of the tungsten powder is 5 to 10 μm.
[0007] Furthermore, in the raw material, the volume fraction of the nickel-plated diamond is 30-60%, and the volume fraction of the tungsten powder is 40-70%.
[0008] Furthermore, the nickel coating has a thickness of 0.4 μm and is deposited on the surface of the diamond particles by magnetron sputtering.
[0009] Further, the following steps are included:
[0010] (1) Preparation of nickel-plated diamond
[0011] Firstly, the diamond particles are ultrasonically treated with concentrated nitric acid, then the diamond particles are ultrasonically cleaned with acetone, and finally the diamond particles are ultrasonically cleaned with deionized water to obtain surface-treated diamonds;
[0012] Depositing a nickel coating on the surface of the surface-treated diamond by magnetron sputtering to obtain nickel-plated diamond;
[0013] (2) Preparation of new high thermal conductivity diamond / tungsten composite materials
[0014] The nickel-plated diamond prepared in step (1) is evenly mixed with tungsten powder, and then sintered by a spark plasma sintering process to obtain the novel high thermal conductivity diamond / tungsten composite material.
[0015] Furthermore, in step (1), the concentration of the concentrated nitric acid is 50%, and the time for ultrasonically treating the diamond particles with the concentrated nitric acid is 1 hour.
[0016] Furthermore, in step (1), the time for ultrasonic cleaning of diamond particles with acetone is more than 30 minutes, and the time for ultrasonic cleaning of diamond particles with deionized water is twice, and each cleaning time is more than 30 minutes.
[0017] The purpose of concentrated nitric acid treatment and subsequent cleaning is to remove impurities on the surface of diamond particles, increase the activity of the diamond surface, and help obtain a coating with better bonding strength.
[0018] Furthermore, the conditions for magnetron sputtering are as follows: first, the vacuum degree is reduced to 5.0×10 -4 Pa, introduce high-purity argon gas to make the chamber pressure reach 1.0Pa, and then turn on the sputtering power, adjust the power to 1.0kW, the negative bias voltage to 300V, and the sputtering time to 0.5h.
[0019] Furthermore, in step (2), the sintering treatment temperature is 1400-1600° C., the time is 3 min, and the pressure is 70 MPa.
[0020] The beneficial effects of the present invention are embodied in:
[0021] The diamond / tungsten composite material adopts spark plasma sintering technology, which can quickly sinter dense materials in a wide temperature range, overcome the disadvantage of no active force between powder particles, help promote the densification of the composite material, and improve the thermal conductivity of the composite material.
[0022] The present invention deposits a uniform, dense and plastic nickel coating on the surface of diamond by magnetron sputtering, thereby improving the interface strength between diamond and tungsten substrate. On the one hand, nickel and diamond undergo an interface reaction to generate nickel carbide (Ni3C), and nickel and tungsten react to generate a tungsten-nickel solid solution, thereby improving the interface bonding state between diamond and tungsten substrate and increasing the density of the composite material. On the other hand, direct contact between diamond and tungsten substrate is avoided, thereby reducing the generation of low thermal conductivity compounds such as tungsten carbide (WC) and ditungsten carbide (W2C) during sintering, thereby increasing the thermal conductivity of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Schematic diagram of the preparation process of the diamond / tungsten composite material of the present invention;
[0024] Figure 2 The microscopic interface structure and schematic diagram of the diamond / tungsten composite material of the present invention. DETAILED DESCRIPTION
[0025] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0026] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or can be obtained by existing known methods; unless otherwise specified, the methods used in the examples of the present invention are methods known to those skilled in the art.
[0027] Example 1
[0028] Preparation of a new type of high thermal conductivity diamond / tungsten composite material
[0029] The raw materials include 30 vol.% nickel-plated diamond and 70 vol.% tungsten powder, wherein the diamond particle size is 200 μm; the purity of tungsten powder is 99.99% and the particle size of tungsten powder is 5 μm; the specific preparation method is as follows:
[0030] (1) Preparation of nickel-plated diamond
[0031] The diamond particles were ultrasonically treated in 50% concentrated nitric acid for 1 hour, and then ultrasonically cleaned with acetone and deionized water for 30 minutes and 60 minutes respectively to obtain surface-treated diamonds.
