Medium-strength and high-toughness titanium alloy and low-cost preparation process method of plate thereof
Through the Ti-Al-Mo-V-Zr-Sn component system and optimized preparation process, the impact toughness and high preparation cost of medium and high toughness titanium alloys are solved, and efficient and low-cost titanium alloy sheet production is achieved. It meets the high strength and high toughness needs of ship and marine engineering.
Patent Information
- Application Number
- CN202411150481.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
AI Technical Summary
The impact toughness of existing medium-strength high-toughness titanium alloys is relatively low, with high production cost and complex process, resulting in low production efficiency and low material yield, making it difficult to meet the application needs in the fields of ships and marine engineering.
Using the Ti-Al-Mo-V-Zr-Sn component system, the titanium alloy component design and preparation process are optimized through electron beam cold bed smelting, machining, multi-fire rolling and annealing heat treatment, combined with surface treatment, and optimize the composition design and preparation process of titanium alloy to reduce oxidation and crack defects, simplify process flow and reduce costs.
It significantly improves the impact toughness of titanium alloy, reduces the preparation cost, simplifies the process flow, improves production efficiency, and obtains high-quality titanium alloy sheets, suitable for mass industrial production, and meets the high strength in the fields of ships and marine engineering. High resilience and low cost demand.
Smart Images

Figure CN119020636A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nonferrous metal processing, and in particular to a medium-strength and high-toughness titanium alloy and a low-cost preparation process method for a plate thereof. Background Art
[0002] Titanium alloys are widely used in aerospace, shipbuilding and marine engineering, petrochemical, 3C electronics, biomedicine and other fields due to their excellent light weight, high specific strength, corrosion resistance, high temperature resistance and non-magnetic properties. Especially in the field of shipbuilding and marine engineering, medium-strength titanium alloys and their plates with a strength of 700MPa or above have good processing performance such as corrosion resistance, easy welding, easy forming and strong plasticity matching, making them an ideal choice for the forming and welding construction of medium and large-sized titanium alloy structural parts. They can greatly reduce the weight of equipment and extend its service life. They are ideal structural metal materials for shipbuilding and marine engineering equipment and can be widely used in equipment superstructures, underwater pressure-resistant and non-pressure-resistant structures in the fields of high-performance ships, submersibles, and offshore platforms.
[0003] However, ships and marine engineering equipment need to continuously withstand the impact of water pressure, undercurrents, wind and waves during service, and the amount of titanium alloy materials used is large. Therefore, titanium alloys are required to have not only high impact toughness, but also low alloy costs to ensure the safe service of the structure and control construction costs. However, the impact energy of existing commonly used titanium alloys for ships and marine engineering, such as TA5, TC4ELI, Ti80, etc., is generally between 24-70J, with low toughness and high overall cost, which has become the main bottleneck restricting its further large-scale application in the field of ships and marine engineering.
[0004] In order to meet the large-scale application needs of lightweight, high-performance, high-reliability, long-life and high-economic-efficiency ships and marine engineering equipment, strongly support the development of marine resources and the protection of marine rights and interests, and promote the implementation of the strategy of building a strong maritime nation, it is particularly important to develop new medium-strength and high-toughness titanium alloy materials and realize their low-cost preparation.
[0005] In the research and development process of titanium alloys, composition design and preparation process are two crucial links. The composition design of existing titanium alloys mainly relies on the joint strengthening of main alloy elements and interstitial impurity elements. However, this design method often leads to poor impact toughness of titanium alloys. At the same time, the traditional titanium alloy preparation process is complicated and requires multiple smelting, forging and machining, resulting in a long production process, low yield, low production efficiency and high production cost. Summary of the invention
[0006] In view of this, the present invention proposes a low-cost preparation process method for medium-strength and high-toughness titanium alloy and its plate, aiming to solve the technical problems of low impact toughness of existing medium-strength and high-toughness titanium alloy and high plate preparation cost and complex process. At the same time, in view of the defects such as oxidation and cracks that are prone to occur in the preparation process of titanium alloy plates, by optimizing the composition design and preparation scheme of the medium-strength and high-toughness titanium alloy, the preparation cost is effectively reduced, the preparation process is simplified, the production efficiency is improved, and the prepared titanium alloy plate has high surface quality without obvious defects such as oxidation and cracks, which meets the needs of practical applications.
[0007] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0008] The first object of the present invention is to disclose a medium-strength and high-toughness titanium alloy, wherein the chemical composition of the titanium alloy is as follows by weight percentage:
[0009] Al: 3.0-6.5%, Mo: 0.5-2.0%, V: 0.5-2.0%, Zr: 1.5-3.0%, Sn: 0.5-2.0%, Fe: ≤0.20%, O ≤0.10%, and the balance is Ti and inevitable impurity elements.
