Magnesium alloy, preparation method thereof, battery and electric device

By adding appropriate amounts of aluminum, zinc, manganese and rare earth elements to the magnesium alloy, and adopting protective gas smelting and die-casting processes, the problem of insufficient corrosion resistance of magnesium alloy is solved, the corrosion resistance and mechanical properties of magnesium alloy are improved, and the corrosion resistance and mechanical properties of magnesium alloy are enhanced. Its application potential in aviation, aerospace and other fields.

CN119020647APending Publication Date: 2024-11-26CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310593601.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing magnesium alloys have insufficient corrosion resistance, which limits its further development and application in the fields of aviation, aerospace, chemicals, etc.

Method used

By adding aluminum (Al), zinc (Zn), manganese (Mn) and rare earth elements neodymium (Nd), lanthanum (La), and cerium (Ce) to the magnesium alloy, the mass percentage is controlled to improve the flowability of the magnesium alloy. Mechanical properties and corrosion resistance, protective gas smelting and die-casting processes are used to prepare magnesium alloys.

Benefits of technology

It significantly improves the corrosion resistance and mechanical properties of magnesium alloys, while reducing the content of impurities, enhancing the reliability and application potential of magnesium alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020647A_ABST
    Figure CN119020647A_ABST
Patent Text Reader

Abstract

The invention discloses a magnesium alloy which comprises the following components in percentage by mass: 5-10.5% of Al; zn with a mass percentage of 0.5%-1.2%; the mass percent of Mn is 0.1%-0.5%; the rare earth elements comprise at least one of rare earth elements of Nd, La and Ce, the mass percent of Nd is 0.1%-1%, the mass percent of La is 0.1%-3%, and the mass percent of Ce is 0.1%-3%; and the balance of magnesium (Mg) and impurities. The invention further provides a preparation method of the magnesium alloy, a battery and an electric device. The magnesium alloy disclosed by the invention has relatively good corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a magnesium alloy and a preparation method of the magnesium alloy, a battery and an electrical device. Background Art

[0002] Magnesium alloys have the advantages of low density, high strength, large elastic modulus, good heat dissipation, good shock absorption, and high recycling rate. Magnesium alloys are mainly used in aviation, aerospace, transportation, chemical industry, rocket and other industrial sectors. However, the existing magnesium alloys still have the problem of insufficient corrosion resistance, which limits the further development and application of magnesium alloys. Therefore, it is of great significance to provide a magnesium alloy with good corrosion resistance. Summary of the invention

[0003] In view of the above problems, the present application provides a magnesium alloy and a preparation method thereof, a battery and an electrical device to solve the above technical problems existing in magnesium alloys.

[0004] In a first aspect, the present application provides a magnesium alloy, comprising:

[0005] Aluminum (Al), wherein the mass percentage of Al is 5%-10.5%;

[0006] Zinc (Zn), wherein the mass percentage of Zn is 0.5%-1.2%;

[0007] Manganese (Mn), wherein the mass percentage of Mn is 0.1%-0.5%;

[0008] Rare earth (RE) elements, the rare earth elements comprising at least one of neodymium (Nd), lanthanum (La), and cerium (Ce), wherein the mass percentage of Nd is 0.1%-1%, the mass percentage of La is 0.1%-3%, and the mass percentage of Ce is 0.1%-3%;

[0009] The rest is magnesium (Mg) and impurities.

[0010] In the technical solution of the embodiment of the present application, Al is the main alloying element in the magnesium alloy. The Al element with a mass percentage of 5%-10.5% can increase the fluidity of the magnesium alloy, so that the magnesium alloy can be die-cast; by controlling the mass percentage of Zn to 0.5%-1.2%, the mechanical properties of the magnesium alloy can be improved without affecting the corrosion resistance of the magnesium alloy; by using 0.1%-0.5% by mass of Mn as a trace additive element, it can partially play a role in refining the grains and improving the yield strength of the magnesium alloy; by controlling the mass percentage of Nd to 0.1%-1%, the mass percentage of La to 0.1%-3%, and the mass percentage of Ce to 0.1%-3%, the magnesium alloy has good corrosion resistance while maintaining the mechanical properties of the magnesium alloy basically stable or improved.

[0011] In some embodiments, the mass percentage of Nd is 0.4%-0.6%, the mass percentage of La is 1.0%-1.5%, and the mass percentage of Ce is 1.0%-1.5%.

[0012] In the technical solution of the embodiment of the present application, by controlling the mass percentage of Nd to 0.4%-0.6%, the mass percentage of La to 1.0%-1.5%, and the mass percentage of Ce to 1.0%-1.5%, the corrosion resistance of the magnesium alloy is further improved without significantly increasing the cost.

[0013] In some embodiments, the mass percentage of impurities is less than or equal to 0.05%.

[0014] The content of impurity elements in magnesium alloys is low, which can reduce the impact of impurities on the performance of magnesium alloys.

[0015] In some embodiments, the impurities include at least one of Fe, Cu, Ni, and Si, wherein the mass percentage of Fe in the magnesium alloy is less than or equal to 0.004%, the mass percentage of Cu in the magnesium alloy is less than or equal to 0.02%, the mass percentage of Ni in the magnesium alloy is less than or equal to 0.001%, and the mass percentage of Si in the magnesium alloy is less than or equal to 0.05%.

[0016] In the technical solution of the embodiment of the present application, the content of impurity elements in the magnesium alloy is low, which can have little impact on the performance of the magnesium alloy.

[0017] In a second aspect, the present application provides a method for preparing the magnesium alloy of any of the above embodiments, comprising:

[0018] Providing pure Mg, pure Al, pure Zn, Mg-Mn master alloy, and Mg-RE master alloy according to the mass percentages of Mg, Al, Zn, Mn, and rare earth elements in the above magnesium alloy;

[0019] Mixing pure Mg, pure Al, pure Zn, Mg-RE master alloy and Mg-Mn master alloy and smelting to obtain magnesium alloy liquid, wherein the smelting is performed in a protective gas;

[0020] The magnesium alloy liquid is poured and die-casted in sequence to obtain a magnesium alloy.