[0032] The nickel coating was deposited on the surface of the surface treated diamond by magnetron sputtering. Specifically, the vacuum degree of the magnetron sputtering equipment was first reduced to 5.0×10 -4Pa, high-purity argon gas was introduced to make the chamber pressure reach 1.0Pa, and then the sputtering power was turned on, the power was adjusted to 1.0kW, the negative bias voltage was adjusted to 300V, and the sputtering time was 0.5h to obtain nickel-plated diamond with a thickness of 0.4μm;
[0033] (2) Preparation of high thermal conductivity diamond / tungsten composite materials
[0034] The nickel-plated diamond and tungsten powder prepared in step (1) are mixed uniformly in proportion, and the desired diamond / tungsten composite material is prepared by spark plasma sintering, that is, the mixture is kept at 1400° C. and 70 MPa for 3 minutes.
[0035] The diamond / tungsten composite material of this embodiment utilizes the interface reaction between nickel and diamond to generate nickel carbide (Ni3C), and the nickel-tungsten reaction to generate a tungsten-nickel solid solution, thereby improving the interface bonding state between diamond and tungsten substrate and increasing the density of the composite material. In addition, direct contact between diamond and tungsten substrate is avoided, and the generation of low thermal conductivity compounds such as tungsten carbide (WC) and ditungsten carbide (W2C) during the sintering process is reduced, thereby obtaining a high thermal conductivity diamond / tungsten composite material.
[0036] Example 2
[0037] Preparation of a new type of high thermal conductivity diamond / tungsten composite material
[0038] The raw materials include 30 vol.% nickel-plated diamond and 70 vol.% tungsten powder, wherein the diamond particle size is 400 μm; the tungsten powder has a purity of 99.99% and a particle size of 5 μm; the specific preparation method is as follows:
[0039] (1) Preparation of nickel-plated diamond
[0040] The diamond raw material was ultrasonically treated in 50% concentrated nitric acid for 1 hour, and ultrasonically cleaned with acetone and deionized water for 30 minutes and 60 minutes respectively to obtain surface-treated diamond.
[0041] The nickel coating was deposited on the surface of the surface treated diamond by magnetron sputtering. Specifically, the vacuum degree of the magnetron sputtering equipment was first reduced to 5.0×10 -4 Pa, high-purity argon gas was introduced to make the chamber pressure reach 1.0Pa, and then the sputtering power was turned on, the power was adjusted to 1.0kW, the negative bias voltage was adjusted to 300V, and the sputtering time was 0.5h, and a nickel-plated diamond with a thickness of about 0.4μm was obtained;
[0042] (2) Preparation of high thermal conductivity diamond / tungsten composite materials
[0043] The nickel-plated diamond and tungsten powder prepared in step (1) are mixed uniformly in proportion, and the desired diamond / tungsten composite material is prepared by spark plasma sintering, that is, the mixture is kept at 1600° C. and 70 MPa for 3 minutes.
[0044] The diamond / tungsten composite material of this embodiment utilizes the interface reaction between nickel and diamond to generate nickel carbide (Ni3C), and the reaction between nickel and tungsten to generate a tungsten-nickel solid solution, thereby improving the interface bonding state between diamond and tungsten substrate and increasing the density of the composite material. In addition, direct contact between diamond and tungsten substrate is avoided, and the generation of low thermal conductivity compounds such as tungsten carbide (WC) and ditungsten carbide (W2C) during the sintering process is reduced, thereby obtaining a high thermal conductivity diamond / tungsten composite material.
[0045] Example 3
[0046] Preparation of a new type of high thermal conductivity diamond / tungsten composite material
[0047] The raw materials include 40 vol.% nickel-plated diamond and 60 vol.% tungsten powder, wherein the diamond particle size is 400 μm; the tungsten powder has a purity of 99.99% and a particle size of 5 μm; the specific preparation method is as follows:
[0048] (1) Preparation of nickel-plated diamond
[0049] The diamond raw material was ultrasonically treated in 50% concentrated nitric acid for 1 hour, and ultrasonically cleaned with acetone and deionized water for 30 minutes and 60 minutes respectively to obtain surface-treated diamond.
[0050] The nickel coating was deposited on the surface of the surface treated diamond by magnetron sputtering. Specifically, the vacuum degree of the magnetron sputtering equipment was first reduced to 5.0×10 -4 Pa, high-purity argon gas was introduced to make the cavity pressure reach 1.0Pa, and then the sputtering power was turned on, the power was adjusted to 1.0kW, the negative bias voltage was adjusted to 300V, and the sputtering time was 0.5h to obtain nickel-plated diamond with a thickness of about 0.4μm.