[0010] The first object of the present invention is to disclose a low-cost preparation process for a medium-strength and high-toughness titanium alloy, which is used to prepare the medium-strength and high-toughness titanium alloy as described above, comprising the following steps:
[0011] S1: Ingot smelting: titanium sponge, Al-Mo master alloy, Al-V master alloy, zirconium sponge, Ti-Sn master alloy, aluminum beans, TiO2 powder and titanium residues of the same material are selected, and uniform furnace materials to be smelted are obtained through batching, mixing and distribution processes, and electron beam cold hearth smelting furnace is used to melt the materials into ingots to be used;
[0012] S2: Machining: sawing and surface machining of the ingot, with the thickness of surface machining being ≥3mm;
[0013] S3: Plate rolling, coating the machined titanium alloy ingot with an anti-oxidation coating or a pure titanium layer, and then rolling it into a plate through at least two fires;
[0014] S4: Plate heat treatment, annealing heat treatment of the rolled plate, annealing temperature [Tβ-100, Tβ-20]℃, holding time 1-3h, air cooling after the holding, the annealed microstructure obtained is a dual-state structure, wherein the content of lamellar β transformation structure is ≥15%;
[0015] S5: Surface treatment, using shot blasting pickling, sand blasting pickling or grinding to remove the oxide layer and defects on the surface of the heat-treated plate to obtain a finished titanium alloy plate.
[0016] Furthermore, in step S1, the phase transition point Tβ is measured by metallographic method.
[0017] Furthermore, in step S2, ultrasonic flaw detection and penetrant testing are used to detect internal and surface defects of the machined titanium alloy ingot, wherein the ultrasonic flaw detection meets the Class B requirements of GB / T 5193 "Ultrasonic flaw detection method for titanium and titanium alloy processed products" standard, and the penetrant testing meets the Class I requirements of JB / T 4730 "Non-destructive testing of pressure equipment Part 5: Penetrant testing" standard.
[0018] Furthermore, in step S3, the coating thickness is 0.2-0.4 mm, and the thickness of the pure titanium coating layer is 0.5-2.0 mm.
[0019] Furthermore, in step S3, the heating temperature of the first-fire rolled billet is Tβ±20°C, the holding time is 1.2-1.5min / mm, and the rolling deformation rate is 50-90%; the heating temperature of the second-fire or second-and third-fire rolled billet is [Tβ-80, Tβ-20]°C, the holding time is 1.0-1.2min / mm, and the rolling deformation rate is 60-85%.
[0020] Furthermore, in step S3, the titanium alloy flat ingot billet coated with anti-oxidation coating or coated with pure titanium layer is subjected to peeling, grinding and polishing after first-fire rolling to remove surface cracks and oxide layer defects, and then reverse rolling is performed in the second fire.
[0021] Furthermore, in step S3, when three-fire rolling is required, the billet after the two-fire rolling needs to be sandblasted, pickled or shot blasted, and ground to remove the surface oxide layer and crack defects, and then three-fire heating and rolling are performed.
[0022] Furthermore, in step S3, after each round of rolling is completed, the plate is straightened using an online straightening machine to improve the plate shape.
[0023] Furthermore, in step S4, after annealing is completed, an online hot straightening machine is used to further improve the plate shape.
[0024] Compared with the prior art, the low-cost preparation process of the medium-strength and high-toughness titanium alloy and its plate described in the present invention has the following advantages:
[0025] (1) The medium-strength and high-toughness titanium alloy described in the present invention eliminates the chromium element and optimizes the content and proportion of other alloy elements, successfully developing a titanium alloy material with high strength, high toughness, good processing performance and corrosion resistance, achieving the effect of increasing the impact toughness of titanium alloys commonly used for ships and marine engineering from 24-70J to more than 100J, thereby improving the comprehensive performance of the alloy and broadening its application field.
[0026] (2) The low-cost preparation process method of the medium-strength and high-toughness titanium alloy described in the present invention is based on the above-mentioned improved Ti-Al-Mo-V-Zr-Sn component system medium-strength and high-toughness titanium alloy, and innovates the plate preparation process to obtain low-cost plates, thus solving the industry problem of low-cost preparation of medium-strength and high-toughness titanium alloy plates.
[0027] (3) The low-cost preparation process for the medium-strength and high-toughness titanium alloy and its plate described in the present invention has a simple titanium alloy component system and a wide hot working and heat treatment process window. Within the wide process window, higher impact toughness can be obtained without a significant reduction in strength, achieving a good match between strength and toughness. It has excellent hot working process performance and strength and impact toughness quality stability, and is particularly suitable for mass industrial production, which has important practical value for large-scale high-reliability engineering applications.
[0028] (4) The low-cost preparation process for the medium-strength and high-toughness titanium alloy and its plate described in the present invention has a simple billet making process, shortens the billet making production process by more than 60%, increases the yield rate by more than 8%, increases the production efficiency by more than 2 times, and reduces the production cost by more than 30%, which can significantly reduce the construction cost of titanium alloy plates and equipment components. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:
[0030] Figure 1 This is a schematic diagram of the microstructure of a 30 mm titanium alloy finished plate prepared in Example 1 of the present invention;
[0031] Figure 2 This is a schematic diagram of the microstructure of a 20 mm titanium alloy finished plate prepared in Example 2 of the present invention;
[0032] Figure 3 This is a schematic diagram of the microstructure of a 12 mm titanium alloy finished plate prepared by heat treatment at 900° C. in Example 3 of the present invention;
[0033] Figure 4 Schematic diagram of the microstructure of a 12 mm titanium alloy finished plate prepared by heat treatment at 860° C. in Example 3 of the present invention; DETAILED DESCRIPTION
[0034] In order to make the technical means, objectives and effects of the present invention easy to understand, the embodiments of the present invention are described in detail below with reference to specific drawings.