[0021] In the technical scheme of the embodiment of the present application, the preparation method of the magnesium alloy is simple. By adding at least one of the rare earth elements Nd, La, and Ce, the morphology of the primary phase can be effectively improved, so that the network Mg-Al alloy Mg17Al12 phase is transformed into a dispersed skeletal or granular state, and a new rare earth phase is formed to prevent the primary phase from growing, thereby refining the magnesium alloy structure and improving the mechanical properties of the magnesium alloy; after at least one of Nd, La, and Ce is added, the melt can be purified in the process of preparing the magnesium alloy to play a role in degassing and slag removal, thereby improving the quality of the melt. During the smelting process, the rare earth elements Nd, La, and Ce easily react with elements such as N, H, and O to form rare earth compounds, reduce the gas content in the melt, and thus improve the corrosion resistance of the magnesium alloy; at the same time, at least one of Nd, La, and Ce can react with the main impurity elements in the magnesium alloy such as Fe, Cu, Ni, and Si to generate high-melting-point binary or multi-component rare earth compounds, reduce the content of impurity elements in the matrix, and the magnesium alloy has good corrosion resistance while maintaining the basic stability or improvement of the mechanical properties of the magnesium alloy.

[0022] In some embodiments, pure Mg is added into a smelting furnace for melting, and pure Al and pure Zn are added after the pure Mg is completely melted, while the temperature of the smelting furnace is maintained and stirring is performed; the temperature is increased, and when the temperature of the smelting furnace reaches 700-720°C, a Mg-RE intermediate alloy is added and stirred; the temperature is continued to be increased, and when the temperature of the smelting furnace reaches 720-740°C, a Mg-Mn intermediate alloy is added and stirred to obtain a magnesium alloy liquid.

[0023] In the technical solution of the embodiment of the present application, Mg-RE intermediate alloy is added at 700-720°C, and Mg-Mn intermediate alloy is added when the temperature reaches 720-740°C, so that the burnout of alloy elements is small, the recovery rate is high, and the dissolution rate of alloy elements is fast.

[0024] In some embodiments, after the step of adding the Mg-Mn master alloy and stirring, the temperature of the smelting furnace is maintained at 720-740° C. for 10-15 minutes to obtain the magnesium alloy liquid.

[0025] In the technical solution of the embodiment of the present application, the molten metal in the smelting furnace is fully mixed and uniformly by maintaining the temperature of the smelting furnace at 720-740°C and standing for 10-15 minutes.

[0026] In some embodiments, the pouring temperature is 680-700°C.

[0027] If the pouring temperature is too low, for example, below 680°C, the fluidity of the magnesium alloy liquid is poor, which may easily cause problems such as insufficient pouring, cold shut, large transition fillet, slag inclusion, sand inclusion, and excessive precipitation pores; if the pouring temperature is too high, for example, above 700°C, it may easily cause problems such as sand sticking, shrinkage, shrinkage, thermal cracking, fire escape, local oxidation, unqualified size, and excessive reactive pores. In the technical solution of the embodiment of the present application, the pouring temperature is controlled at 680-700°C, which is conducive to the pouring operation and can alleviate the problems caused by the above-mentioned pouring temperature being too high or too low.

[0028] In some embodiments, the die-casting is performed by a die-casting machine, which includes an injection barrel. The poured magnesium alloy liquid is delivered into the injection barrel, and the residence time in the injection barrel is 3-5 seconds.

[0029] In the technical solution of the embodiment of the present application, by controlling the magnesium alloy liquid to stay in the injection barrel for 3-5 seconds, the contact time between the alloy liquid and the atmosphere is reduced, the alloy liquid is prevented from being oxidized, and the alloy has better surface quality.

[0030] In some embodiments, the die-casting process parameters include: injection pressure of 120-135 MPa, boost pressure of 100-120 MPa, cooling time of 3-5 s, injection speed of 9-14 m / s, and demolding time of 5-8 s.

[0031] In the technical solution of the embodiment of the present application, during the die-casting process, the molding quality of the magnesium alloy is better by controlling the injection pressure to 120-135Mpa, the boost pressure to 100-120Mpa, the cooling time to 3-5s, the injection speed to 9-14m / s, and the demolding time to 5-8s.

[0032] In a third aspect, the present application provides a battery, comprising the magnesium alloy as described above or a magnesium alloy prepared by the method for preparing the magnesium alloy as described above.

[0033] In the technical solution of the embodiment of the present application, since magnesium alloy has good corrosion resistance, it can be applied to batteries to increase the reliability of the batteries.

[0034] In some embodiments, a battery includes a battery module, the battery module includes an end plate, the end plate is located at an end of the battery module, and a magnesium alloy is used for the end plate.

[0035] In the technical solution of the embodiment of the present application, since magnesium alloy has good corrosion resistance, it is applied to the end plate of the battery to increase the reliability of the battery.

[0036] In a fourth aspect, the present application provides an electrical device, comprising the battery as described above.

[0037] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific embodiments of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present application. Moreover, the same reference numerals are used throughout the drawings to represent the same components. In the drawings:

[0039] Figure 1 A schematic diagram of the structure of an electric device in some embodiments of the present application;

[0040] Figure 2 A schematic diagram of the exploded structure of a battery according to some embodiments of the present application;

[0041] Figure 3 This is a schematic diagram of the exploded structure of a battery module according to some embodiments of the present application;

[0042] Figure 4 A schematic diagram of the exploded structure of a battery cell according to some embodiments of the present application;

[0043] Figure 5 This is a flow chart of a method for preparing magnesium alloys according to some embodiments of the present application. DETAILED DESCRIPTION

[0044] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.

[0045] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0046] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0047] The “mass percentage” mentioned herein refers to the percentage of the mass of the element to the total mass of the magnesium alloy.