[0051] (2) Preparation of high thermal conductivity diamond / tungsten composite materials
[0052] The nickel-plated diamond and tungsten powder prepared in step (1) are mixed uniformly in proportion, and the desired diamond / tungsten composite material is prepared by spark plasma sintering, that is, the mixture is kept at 1600° C. and 70 MPa for 3 minutes.
[0053] The diamond / tungsten composite material of this embodiment utilizes the interface reaction between nickel and diamond to generate nickel carbide (Ni3C), and the reaction between nickel and tungsten to generate a tungsten (nickel) solid solution, thereby improving the interface bonding state between diamond and tungsten substrate and increasing the density of the composite material. In addition, direct contact between diamond and tungsten substrate is avoided, and the generation of low thermal conductivity compounds such as tungsten carbide (WC) and ditungsten carbide (W2C) during the sintering process is reduced, thereby obtaining a high thermal conductivity diamond / tungsten composite material.
[0054] Example 4
[0055] Preparation of a new type of high thermal conductivity diamond / tungsten composite material
[0056] The raw materials include 50 vol.% nickel-plated diamond and 50 vol.% tungsten powder, wherein the diamond particle size is 400 μm; the tungsten powder has a purity of 99.99% and a particle size of 5 μm; the specific preparation method is as follows:
[0057] (1) Preparation of nickel-plated diamond
[0058] The diamond raw material was ultrasonically treated in 50% concentrated nitric acid for 1 hour, and ultrasonically cleaned with acetone and deionized water for 30 minutes and 60 minutes respectively to obtain surface-treated diamond.
[0059] The nickel coating was deposited on the surface of the surface treated diamond by magnetron sputtering. Specifically, the vacuum degree of the magnetron sputtering equipment was first reduced to 5.0×10 -4 Pa, high-purity argon gas was introduced to make the cavity pressure reach 1.0Pa, and then the sputtering power was turned on, the power was adjusted to 1.0kW, the negative bias voltage was adjusted to 300V, and the sputtering time was 0.5h to obtain nickel-plated diamond with a thickness of about 0.4μm.
[0060] (2) Preparation of high thermal conductivity diamond / tungsten composite materials
[0061] The nickel-plated diamond and tungsten powder prepared in step (1) are mixed uniformly in proportion, and the desired diamond / tungsten composite material is prepared by spark plasma sintering, that is, the mixture is kept at 1600° C. and 70 MPa for 3 minutes.
[0062] The diamond / tungsten composite material of this embodiment utilizes the interface reaction between nickel and diamond to generate nickel carbide (Ni3C), and the reaction between nickel and tungsten to generate a tungsten (nickel) solid solution, thereby improving the interface bonding state between diamond and tungsten substrate and increasing the density of the composite material. In addition, direct contact between diamond and tungsten substrate is avoided, and the generation of low thermal conductivity compounds such as tungsten carbide (WC) and ditungsten carbide (W2C) during the sintering process is reduced, thereby obtaining a high thermal conductivity diamond / tungsten composite material.
[0063] Example 5
[0064] Preparation of a new type of high thermal conductivity diamond / tungsten composite material
[0065] The raw materials include 60 vol.% nickel-plated diamond and 40 vol.% tungsten powder, wherein the diamond particle size is 400 μm; the tungsten powder has a purity of 99.99% and a particle size of 5 μm; the specific preparation method is as follows:
[0066] (1) Preparation of nickel-plated diamond
[0067] The diamond raw material was ultrasonically treated in 50% concentrated nitric acid for 1 hour, and ultrasonically cleaned with acetone and deionized water for 30 minutes and 60 minutes respectively to obtain surface-treated diamond.
[0068] The nickel coating was deposited on the surface of the surface treated diamond by magnetron sputtering. Specifically, the vacuum degree of the magnetron sputtering equipment was first reduced to 5.0×10 -4 Pa, high-purity argon gas was introduced to make the cavity pressure reach 1.0Pa, and then the sputtering power was turned on, the power was adjusted to 1.0kW, the negative bias voltage was adjusted to 300V, and the sputtering time was 0.5h to obtain nickel-plated diamond with a thickness of about 0.4μm.
[0069] (2) Preparation of high thermal conductivity diamond / tungsten composite materials
[0070] The nickel-plated diamond and tungsten powder prepared in step (1) are mixed uniformly in proportion, and the desired diamond / tungsten composite material is prepared by spark plasma sintering, that is, the mixture is kept at 1600° C. and 70 MPa for 3 minutes.