[0035] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. The descriptions involving "first", "second", etc. in the present invention are only for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0036] In the research and development of titanium alloy materials, medium-strength and high-toughness titanium alloys and high-strength and high-toughness titanium alloys have attracted much attention due to their excellent comprehensive mechanical properties. The design of traditional medium-strength titanium alloys often relies on the joint strengthening effect of the main alloying elements and interstitial impurity elements, especially the addition of oxygen (O), which improves the strength of the alloy to a certain extent, but also has an adverse effect on impact toughness and welding performance. At the same time, traditional alloys are prone to microstructure growth and coarsening during hot working, which limits their further application.
[0037] In response to the problems existing in traditional medium-strength titanium alloys, this application proposes an innovative composition design concept, which aims to improve the impact toughness and comprehensive mechanical properties of the alloy by optimizing the alloy element composition and reducing the content of harmful interstitial elements.
[0038] The present invention discloses a medium-strength and high-toughness titanium alloy. The chemical composition of the titanium alloy is as follows by weight percentage:
[0039] Al: 3.0-6.5%, Mo: 0.5-2.0%, V: 0.5-2.0%, Zr: 1.5-3.0%, Sn: 0.5-2.0%, Fe: ≤0.20%, O ≤0.10%, and the balance is Ti and inevitable impurity elements.
[0040] The research and development mechanism of the medium-strength and high-impact toughness titanium alloy of the present invention is:
[0041] 1. In terms of the design principle of titanium alloy composition, unlike the existing commonly used medium-strength titanium alloys that are strengthened by the main alloying elements and interstitial impurity elements (Note: the actual value of the O content by weight is usually 0.10-0.20%), the titanium alloy composition of this application mainly adopts multi-component main alloying elements to add and strengthen to obtain strength, and reduces the impurity content of O interstitial impurity strengthening elements to improve impact toughness;
[0042] 2. In terms of the design of the main alloying elements of titanium alloy, in addition to adding the commonly used Al and V alloying elements, this application also adds titanium alloy slow diffusion elements Mo, Zr, and Sn, which can effectively slow down the growth and coarsening of the microstructure of titanium alloy during hot processing and near-β high-temperature annealing. At the same time, this application adopts high-temperature annealing in the near-β phase region to obtain a dual-state structure with a lamellar β transformation structure characteristic of more than 15% content to improve impact toughness, and the addition of Mo, Zr, and Sn slow diffusion elements can effectively inhibit the growth and coarsening of α phase and lamellar transformation β phase grains, and obtain a dual-state structure with fine-grained structure characteristics, so as to achieve the improvement of impact toughness without significantly reducing strength, obtain good strength and toughness matching, and achieve a good high-toughness implementation effect, which provides a new idea for the design of medium-strength and high-toughness titanium alloy composition.
[0043] 3. In terms of interstitial impurity element design, a low O element content design is adopted, with a design value of ≤0.10%, preferably ≤0.08%. This is because the O content has a significant adverse effect on the impact toughness and welding performance. Reducing the amount of O interstitial element addition can help improve impact toughness and welding performance, inhibit the occurrence of delayed cracks in welded structural parts under long-term impact conditions, and improve the safe service performance of equipment.
[0044] The medium-strength and high-toughness titanium alloy in this application is invented by innovating the design of titanium alloy material composition. A medium-strength and high-toughness titanium alloy in the Ti-Al-Mo-V-Zr-Sn composition system is invented, and the chromium element in the raw material system is eliminated. A good match between the high strength and high toughness of the titanium alloy is successfully achieved, so that the alloy can maintain high fracture toughness and impact resistance while bearing high stress loads.
[0045] The medium-strength and high-toughness titanium alloy disclosed in this application has successfully developed a titanium alloy material with high strength, high toughness, good processing performance and corrosion resistance by eliminating the chromium element and optimizing the content and proportion of other alloy elements. This improvement not only improves the comprehensive performance of the alloy, but also broadens its application field, which has important technical significance and economic value.
[0046] The present application also discloses a low-cost preparation process for a medium-strength and high-toughness titanium alloy, which is used to prepare the medium-strength and high-toughness titanium alloy of the above composition, comprising the following steps:
[0047] S1: Ingot smelting: titanium sponge, Al-Mo master alloy, Al-V master alloy, zirconium sponge, Ti-Sn master alloy, aluminum beans, TiO2 powder and titanium residues of the same material are selected, and uniform furnace materials to be smelted are obtained through batching, mixing and distribution processes, and electron beam cold hearth smelting furnace is used to melt the materials into ingots to be used;
[0048] S2: Machining: sawing and surface machining of the ingot, with the thickness of surface machining being ≥3mm;
[0049] S3: Plate rolling, the machined titanium alloy flat ingot is coated with an anti-oxidation coating or a pure titanium layer, and then rolled into a plate through 2 to 3 fires;
[0050] S4: Plate heat treatment, annealing heat treatment of the rolled plate, annealing temperature [Tβ-100, Tβ-20]℃, holding time 1-3h, air cooling after the holding, the annealed microstructure obtained is a dual-state structure, wherein the content of lamellar β transformation structure is ≥15%;
[0051] S5: Surface treatment, using shot blasting pickling, sand blasting pickling or grinding to remove the oxide layer and defects on the surface of the heat-treated plate to obtain a finished titanium alloy plate.