[0048] Existing magnesium alloys have the problem of insufficient corrosion resistance, which limits the further development and application of magnesium alloys.

[0049] In order to solve the problems of insufficient corrosion resistance of existing magnesium alloys, the present invention designs a magnesium alloy, including: 5%-10.5% by mass of aluminum (Al), 0.5%-1.2% by mass of zinc (Zn), 0.1%-0.5% by mass of manganese (Mn), and rare earth (RE) elements, wherein the rare earth elements include at least one of neodymium (Nd), lanthanum (La), and cerium (Ce), wherein the mass percentage of Nd is 0.1%-1%, the mass percentage of La is 0.1%-3%, the mass percentage of Ce is 0.1%-3%, and the rest is magnesium (Mg) and impurities.

[0050] In the technical solution of the embodiment of the present application, Al is the main alloying element in the magnesium alloy. The Al element with a mass percentage of 5%-10.5% can increase the fluidity of the magnesium alloy, so that the magnesium alloy can be die-cast; by controlling the mass percentage of Zn to 0.5%-1.2%, the mechanical properties of the magnesium alloy can be improved without affecting the corrosion resistance of the magnesium alloy; by using 0.1%-0.5% by mass of Mn as a trace additive element, it can partially play a role in refining the grains and improving the yield strength of the magnesium alloy; by controlling the mass percentage of Nd to 0.1%-1%, the mass percentage of La to 0.1%-3%, and the mass percentage of Ce to 0.1%-3%, the magnesium alloy has good corrosion resistance while maintaining the mechanical properties of the magnesium alloy basically stable or improved.

[0051] Adding at least one of Nd, La, and Ce as a rare earth element to the magnesium alloy can effectively improve the morphology of the primary phase, transform the network Mg-Al alloy Mg17Al12 phase into a dispersed skeletal or granular state, and form a new rare earth phase to prevent the primary phase from growing, thereby refining the magnesium alloy structure and improving the mechanical properties of the magnesium alloy; after adding at least one of Nd, La, and Ce, in the process of preparing the magnesium alloy, the melt can be purified to play a role in degassing and deslagging, thereby improving the quality of the melt. During the smelting process, the rare earth elements Nd, La, and Ce easily react with elements such as N, H, and O to form rare earth compounds, reduce the gas content in the melt, and thereby improve the corrosion resistance of the magnesium alloy; at the same time, at least one of Nd, La, and Ce can react with the main impurity elements in the magnesium alloy such as Fe, Cu, Ni, and Si to generate high-melting-point binary or multi-component rare earth compounds, reduce the content of impurity elements in the matrix, and further improve the corrosion resistance of the magnesium alloy.

[0052] Moreover, by controlling the mass percentage of Nd to 0.1%-1%, the mass percentage of La to 0.1%-3%, and the mass percentage of Ce to 0.1%-3%, the corrosion resistance of the magnesium alloy can be significantly improved without significantly increasing the cost.

[0053] The magnesium alloy disclosed in the embodiments of the present application can be used in, but not limited to, the automotive field, the electronics industry field, the aerospace field, etc. For example, housing materials and bracket materials in automobiles, computers, mobile phones, cameras, airplanes, etc. Any product using magnesium alloy can use the magnesium alloy provided in the embodiments of the present application.

[0054] For the convenience of description, the following embodiments are described by taking an electric device 1000 of an embodiment of the present application as a vehicle as an example.

[0055] Please refer to Figure 1 , Figure 1 A schematic diagram of the structure of an electric device 1000 provided for some embodiments of the present application. The electric device 1000 may be a fuel vehicle, a gas vehicle or a new energy vehicle. The new energy vehicle may be a pure electric vehicle, a hybrid vehicle or an extended-range vehicle, etc. A battery 100 is arranged inside the electric device 1000, and the battery 100 may be arranged at the bottom, head or tail of the electric device 1000. The battery 100 may be used to power the electric device 1000. For example, the battery 100 may be used as an operating power source for the electric device 1000. The electric device 1000 may also include a controller 200 and a motor 300. The controller 200 is used to control the battery 100 to power the motor 300, for example, for starting, navigating and driving the electric device 1000.

[0056] In some embodiments of the present application, the battery 100 can not only serve as an operating power source for the electrical device 1000, but also serve as a driving power source for the electrical device 1000, replacing or partially replacing fuel or natural gas to provide driving power for the electrical device 1000.

[0057] Please refer to Figure 2 , Figure 2 Schematic diagram of the exploded structure of the battery 100 provided for some embodiments of the present application. The battery 100 includes a box 10 and a battery module 20, and the battery module 20 is accommodated in the box 10. Among them, the box 10 is used to provide a storage space for the battery module 20, and the box 10 can adopt a variety of structures. In some embodiments, the box 10 may include a first part 11 and a second part 12, the first part 11 and the second part 12 cover each other, and the first part 11 and the second part 12 jointly define a storage space for accommodating the battery module 20. The second part 12 can be a hollow structure with one end open, the first part 11 can be a plate-like structure, and the first part 11 covers the open side of the second part 12, so that the first part 11 and the second part 12 jointly define a storage space; the first part 11 and the second part 12 can also be hollow structures with one side open, and the open side of the first part 11 covers the open side of the second part 12. Of course, the box 10 formed by the first part 11 and the second part 12 can be in a variety of shapes, such as a cylinder, a cuboid, etc.

[0058] In the battery 100, there may be multiple battery modules 20, and the multiple battery modules 20 may be connected in series, in parallel, or in mixed connection. Mixed connection means that the multiple battery modules 20 are both connected in series and in parallel. The multiple battery modules 20 may be directly connected in series, in parallel, or in mixed connection, and then the whole formed by the multiple battery modules 20 is accommodated in the box 10; of course, the battery 100 may also be a battery module formed by connecting multiple battery modules 20 in series, in parallel, or in mixed connection, and then the multiple battery modules are connected in series, in parallel, or in mixed connection to form a whole, and then accommodated in the box 10. The battery 100 may also include other structures, for example, the battery 100 may also include a converging component for realizing electrical connection between the multiple battery modules 20.