[0071] The diamond / tungsten composite material of this embodiment utilizes the interface reaction between nickel and diamond to generate nickel carbide (Ni3C), and the reaction between nickel and tungsten to generate a tungsten (nickel) solid solution, thereby improving the interface bonding state between diamond and tungsten substrate and increasing the density of the composite material. In addition, direct contact between diamond and tungsten substrate is avoided, and the generation of low thermal conductivity compounds such as tungsten carbide (WC) and ditungsten carbide (W2C) during the sintering process is reduced, thereby obtaining a high thermal conductivity diamond / tungsten composite material.
[0072] Structural analysis of materials
[0073] The microstructure analysis of the composite material prepared in Example 5 above shows that Ni forms amorphous NiW or crystalline NiW solid solution by diffusion with W, and at the same time induces C atoms on the surface of diamond to form an amorphous C layer, forming a W-crystalline NiW or amorphous NiW-Ni-amorphous C-Dia interface structure, such as Figure 2 As shown in the figure, the Ni coating effectively avoids the formation of WC and W2C, improves the interface bonding strength between diamond and W phases, greatly reduces the interface thermal resistance of the composite material, and effectively improves the thermal conductivity of the composite material.
[0074] Material performance testing
[0075] The density, compactness and thermal conductivity of the novel high thermal conductivity diamond / tungsten composite material obtained in Examples 1-5 were tested. The results are shown in Table 1.
[0076] Table 1 Performance test results
[0077]
[0078] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A new type of high thermal conductivity diamond / tungsten composite material, characterized in that: The invention is formed by sintering raw materials including nickel-plated diamond and tungsten powder; the nickel-plated diamond is obtained by depositing a nickel coating on the surface of diamond particles with a particle size of 200-400 μm, and the particle size of the tungsten powder is 5-10 μm.
2. The novel diamond / tungsten composite material according to claim 1, characterized in that: In the raw materials, the volume fraction of the nickel-plated diamond is 30-60%, and the volume fraction of the tungsten powder is 40-70%.
3. The novel diamond / tungsten composite material according to claim 1 or 2, characterized in that: The nickel coating has a thickness of 0.4 μm and is deposited on the surface of the diamond particles by magnetron sputtering.
4. The method for preparing the novel diamond / tungsten composite material according to claim 1, 2 or 3, characterized in that: The following steps are involved: (1) Preparation of nickel-plated diamond Firstly, the diamond particles are ultrasonically treated with concentrated nitric acid, then the diamond particles are ultrasonically cleaned with acetone, and finally the diamond particles are ultrasonically cleaned with deionized water to obtain surface-treated diamonds; Depositing a nickel coating on the surface of the surface-treated diamond by magnetron sputtering to obtain nickel-plated diamond; (2) Preparation of new high thermal conductivity diamond / tungsten composite materials The nickel-plated diamond prepared in step (1) is evenly mixed with tungsten powder, and then sintered by a spark plasma sintering process to obtain the novel high thermal conductivity diamond / tungsten composite material.
5. The method for preparing the novel diamond / tungsten composite material according to claim 4, characterized in that: In step (1), the concentration of the concentrated nitric acid is 50%, and the time for ultrasonically treating the diamond particles with the concentrated nitric acid is 1 hour.
6. The method for preparing the novel diamond / tungsten composite material according to claim 4 or 5, characterized in that: In step (1), the time for ultrasonic cleaning of diamond particles with acetone is more than 30 minutes, and the time for ultrasonic cleaning of diamond particles with deionized water is twice, and each cleaning time is more than 30 minutes.
7. The method for preparing the novel diamond / tungsten composite material according to claim 4 or 5, characterized in that: In step (1), the conditions for magnetron sputtering are: first, the vacuum degree is reduced to 5.0×10 -4 Pa, introduce high-purity argon gas to make the chamber pressure reach 1.0Pa, and then turn on the sputtering power, adjust the power to 1.0kW, the negative bias voltage to 300V, and the sputtering time to 0.5h.
8. The method for preparing the high thermal conductivity diamond / tungsten composite material according to claim 4 or 5, characterized in that: In step (2), the sintering temperature is 1400-1600° C., the time is 3 minutes, and the pressure is 70 MPa.
Citation Information
Cited By
Copper-tungsten boron-containing diamond electric resistance welding electrode and preparation method thereof
CN120006152A