[0052] The low-cost preparation process method of medium-strength and high-toughness titanium alloy disclosed in the present application adopts an electron beam cold hearth melting furnace to obtain a cast ingot with uniform composition through one-time melting, thereby ensuring the purity and composition consistency of the raw materials, and eliminating the need for multiple melting and forging, significantly reducing the construction cost of titanium alloy plates and equipment components, and avoiding the energy consumption and raw material waste of multiple melting; subsequently, surface defects are removed through fine machining, and then the material is subjected to multiple rolling, so that the structure is refined and densified during the rolling process, reducing material loss and improving the yield; the rolled plate is subjected to a precisely controlled annealing heat treatment to form a dual-state structure with excellent mechanical properties, so that it meets the requirements of matching medium-high strength and high toughness, and at the same time, the reasonable selection of the annealing temperature range also reduces energy consumption; finally, the oxide layer and defects are removed through surface treatment, thereby improving the appearance quality and corrosion resistance of the product, and obtaining a high-quality finished titanium alloy plate.
[0053] The low-cost preparation process method for medium-strength and high-toughness titanium alloy disclosed in this application, based on the above-mentioned improved Ti-Al-Mo-V-Zr-Sn component system medium-strength and high-toughness titanium alloy, innovates the plate preparation process to obtain low-cost plates, solves the industry problem of low-cost preparation of medium-strength and high-toughness titanium alloy plates, and has broad application prospects in the future.
[0054] As a preferred example of the present application, in step S1, the phase transition point Tβ is measured by metallographic method.
[0055] The precise determination of the phase transition point Tβ of titanium alloy by metallographic method provides a scientific basis for the entire preparation process. Accurate phase transition point information helps to optimize the smelting and heat treatment process parameters, ensure the uniform composition of titanium alloy during the smelting process, avoid overheating or overburning, and ensure that the titanium alloy obtains the expected microstructure and mechanical properties. At the same time, accurate phase transition point determination also helps to control production costs and avoid material waste and increased energy consumption due to improper process parameters.
[0056] As a preferred example of the present application, in step S2, ultrasonic flaw detection and penetrant testing are used to detect internal and surface defects of the machined titanium alloy ingot, wherein the ultrasonic flaw detection meets the Class B requirements of GB / T 5193 "Ultrasonic flaw detection method for titanium and titanium alloy processed products" standard, and the penetrant testing meets the Class I requirements of JB / T 4730 "Non-destructive testing of pressure equipment Part 5: Penetrant testing" standard.
[0057] Ultrasonic flaw detection can effectively detect internal cracks, inclusions and other imperceptible defects, thus avoiding fracture or performance degradation during subsequent processing; penetrant testing can clearly display surface opening defects such as cracks and pores, ensuring the surface quality of the ingots. Through the application of ultrasonic flaw detection and penetrant testing, the internal and surface defects of titanium alloy ingots can be fully and accurately detected to ensure the quality of the ingots, which not only improves the yield and reliability of titanium alloy plates, but also provides a high-quality raw material foundation for subsequent rolling and heat treatment processes, thereby improving overall production efficiency and product quality. At the same time, following relevant standards for testing also ensures the standardization and comparability of the test results.
[0058] As a preferred example of the present application, in step S3, the coating thickness is 0.2-0.4 mm, and the thickness of the pure titanium coating layer is 0.5-2.0 mm.
[0059] By precisely controlling the thickness of the coating and the pure titanium coating, step S3 achieves reliable protection of the titanium alloy substrate. Reasonable thickness design also ensures the stability of the coating structure, avoiding stress concentration problems caused by excessively thick coatings and the risk of losing protective effects due to excessively thin coatings.
[0060] As a preferred example of the present application, in step S3, the heating temperature of the first-fire rolled billet is Tβ±20℃, the holding time is 1.2-1.5min / mm, and the rolling deformation rate is 50-90%; the heating temperature of the second-fire and third-fire rolled billet is [Tβ-80, Tβ-20]℃, the holding time is 1.0-1.2min / mm, and the rolling deformation rate is 60-85%.