[0059] In the battery 100 , there may be one or more battery modules 20 , and each battery module 20 may be fixed to the housing 10 by a corresponding fastener (such as a bolt), or each battery module 20 may be fixed to the housing 10 by bonding.

[0060] Figure 3A schematic diagram of the exploded structure of a battery module 20 provided for some embodiments of the present application. The battery module 20 includes a plurality of stacked battery cells 20a, an end plate 30, and a connector (not shown in the figure). Two end plates 30 are arranged at both ends of the battery module 20 along the stacking direction of the battery cells 20a, and the two end plates 30 are connected by a connector. The end plates 30 and the connector provide a clamping force to the battery cells 20a, and the battery cells 20a are fastened to form a battery module 20 with a certain structural strength. The multiple battery cells 20a in the battery module 20 can be electrically connected through a busbar component (not shown in the figure) to achieve parallel, series or mixed connection of the multiple battery cells 20a in the battery module 20. There may be one or more busbar components, and each busbar component is used to electrically connect at least two battery cells 20a.

[0061] Each battery cell 20a may be a secondary battery, a lithium-sulfur battery, a lithium-ion battery or a lithium metal battery, but is not limited thereto. The battery cell 20a may be cylindrical, flat, rectangular or in other shapes.

[0062] Please refer to Figure 4 , Figure 4 The schematic diagram of the decomposed structure of a battery cell 20a provided in some embodiments of the present application. The battery cell 20a refers to the smallest unit that constitutes a battery. Figure 4 The battery cell 20a includes an end cover 21, a shell 22, a battery cell assembly 23 and other functional components.

[0063] The end cap 21 refers to a component that covers the opening of the shell 22 to isolate the internal environment of the battery cell 20a from the external environment. Without limitation, the shape of the end cap 21 can be adapted to the shape of the shell 22 to match the shell 22. The end cap 21 can be made of a material with a certain hardness and strength (such as aluminum alloy), so that the end cap 21 is not easily deformed when squeezed and collided, so that the battery cell 20a can have a higher structural strength and the safety performance can also be improved. Functional components such as electrode terminals 21a can be provided on the end cap 21. The electrode terminal 21a can be used to electrically connect to the battery cell assembly 23 for outputting or inputting electrical energy of the battery cell 20a. In some embodiments, the end cap 21 can also be provided with a pressure relief mechanism for releasing the internal pressure when the internal pressure or temperature of the battery cell 20a reaches a threshold. The material of the end cap 21 can also be a variety of materials, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and the embodiments of the present application do not impose special restrictions on this. In some embodiments, an insulating member may be provided inside the end cap 21, and the insulating member may be used to isolate the electrical connection components in the housing 22 from the end cap 21 to reduce the risk of short circuit. For example, the insulating member may be plastic, rubber, or the like.

[0064] The shell 22 is a component used to cooperate with the end cover 21 to form the internal environment of the battery cell 20a, wherein the formed internal environment can be used to accommodate the battery cell assembly 23, electrolyte and other components. The shell 22 and the end cover 21 can be independent components, and an opening can be set on the shell 22, and the internal environment of the battery cell 20a is formed by covering the opening with the end cover 21 at the opening. Without limitation, the end cover 21 and the shell 22 can also be integrated. Specifically, the end cover 21 and the shell 22 can form a common connection surface before other components are put into the shell, and when the interior of the shell 22 needs to be encapsulated, the end cover 21 covers the shell 22. The shell 22 can be of various shapes and sizes, such as a rectangular parallelepiped, a cylindrical shape, a hexagonal prism, etc. Specifically, the shape of the shell 22 can be determined according to the specific shape and size of the battery cell assembly 23. The material of the shell 22 can be various, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and the embodiment of the present application does not impose any special restrictions on this.

[0065] The battery cell assembly 23 is a component in the battery cell 100 where electrochemical reactions occur. One or more battery cell assemblies 23 may be included in the housing 22. The battery cell assembly 23 is mainly formed by winding or stacking cathode sheets and anode sheets, and a separator is usually provided between the cathode sheets and the anode sheets. The parts of the cathode sheets and the anode sheets with active substances constitute the main body of the battery cell assembly, and the parts of the cathode sheets and the anode sheets without active substances each constitute a tab 23a. The cathode tab and the anode tab may be located together at one end of the main body or respectively at both ends of the main body. During the charge and discharge process of the battery, the cathode active substance and the anode active substance react with the electrolyte, and the tab 23a connects the electrode terminals to form a current loop.

[0066] According to some embodiments of the present application, the present application provides a magnesium alloy, including: aluminum (Al), the mass percentage of Al is 5%-10.5%; zinc (Zn), the mass percentage of Zn is 0.5%-1.2%; manganese (Mn), the mass percentage of Mn is 0.1%-0.5%; rare earth (RE) elements, the rare earth elements include at least one of neodymium (Nd), lanthanum (La), and cerium (Ce), wherein the mass percentage of Nd is 0.1%-1%, the mass percentage of La is 0.1%-3%, and the mass percentage of Ce is 0.1%-3%; the rest is magnesium (Mg) and impurities.

[0067] In the technical solution of the embodiment of the present application, Al is the main alloying element in the magnesium alloy. The Al element with a mass percentage of 5%-10.5% can increase the fluidity of the magnesium alloy, so that the magnesium alloy can be die-cast; by controlling the mass percentage of Zn to 0.5%-1.2%, the mechanical properties of the magnesium alloy can be improved without affecting the corrosion resistance of the magnesium alloy; by using 0.1%-0.5% by mass of Mn as a trace additive element, it can partially play a role in refining the grains and improving the yield strength of the magnesium alloy; by controlling the mass percentage of Nd to 0.1%-1%, the mass percentage of La to 0.1%-3%, and the mass percentage of Ce to 0.1%-3%, the magnesium alloy has good corrosion resistance while maintaining the mechanical properties of the magnesium alloy basically stable or improved.

[0068] As an example, the mass percentage of Al can be 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, etc. The mass percentage of Al can also be 5%-5.5%, 5.5%-6%, 6%-6.5%, 6.5%-7%, 7%-7.5%, 7.5%-8%, 8%-8.5%, 8.5%-9%, 9%-9.5%, 9.5%-10%, 10%-10.5%, etc. It can be understood that the mass percentage of Al is not limited to the mass percentages listed above, and can be selected according to actual needs, as long as the mass percentage of Al is 5%-10.5%.

[0069] Al is the main alloying element in magnesium alloy. If the mass percentage of Al is too low, for example, less than 5%, the fluidity of magnesium alloy is poor, which is not conducive to die casting; if the mass percentage of Al is too high, for example, higher than 10.5%, it will cause the weight of magnesium alloy to increase greatly, affecting the performance of magnesium alloy. Al element with a mass percentage of 5%-10.5% can increase the fluidity of magnesium alloy, enable magnesium alloy to be die cast, and alleviate the weight increase of magnesium alloy.

[0070] As an example, the mass percentage of Zn can be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, etc. The mass percentage of Zn can also be 0.5%-0.6%, 0.6%-0.7%, 0.7%-0.8%, 0.8%-0.9%, 0.9%-1.0%, 1.0%-1.1%, 1.1%-1.2%, etc. It can be understood that the mass percentage of Zn is not limited to the mass percentages listed above, and can be selected according to actual needs, as long as the mass percentage of Zn is guaranteed to be 0.5%-1.2%.

[0071] If the mass percentage of Zn is too high, for example, the mass percentage is greater than 1.2%, the corrosion resistance of the magnesium alloy will be affected; if the mass percentage of Zn is too low, for example, the mass percentage is less than 0.5%, the mechanical properties of the magnesium alloy will not be significantly improved. By controlling the mass percentage of Zn to 0.5%-1.2%, the mechanical properties of the magnesium alloy can be improved without affecting the corrosion resistance of the magnesium alloy.

[0072] As an example, the mass percentage of Mn can be 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, etc. The mass percentage of Mn can also be 0.1%-0.15%, 0.15%-0.2%, 0.2%-0.25%, 0.25%-0.3%, 0.3%-0.35%, 0.35%-0.4%, 0.4%-0.45%, 0.45%-0.5%, etc. It can be understood that the mass percentage of Mn is not limited to the mass percentages listed above, and can be selected according to actual needs, as long as the mass percentage of Mn is guaranteed to be 0.1%-0.5%.

[0073] 0.1%-0.5% by mass of Mn as a trace element can partially refine the grains and improve the yield strength of the magnesium alloy.

[0074] In some embodiments, the rare earth element includes one of Nd, La, and Ce. In some embodiments, the rare earth element includes two of Nd, La, and Ce. In some embodiments, the rare earth element includes Nd, La, and Ce at the same time.

[0075] As an example, the mass percentage of Nd can be 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, 1%, etc. The mass percentage of Nd can also be 0.1%-0.15%, 0.15%-0.2%, 0.2%-0.25%, 0.25%-0.3%, 0.3%-0.35%, 0.35%-0.4%, 0.4%-0.45%, 0.45%-0.5%, 0.5%-0.55%, 0.55%-0.6%, 0.6%-0.65%, 0.65%-0.7%, 0.7%-0.75%, 0.75%-0.8%, 0.8%-0.85%, 0.85%-0.9%, 0.9%-0.95%, 0.95%-1%, etc.

[0076] As an example, the mass percentage of La may be 0.1%, 0.5%, 1%, 1.25%, 1.5%, 2.0%, 2.5%, 3%, etc. The mass percentage of La may also be 0.1%-0.5%, 0.5%-1%, 1%-1.25%, 1.25%-1.5%, 1.5%-2.0%, 2.0%-2.5%, 2.5%-3%, etc.

[0077] As an example, the mass percentage of Ce may be 0.1%, 0.5%, 1%, 1.25%, 1.5%, 2.0%, 2.5%, 3%, etc. The mass percentage of Ce may also be 0.1%-0.5%, 0.5%-1%, 1%-1.25%, 1.25%-1.5%, 1.5%-2.0%, 2.0%-2.5%, 2.5%-3%, etc.

[0078] It is understandable that the mass percentages of Nd, La and Ce are not limited to the mass percentages listed above and can be selected according to actual needs, as long as the mass percentage of Nd is 0.1%-1%, the mass percentage of La is 0.1%-3%, and the mass percentage of Ce is 0.1%-3%.

[0079] When the mass percentage of a single rare earth element Nd, La, or Ce is less than 0.1%, the effect of the rare earth element Nd, La, or Ce is significantly weakened, and the effect of improving the corrosion resistance of the magnesium alloy is not obvious; when the mass percentage of a single rare earth element Nd, La, or Ce is too high, for example, the mass percentage of Nd is greater than 1%, the mass percentage of La is greater than 3%, and the mass percentage of Ce is greater than 3%, the cost of the magnesium alloy increases significantly, which is not conducive to industrial application. By controlling the mass percentage of Nd to 0.1%-1%, the mass percentage of La to 0.1%-3%, and the mass percentage of Ce to 0.1%-3%, the corrosion resistance of the magnesium alloy is significantly improved without significantly increasing the cost.