[0061] By precisely controlling the heating temperature, holding time and rolling deformation rate of different rolling fires, the optimized rolling of titanium alloy billets is achieved. During the first fire rolling, a temperature close to the phase transformation point Tβ is selected to refine the grains and ensure that the billet has good plasticity. At the same time, an appropriate holding time and a higher rolling deformation rate are set. High temperature, short holding and a larger deformation rate promote uniform deformation and recrystallization of the billet to promote grain refinement; in the subsequent second and third fire rolling, the heating temperature is reduced to a certain range below Tβ to control grain growth. At the same time, by adjusting the holding time and rolling deformation rate, the organizational structure and mechanical properties of the material are further improved, and the material is further strengthened through cumulative deformation. Through this series of temperature, time and deformation rate control, not only the strength and toughness of the titanium alloy plate are improved, but also its surface quality and internal organizational uniformity are improved, laying a solid foundation for the preparation of high-performance titanium alloy products.
[0062] As a preferred example of the present application, in step S3, the titanium alloy flat ingot billet coated with an anti-oxidation coating or coated with a pure titanium layer is subjected to a first-fire rolling and then peeled, ground, and polished to remove surface cracks and oxide layer defects, and then reversing rolling is performed in the second fire. After the titanium alloy billet is subjected to a first-fire rolling, it is subjected to peeling, grinding, and polishing to thoroughly remove defects such as cracks and oxide layers that may exist on the surface. This treatment process ensures the flatness and cleanliness of the billet surface, provides a good foundation for the subsequent second-fire reversing rolling, and reduces the quality problems of the finished product caused by surface defects; the second-fire rolling adopts a reversing method, which helps to evenly distribute the stress inside the material by changing the rolling direction, and avoids the anisotropy generated during the rolling process, thereby further improving the uniformity of the structure and mechanical properties of the titanium alloy sheet, and improving the strength and toughness of the sheet.
[0063] As a preferred example of the present application, in step S3, when three-fire rolling is required, the billet after two-fire rolling needs to be sandblasted, pickled or shot blasted, and ground to remove the surface oxide layer and crack defects, and then three-fire heating and rolling are performed.
[0064] Through sandblasting pickling or shot blasting pickling and grinding treatment, the purpose is to completely remove the surface oxide layer and potential crack defects through the dual effects of mechanical impact and chemical corrosion. The surface of the billet after the second fire rolling is effectively cleaned and flattened, and defects such as oxide layer and cracks are completely eliminated, creating favorable conditions for the subsequent third fire rolling. This setting not only improves the surface quality of the plate during the rolling process, but also avoids internal stress concentration and performance degradation caused by surface defects, so that the final titanium alloy plate has reached a higher level in mechanical properties, corrosion resistance and appearance quality, meeting the strict requirements of high-end application fields.
[0065] As a preferred example of the present application, in step S3, after each round of rolling is completed, an online straightening machine is used to correct the plate shape to improve the plate shape.
[0066] The online straightening machine applies appropriate pressure or tension to make the plate slightly bent in the length direction to offset the original bending or unevenness, thereby achieving the purpose of improving the plate shape. Timely straightening treatment after each round of rolling not only improves the flatness of the plate, but also reduces material waste and processing difficulty in subsequent processing, making the final titanium alloy plate more in line with quality standards and use requirements, and improving the overall competitiveness and market value of the product.
[0067] As a preferred example of the present application, in step S4, the annealed microstructure obtained is a dual-state structure, in which the lamellar β transformation structure content ranges from 15% to 80%. Preferably, in step S4, after annealing is completed, an online hot straightening machine is used to further improve the plate shape. The online hot straightening machine applies precise bending force to the plate at high temperature, and uses the thermoplasticity of the material to adjust the curvature and unevenness of the plate to achieve an ideal plate shape. Combined with the precisely controlled bending force and plate temperature, the plate shape defects that may occur during the annealing process, such as wavy shape, distortion, etc., are successfully corrected. This setting not only improves the appearance quality of the plate, but also optimizes the internal stress distribution of the plate, improves its overall mechanical properties, and enables the heat-treated titanium alloy plate to reach higher standards in plate shape, flatness and mechanical properties, better meeting the needs of high-end application fields.
[0068] The low-cost preparation process method for medium-strength and high-toughness titanium alloy described in this application is achieved through innovative design of main alloying elements and interstitial elements in titanium alloy. The strength is mainly guaranteed by strengthening of the main alloying elements and strengthening of fine grains. As for improving impact toughness, innovative composition design is achieved by adopting a high-temperature annealing process in the near-β phase region to obtain a fine dual-state structure with excellent impact properties. At the same time, a low O content is used to improve the impact properties. Multiple approaches work together to achieve the design goal of a high impact toughness alloy.
[0069] The low-cost preparation process of the medium-strength and high-toughness titanium alloy and its plate described in the present invention has a simple titanium alloy component system, a wide hot working and heat treatment process window, and can obtain high impact toughness within a wide process range without significantly reducing strength, thereby achieving a good match of strength and toughness. In addition, the present invention adopts a single electron beam cold bed furnace smelting to obtain a flat ingot casting, and directly obtains a titanium alloy plate by direct rolling of the flat ingot casting without multiple smelting and forging, which significantly shortens the production process of the billet, improves the yield rate and production efficiency, and reduces the production cost.
[0070] The present invention solves the industry problem of low-cost preparation of medium-strength and high-toughness titanium alloy plates by innovating the design of titanium alloy material composition and preparation process, laying a solid foundation for its wide application in the fields of shipbuilding and marine engineering in the future. The titanium alloy plate of the present invention not only has the mechanical properties of medium-strength and high-toughness, but also has the advantage of low cost, which can well meet the demand for titanium alloys in the field of shipbuilding and marine engineering, and has broad application prospects.
[0071] The low-cost preparation process of the medium-strength and high-toughness titanium alloy and its plate described in the present invention has the following advantages compared with the prior art:
[0072] 1. By innovating the design concept of medium-strength and high-toughness titanium alloy composition, adding slow alloy diffusion elements Mo, Zr, Sn, and controlling the content of interstitial impurity element O, and combining high-temperature heat treatment in the near-β phase region to obtain a dual-state microstructure with excellent impact toughness, a good matching effect of medium-strength and high-toughness of titanium alloy is achieved, and the impact toughness of titanium alloys used in ships and marine engineering is increased from 24-70J to more than 100J.
[0073] 2. The titanium alloy composition system of the present invention is simple, and the hot working and heat treatment process window is wide. Within the wide process window, higher impact toughness can be obtained without significantly reducing the strength, achieving a good match between strength and toughness. It has excellent hot working process performance and strength and impact toughness quality stability, and is particularly suitable for mass industrial production, which has important practical value for large-scale high-reliability engineering applications.
[0074] 3. The present application adopts a single electron beam cold hearth furnace smelting to obtain flat ingot castings, and directly obtains titanium alloy plates by direct rolling of flat ingot castings without multiple smelting and forging. Compared with the existing commonly used ship and marine engineering titanium alloy plates adopting the "2-3 times vacuum consumable arc furnace smelting → multiple heating forging and grinding → machining" billet making process route, the billet production process is shortened by more than 60%, the yield rate is increased by more than 8%, the production efficiency is increased by more than 2 times, and the production cost is reduced by more than 30%, which can significantly reduce the construction cost of titanium alloy plates and equipment components, and has important economic value.
[0075] Example 1: 30mm titanium alloy plate
[0076] Step 1, ingot smelting: select sponge titanium, Al-Mo master alloy, Al-V master alloy, sponge zirconium, Ti-Sn master alloy, aluminum beans, TiO2 powder and titanium residues of the same material and other raw materials, and obtain uniform furnace charge to be smelted through batching, mixing and distribution processes, and use electron beam cold bed melting furnace to melt the ingot into ready-to-use ingot. The alloy element content is measured to be Al: 4.62%, Mo: 1.20%, V: 1.22%, Zr: 2.21%, Sn: 1.2%, Fe: 0.03%, O: 0.066%, and the phase change point is 945℃ measured by metallographic method.
[0077] The second step is machining: sawing and surface machining of the ingot. The surface machining removes 4.0mm of thickness. After machining, the ultrasonic flaw detection of the slab meets the requirements of Class B of GB / T 5193 standard, and the penetration test meets the requirements of Class I of JB / T 4730 standard.
[0078] The third step is plate rolling: the machined titanium alloy flat ingot is coated with anti-oxidation coating, and then rolled into plates through two fires. Among them, the coating thickness is 0.30mm, the heating temperature of the billet in the first fire rolling is 930℃, the holding time is 1.4min / mm, and the rolling process deformation rate is 50%; the heating temperature of the billet in the second fire rolling is 880℃, the holding time is 1.2min / mm, the rolling process deformation rate is 70%, and the rolling target thickness is 30mm; after the first fire rolling, the billet is peeled, ground, and polished to remove surface cracks, oxide layers and other defects, and the second fire is reversed rolling. After rolling, it is straightened by an online straightening machine.
[0079] The fourth step is plate heat treatment: the rolled plate is annealed at 880°C for 2 hours, followed by air cooling. The dual-state microstructure of the titanium alloy finished plate is as follows: Figure 1 As shown, the content of lamellar β transformation structure is 22%; after annealing, the plate is corrected by online hot straightening machine to further improve the plate shape.
[0080] Step 5: Surface treatment: Polishing is used to remove the oxide layer and defects on the surface of the heat-treated plate to obtain a finished titanium alloy plate.
[0081] The 30mm thick titanium alloy finished plate obtained through the above steps has a tensile strength of 765MPa, a yield strength of 702MPa, an elongation of 13.8%, and impact energies of 106J, 109J, and 111J, respectively.
[0082] Example 2: 20mm titanium alloy plate
[0083] Step 1: Ingot smelting: Select raw materials such as sponge titanium, Al-Mo master alloy, Al-V master alloy, sponge zirconium, Ti-Sn master alloy, aluminum beans, TiO2 powder and titanium residues of the same material, and obtain uniform furnace charge to be smelted through batching, mixing and distribution processes. Use electron beam cold bed melting furnace to melt the ingot into ready-to-use ingot. The alloy element content is measured to be Al: 3.67%, Mo: 1.03%, V: 1.02, Zr: 1.99%, Sn: 1.22%, Fe: 0.03%, O: 0.050%, and the phase change point is 938°C measured by metallographic method.