[0080] Adding at least one rare earth element among Nd, La and Ce to magnesium alloy can effectively improve the morphology of primary phase and make the network Mg-Al alloy Mg 17 A l12The phase changes into a dispersed skeleton or granular shape, and a new rare earth phase is formed to prevent the primary phase from growing, thereby refining the magnesium alloy structure and improving the mechanical properties of the magnesium alloy; after at least one element of Nd, La, and Ce is added, the melt can be purified in the process of preparing the magnesium alloy to play the role of degassing and slag removal, improving the quality of the melt, and in the smelting process, the rare earth elements of Nd, La, and Ce easily react with elements such as N, H, and O to form rare earth compounds, reduce the gas content in the melt, and thus improve the corrosion resistance of the magnesium alloy; at the same time, at least one element of Nd, La, and Ce can react with the main impurity elements in magnesium alloys such as Fe, Cu, Ni, and Si to generate binary or multi-component rare earth compounds with high melting points, reduce the content of impurity elements in the matrix, and further improve the corrosion resistance of the magnesium alloy. Therefore, compared with the existing magnesium alloys, the magnesium alloy provided by the embodiment of the present application has better corrosion resistance.

[0081] Impurities are impurities that are unavoidable during the preparation process of magnesium alloys.

[0082] According to some optional embodiments of the present application, the mass percentage of Nd is 0.4%-0.6%, the mass percentage of La is 1.0%-1.5%, and the mass percentage of Ce is 1.0%-1.5%.

[0083] By controlling the mass percentage of Nd to 0.4%-0.6%, the mass percentage of La to 1.0%-1.5%, and the mass percentage of Ce to 1.0%-1.5%, the corrosion resistance of the magnesium alloy is further improved without significantly increasing the cost.

[0084] According to some embodiments of the present application, the mass percentage of impurities is less than or equal to 0.05%.

[0085] As an example, the mass percentage of impurities may be less than or equal to 0.05%, 0.04%, 0.035%, 0.03%, 0.02%, 0.01%, 0.001%, 0.0001%, etc.

[0086] In the technical solution of the embodiment of the present application, the content of impurity elements in the magnesium alloy is relatively low, which can reduce the impact of impurities on the performance of the magnesium alloy.

[0087] According to some embodiments of the present application, the impurities include at least one of Fe, Cu, Ni, and Si, wherein the mass percentage of Fe in the magnesium alloy is less than 0.004%, the mass percentage of Cu in the magnesium alloy is less than 0.02%, the mass percentage of Ni in the magnesium alloy is less than 0.001%, and the mass percentage of Si in the magnesium alloy is less than 0.05%.

[0088] As an example, the mass percentage of Fe in the magnesium alloy may be less than or equal to 0.004%, 0.0035%, 0.003%, 0.002%, 0.001%, 0.0001%, etc.

[0089] As an example, the mass percentage of Cu in the magnesium alloy may be less than or equal to 0.02%, 0.015%, 0.012%, 0.01%, 0.005%, 0.001%, 0.0001%, etc.

[0090] As an example, the mass percentage of Ni in the magnesium alloy may be less than or equal to 0.001%, 0.0008%, 0.0007%, 0.0005%, 0.0002%, 0.0001%, 0.00001%, etc.

[0091] As an example, the mass percentage of Si in the magnesium alloy may be less than or equal to 0.05%, 0.04%, 0.03%, 0.02%, 0.015%, 0.01%, 0.001%, 0.0001%, etc.

[0092] In the technical solution of the embodiment of the present application, the content of impurity elements in the magnesium alloy is relatively low, which can reduce the impact of impurities on the performance of the magnesium alloy.

[0093] See also Figure 5 According to some embodiments of the present application, the present application also provides a method for preparing the magnesium alloy in any of the above embodiments, comprising:

[0094] Providing pure Mg, pure Al, pure Zn, Mg-Mn master alloy, and Mg-RE master alloy according to the mass percentages of Mg, Al, Zn, Mn, and rare earth elements in the above magnesium alloy;

[0095] Mixing pure Mg, pure Al, pure Zn, Mg-RE master alloy and Mg-Mn master alloy and smelting to obtain magnesium alloy liquid, and the smelting is carried out in a protective gas;

[0096] The magnesium alloy liquid is poured and die-casted in sequence to obtain the magnesium alloy.

[0097] The preparation method of the magnesium alloy provided in the embodiment of the present application can effectively improve the morphology of the primary phase by adding Mg-RE master alloy during the preparation process, wherein the RE element includes at least one of Nd, La, and Ce, so as to make the network Mg-Al alloy Mg 17 A l12The phase changes into a dispersed skeleton or granular shape, and a new rare earth phase is formed to prevent the primary phase from growing, thereby refining the magnesium alloy structure and improving the mechanical properties of the magnesium alloy; after at least one bathing element among Nd, La, and Ce is added, the melt can be purified in the process of preparing the magnesium alloy to play the role of degassing and deslagging, improving the quality of the melt, and in the smelting process, the rare earth elements Nd, La, and Ce easily react with elements such as N, H, and O to form rare earth compounds, reduce the gas content in the melt, and thus improve the corrosion resistance of the magnesium alloy; at the same time, at least one element among Nd, La, and Ce can react with the main impurity elements in magnesium alloys such as Fe, Cu, Ni, and Si to generate binary or multi-component rare earth compounds with high melting points, reduce the content of impurity elements in the matrix, and further improve the corrosion resistance of the magnesium alloy. Therefore, the magnesium alloy obtained by the preparation method of the embodiment of the present application has good corrosion resistance.

[0098] According to some embodiments of the present application, mixing pure Mg, pure Al, pure Zn, Mg-RE intermediate alloy and Mg-Mn intermediate alloy and smelting to obtain a magnesium alloy liquid further includes: introducing a protective gas into a smelting furnace, adding pure Mg into the smelting furnace for melting, adding pure Al and pure Zn after the pure Mg is completely melted, maintaining the temperature of the smelting furnace while stirring; heating, when the temperature of the smelting furnace reaches 700-720°C, adding the Mg-RE intermediate alloy and stirring; continuing to heat, when the temperature of the smelting furnace reaches 720-740°C, adding the Mg-Mn intermediate alloy and stirring to obtain a magnesium alloy liquid.

[0099] The type of the smelting furnace can be selected according to actual needs. In some optional embodiments, the smelting furnace is a protective gas smelting furnace, and a protective gas can be introduced into the smelting furnace.

[0100] The melting point of pure Mg is 649° C. In some optional embodiments, pure Mg is added into a smelting furnace and the temperature is raised to 650-680° C. to completely melt the pure Mg.

[0101] In some optional embodiments, the stirring methods include but are not limited to natural convection stirring, manual stirring, steel flow impact stirring, mechanical stirring, electromagnetic stirring and gas stirring, etc., which can be selected according to actual needs.

[0102] As an example, the addition temperature of the Mg-RE master alloy may be but not limited to 700°C, 705°C, 710°C, 715°C, 720°C, etc.; it may also be but not limited to 700-705°C, 705-710°C, 710-715°C, 715-720°C, etc.

[0103] The addition temperature of the Mg-Mn master alloy may be, but not limited to, 720°C, 725°C, 730°C, 735°C, 740°C, etc.; it may also be, but not limited to, 720-725°C, 725-730°C, 730-735°C, 735-740°C, etc.

[0104] If the adding temperature of Mg-RE master alloy and Mg-Mn master alloy is too high, for example, the adding temperature of Mg-RE master alloy is higher than 720℃, and the adding temperature of Mg-Mn master alloy is higher than 740℃, the burning loss of alloy elements will increase and the recovery rate of alloy elements will decrease; if the adding temperature of Mg-RE master alloy and Mg-Mn master alloy is too low, for example, the adding temperature of Mg-RE master alloy is lower than 700℃, and the adding temperature of Mg-Mn master alloy is lower than 720℃, the dissolution rate of alloy elements will slow down or even fail to dissolve completely. By controlling the addition of Mg-RE master alloy at 700-720℃ and the addition of Mg-Mn master alloy at 720-740℃, the burning loss of alloy elements is small, the recovery rate is high, and the dissolution rate of alloy elements is fast.

[0105] According to some embodiments of the present application, the molten metal in the smelting furnace is fully mixed and uniformly by maintaining the temperature of the smelting furnace at 720-740° C. and standing for 10-15 minutes.

[0106] As an example, the standing time may be, but is not limited to, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, etc.; it may also be, but is not limited to, 10-11 min, 11-12 min, 12-13 min, 13-14 min, 14-15 min, etc.

[0107] According to some embodiments of the present application, the magnesium alloy liquid is poured into a quantitative pouring device, and the magnesium alloy liquid in the quantitative pouring device is delivered to a die-casting machine for die-casting to obtain a magnesium alloy.

[0108] The type of quantitative pouring equipment can be selected according to actual needs. In some optional embodiments, the quantitative pouring equipment is a quantitative pouring furnace. In some optional embodiments, pouring the magnesium alloy liquid into the quantitative pouring equipment and delivering the magnesium alloy liquid in the quantitative pouring equipment to the die-casting machine for die-casting are all fully automatic and continuous operations. In some optional embodiments, the die-casting machine is directly equipped with the quantitative pouring equipment.

[0109] According to some embodiments of the present application, the pouring temperature is 680-700°C.

[0110] As an example, the temperature of pouring the magnesium alloy liquid into the quantitative pouring equipment can be but not limited to 680°C, 685°C, 690°C, 695°C, 700°C, etc., and can also be but not limited to 680-685°C, 685-690°C, 690-695°C, 695-700°C, etc.

[0111] If the pouring temperature is too low, for example, below 680℃, the fluidity of magnesium alloy liquid is poor, which may cause problems such as insufficient pouring, cold shut, large transition fillet, slag inclusion, sand inclusion, and excessive precipitation pores. If the pouring temperature is too high, for example, above 700℃, it may cause problems such as sand sticking, shrinkage, shrinkage, thermal cracking, fire escape, local oxidation, unqualified size, and excessive reactive pores. In the preparation process of magnesium alloy, controlling the pouring temperature to 680-700℃ is conducive to the pouring operation and can alleviate the problems caused by excessively high and low pouring temperatures.

[0112] According to some optional embodiments of the present application, the die-casting is performed by a die-casting machine, which includes an injection barrel. The poured magnesium alloy liquid is delivered into the injection barrel and stays in the injection barrel for 3-5 seconds.

[0113] Optionally, the poured magnesium alloy liquid is delivered to the injection barrel in a fully automatic and continuous operation to prevent oxidation of the magnesium alloy.

[0114] As an example, the residence time of the magnesium alloy liquid in the injection barrel can be 3s, 3.1s, 3.5s, 4s, 4.5s, 4.9s, 5s, etc., or it can be 3-3.1s, 3.1-3.5s, 3.5-4s, 4-4.5s, 4.5-4.9s, 4.9-5s, etc.

[0115] By controlling the magnesium alloy liquid to stay in the injection barrel for 3-5 seconds, the contact time between the alloy liquid and the atmosphere is reduced, the alloy liquid is prevented from being oxidized, and the alloy has better surface quality.

[0116] According to some embodiments of the present application, the shielding gas may include, but is not limited to, a mixed gas of sulfur hexafluoride (SF6) and nitrogen (N2), a mixed gas of argon and SF6, a mixed gas of SF6 and carbon dioxide (CO2), etc. The volume ratio of SF6 to N2 in the mixed gas of SF6 and N2, the volume ratio of SF6 in the mixed gas of argon and SF6, and the volume ratio of SF6 to CO2 in the mixed gas of SF6 and CO2 can be selected according to actual needs.

[0117] According to some optional embodiments of the present application, the protective gas is a mixed gas of sulfur hexafluoride (SF6) and nitrogen (N2).

[0118] During the smelting process, by introducing protective gas, the contact time between the magnesium alloy liquid and the atmosphere can be reduced, thereby preventing the magnesium alloy liquid from being oxidized.

[0119] The die casting of magnesium alloy can be carried out by using a hot chamber die casting machine or a cold chamber die casting machine as required. According to some optional embodiments of the present application, the die casting adopts a cold chamber die casting machine. The die casting adopts a cold chamber die casting machine, which has the advantages of high precision, high efficiency, strong selectivity, and can be directly equipped with quantitative pouring equipment.