[0084] The second step is machining: sawing and surface machining of the ingot. The surface machining removes 3.5mm of thickness. After machining, the ultrasonic flaw detection of the slab meets the requirements of Class B of GB / T 5193 standard, and the penetration test meets the requirements of Class I of JB / T 4730 standard.
[0085] The third step is plate rolling: the machined titanium alloy flat ingot is coated with a pure titanium layer, and then rolled into a plate through two fires. Among them, the thickness of the pure titanium layer is 1.0mm, the heating temperature of the billet for the first fire rolling is 940℃, the holding time is 1.4min / mm, and the rolling process deformation rate is 67%; the heating temperature of the billet for the second fire rolling is 900℃, the holding time is 1.2min / mm, the rolling process deformation rate is 67%, and the rolling target thickness is 20mm; after the first fire rolling, the billet is peeled, ground, and polished to remove surface cracks, oxide layers and other defects, and the second fire is reversed rolling. After rolling, it is straightened by an online straightening machine.
[0086] The fourth step is plate heat treatment: the rolled plate is annealed at 900°C for 1.5 hours. After the insulation, it is air-cooled. The dual-state microstructure of the titanium alloy finished plate is as follows: Figure 2 As shown, the content of lamellar β transformation structure is 31%; after annealing, the plate is corrected by online hot straightening machine to further improve the plate shape.
[0087] Step 5: Surface treatment: Polishing is used to remove the oxide layer and defects on the surface of the heat-treated plate to obtain a finished titanium alloy plate.
[0088] The 20 mm thick titanium alloy finished plate obtained through the above steps has a tensile strength of 715 MPa, a yield strength of 660 MPa, an elongation of 14.5%, and impact energies of 129 J, 113 J, and 142 J, respectively.
[0089] Example 3: 12mm titanium alloy plate
[0090] Step 1: Ingot smelting: Select raw materials such as sponge titanium, Al-Mo master alloy, Al-V master alloy, sponge zirconium, Ti-Sn master alloy, aluminum beans, TiO2 powder and titanium residues of the same material, and obtain uniform furnace charge to be smelted through batching, mixing and distribution processes. Use electron beam cold bed melting furnace to melt the ingot into ready-to-use ingot. The alloy element content is measured to be Al: 3.45%, Mo: 1.07%, V: 1.12%, Zr: 1.91%, Sn: 1.12%, Fe: 0.04%, O: 0.46%, and the phase change point is 935°C measured by metallographic method.
[0091] The second step is machining: sawing and surface machining of the ingot. The surface machining removes 3.7mm of thickness. After machining, the ultrasonic flaw detection of the slab meets the requirements of Class B of GB / T 5193 standard, and the penetration test meets the requirements of Class I of JB / T 4730 standard.
[0092] The third step is plate rolling: the machined titanium alloy flat ingot is coated with a pure titanium layer, and then rolled into a plate through two fires. Among them, the thickness of the pure titanium layer is 1.0mm, the heating temperature of the billet for the first fire rolling is 940℃, the holding time is 1.4min / mm, and the rolling process deformation rate is 83%; the heating temperature of the billet for the second fire rolling is 900℃, the holding time is 1.2min / mm, the rolling process deformation rate is 65%, and the rolling target thickness is 12mm; after the first fire rolling, the billet is peeled, ground, and polished to remove surface cracks, oxide layers and other defects, and the second fire is reversed rolling. After rolling, it is straightened by an online straightening machine.
[0093] The fourth step is plate heat treatment: the rolled plate is annealed at 900°C for 1.2 hours. After the insulation, it is air-cooled. The dual-state microstructure of the titanium alloy finished plate is as follows: Figure 3 As shown, the content of lamellar β transformation structure is 38%; after annealing, the plate is corrected by online hot straightening machine to further improve the plate shape.
[0094] Step 5: Surface treatment: Polishing is used to remove the oxide layer and defects on the surface of the heat-treated plate to obtain a finished titanium alloy plate.
[0095] The 12 mm thick titanium alloy finished plate obtained through the above steps has a tensile strength of 727 MPa, a yield strength of 671 MPa, an elongation of 16.2%, and impact energies of 138 J, 132 J, and 148 J, respectively.
[0096] At the same time, the annealing temperature is 860℃ for heat treatment of the 12mm thick titanium alloy finished plate. The rest of the process is the same as the above 900℃ heat treatment temperature for preparing the 12mm thick titanium alloy plate. The microstructure obtained is as follows: Figure 4As shown in the figure, the finished plate has a tensile strength of 743MPa, a yield strength of 687MPa, an elongation of 15.2%, and an impact energy of 123J, 127J, and 121J, respectively. It can be seen that the titanium alloy has a wide heat treatment temperature process window and has good strength and impact toughness stability.
[0097] The medium-strength and high-toughness titanium alloy and the low-cost preparation process method of the plate thereof described in the present invention, in view of the deficiencies of the prior art, innovatively proposes a medium-strength and high-toughness titanium alloy of the Ti-Al-Mo-V-Zr-Sn component system, and optimizes the preparation process of the component plate. The prepared titanium alloy plate has a tensile strength of more than 700MPa, a yield strength of more than 650MPa, and an impact energy of more than 100J. It has excellent strength-toughness matching and welding process performance, and has a short production process and low overall cost. It can meet the high-toughness and low-cost use requirements of titanium alloys used in the field of shipbuilding and marine engineering, and has the conditions for mass production and engineering application. The Ti-Al-Mo-V-Zr-Sn component system titanium alloy plate prepared by the present invention has the advantages of medium-strength, high-toughness and low cost, which can well meet the demand for titanium alloys in the ship and marine field, and has broad application prospects in the future.
[0098] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A medium-strength and high-toughness titanium alloy, characterized in that: The chemical composition of the titanium alloy is as follows by weight percentage: Al: 3.0-6.5%, Mo: 0.5-2.0%, V: 0.5-2.0%, Zr: 1.5-3.0%, Sn: 0.5-2.0%, Fe: ≤0.20%, O ≤0.10%, and the balance is Ti and inevitable impurity elements.
2. A low-cost preparation process for medium-strength and high-toughness titanium alloy, characterized in that: The method for preparing the medium-strength and high-toughness titanium alloy as claimed in claim 1 comprises the following steps: S1: Ingot smelting: titanium sponge, Al-Mo master alloy, Al-V master alloy, zirconium sponge, Ti-Sn master alloy, aluminum beans, TiO2 powder and titanium residues of the same material are selected, and uniform furnace materials to be smelted are obtained through batching, mixing and distribution processes, and electron beam cold hearth smelting furnace is used to melt the materials into ingots to be used; S2: Machining: sawing and surface machining of the ingot, with the thickness of surface machining being ≥3mm; S3: Plate rolling, coating the machined titanium alloy ingot with an anti-oxidation coating or a pure titanium layer, and then rolling it into a plate through at least two fires; S4: Plate heat treatment, annealing heat treatment of the rolled plate, annealing temperature [Tβ-100, Tβ-20]℃, holding time 1-3h, air cooling after the holding, the annealed microstructure obtained is a dual-state structure, wherein the content of lamellar β transformation structure is ≥15%; S5: Surface treatment, using shot blasting pickling, sand blasting pickling or grinding to remove the oxide layer and defects on the surface of the heat-treated plate to obtain a finished titanium alloy plate.
3. The low-cost preparation process of medium-strength and high-toughness titanium alloy according to claim 2 is characterized in that: In step S1, the phase transition point Tβ is measured by metallographic method.
4. The low-cost preparation process of medium-strength and high-toughness titanium alloy according to claim 2 is characterized in that: In step S2, ultrasonic flaw detection and penetrant testing are used to detect internal and surface defects of the machined titanium alloy ingot, wherein the ultrasonic flaw detection meets the Class B requirements of GB / T 5193 "Ultrasonic flaw detection method for titanium and titanium alloy processed products" standard, and the penetrant testing meets the Class I requirements of JB / T 4730 "Non-destructive testing of pressure equipment Part 5: Penetrant testing" standard.
5. The low-cost preparation process of medium-strength and high-toughness titanium alloy according to claim 2 is characterized in that: In step S3, the coating thickness is 0.2-0.4 mm, and the thickness of the pure titanium coating layer is 0.5-2.0 mm.
6. The low-cost preparation process of medium-strength and high-toughness titanium alloy according to claim 2 or 5, characterized in that: In step S3, the heating temperature of the first-fire rolled billet is Tβ±20℃, the holding time is 1.2-1.5min / mm, and the rolling deformation rate is 50-90%; the heating temperature of the second-fire or second-fire and third-fire rolled billet is [Tβ-80, Tβ-20]℃, the holding time is 1.0-1.2min / mm, and the rolling deformation rate is 60-85%.
7. The low-cost preparation process of medium-strength and high-toughness titanium alloy according to claim 6 is characterized in that: In step S3, the titanium alloy flat ingot billet coated with an anti-oxidation coating or coated with a pure titanium layer is subjected to a first-fire rolling process, followed by peeling, grinding, and polishing to remove surface cracks and oxide layer defects, and then subjected to a second-fire rolling process.
8. The low-cost preparation process of medium-strength and high-toughness titanium alloy according to claim 7 is characterized in that: In step S3, when three-fire rolling is required, the billet after two-fire rolling needs to be sandblasted, pickled or shot blasted, and ground to remove the surface oxide layer and crack defects, and then three-fire heating and rolling are performed.
9. The low-cost preparation process of medium-strength and high-toughness titanium alloy according to claim 8 is characterized in that: In step S3, after each round of rolling is completed, the plate is straightened using an online straightening machine to improve the plate shape.
10. The low-cost preparation process of medium-strength and high-toughness titanium alloy according to claim 2, characterized in that: In step S4, after annealing is completed, the plate is straightened in an online hot straightening machine to further improve the plate shape.
Citation Information
Cited By
Thermal mechanical treatment method of TC4B titanium alloy for armor
CN119794076A
High-performance low-cost tc32 titanium alloy roll-bond ultra-thin plate and preparation process thereof
CN122669250A