[0120] According to some optional embodiments of the present application, the die-casting process parameters include but are not limited to: injection pressure of 120-135Mpa, boost pressure of 100-120Mpa, cooling time of 3-5s, injection speed of 9-14m / s, and demolding time of 5-8s.

[0121] As an example, the injection pressure may be but is not limited to 120 MPa, 125 MPa, 128 MPa, 130 MPa, 131 MPa, 132 MPa, 133 MPa, 134 MPa, 135 MPa, etc.; it may also be but is not limited to 120-134 MPa, 125-131 MPa, 128-132 MPa, 133-135 MPa, etc.

[0122] As an example, the boost pressure may be, but not limited to, 100 MPa, 105 MPa, 110 MPa, 115 MPa, 118 MPa, 120 MPa, etc.; it may also be, but not limited to, 100-118 MPa, 105-115 MPa, 110-120 MPa, etc.

[0123] As an example, the cooling time may be, but not limited to, 3s, 3.5s, 4s, 4.5s, 5s, etc.; it may also be, but not limited to, 3-4s, 3.5-4.5s, 4-5s, etc.

[0124] As an example, the injection speed can be but not limited to 9m / s, 8.5m / s, 10m / s, 11m / s, 12m / s, 12.5m / s, 12.8m / s, 13m / s, 14m / s, etc., and can also be but not limited to 9-12m / s, 10m / s-12.5m / s, 8.5-12.8m / s, 13-14m / s, etc.

[0125] As an example, the demoulding time may be, but not limited to, 3s, 4.5s, 5s, 6.5s, 7s, 7.5s, 8s, etc.; it may also be, but not limited to, 3-5s, 6.5-7s, 4.5-8s, etc.

[0126] During the die-casting process, the molding quality of the magnesium alloy is better by controlling the injection pressure to 120-135Mpa, the boost pressure to 100-120Mpa, the cooling time to 3-5s, the injection speed to 9-14m / s, and the demolding time to 5-8s.

[0127] It can be understood that all elements, devices, apparatus, equipment, etc. of the magnesium alloy including any of the above embodiments, or the magnesium alloy prepared by the preparation method of any of the above embodiments, should be included in the scope of the claims and description of the present application.

[0128] According to some embodiments of the present application, the present application also provides a battery, the battery comprising the magnesium alloy as described above or a magnesium alloy prepared by the method for preparing the magnesium alloy as described above.

[0129] In the technical solution of the embodiment of the present application, since magnesium alloy has good corrosion resistance, it can be applied to batteries to increase the reliability of the batteries.

[0130] In some embodiments, a battery includes a battery module, the battery module includes an end plate, the end plate is located at an end of the battery module, and a magnesium alloy is used for the end plate.

[0131] The magnesium alloy provided in the present application can be used for the end plate 30 of the battery 100. The end plate 30 is located at the end of the battery module 20. The end plate 30 can be fixedly connected to the battery module 20. The end plate 30 can be used to fix and squeeze the battery cells 20a after grouping. The end plate 30 can be a plate-shaped structural member located at the end of the battery module 20, or a bracket structural member constituting the frame of the battery module 20.

[0132] In the technical solution of the embodiment of the present application, since magnesium alloy has good corrosion resistance, it is applied to the end plate of the battery to increase the reliability of the battery.

[0133] According to some embodiments of the present application, the present application further provides an electrical device, comprising a battery provided by any of the embodiments described above, and the battery is used to provide electrical energy to the electrical device.

[0134] The electrical device may be, but is not limited to, any of the aforementioned devices or systems using batteries.

[0135] The following is an introduction to magnesium alloys, their preparation process and test data:

[0136] Embodiment 1:

[0137] The composition of the magnesium alloy provided in Example 1 is: the mass percentage of Al is 8.5%; the mass percentage of Zn is 0.8%; the mass percentage of Mn is 0.2%; the mass percentage of Nd is 0.2%, the mass percentage of La is 1%, and the mass percentage of Ce is 1.5%; the impurities Fe<0.004%, Cu<0.02%, Ni<0.001%, Si<0.05%; and the rest is magnesium.

[0138] The preparation method of the magnesium alloy in this embodiment includes:

[0139] According to the mass percentages of Mg, Al, Zn, Mn, Nd, La and Ce in the above magnesium alloy, weigh the corresponding pure Mg, pure Al, pure Zn, Mg-20Mn and Mg-30RE (RE includes Nd, La and Ce) master alloys;

[0140] Introduce SF6+N2 mixed gas into the smelting furnace, add pure Mg into the smelting furnace, heat it to 650-680°C for melting, add pure Al and pure Zn after the pure Mg is completely melted, maintain the temperature of the smelting furnace and stir at the same time; heat up, when the temperature of the smelting furnace reaches 700-720°C, add Mg-30RE master alloy and stir; continue to heat up, when the temperature of the smelting furnace reaches 720-740°C, add Mg-20Mn master alloy and stir; maintain the temperature of the smelting furnace at 720-740°C and stand for 10-15 minutes to obtain magnesium alloy liquid;

[0141] A cold chamber die casting machine is used for die casting. The cold chamber die casting machine is directly equipped with a quantitative furnace. The magnesium alloy liquid is poured into the quantitative furnace. The pouring temperature is controlled between 680-700°C. The magnesium alloy liquid in the quantitative furnace is delivered to the injection barrel and stays in the injection barrel for 3-5s. Then it is injected into the die casting mold for die casting. Among them, the pouring of the quantitative furnace and the injection of the die casting machine are fully automatic and continuous operations. The die casting mold uses H13 mold steel. The die casting process parameters are injection pressure: 120-135Mpa, boost pressure set to 100-120Mpa, cooling time: 3-5s, injection speed: 9-14m / s, demoulding time: 5-8s.

[0142] Examples 2-12 and Comparative Examples 1-6:

[0143] Examples 2-12 and Comparative Examples 1-6 are substantially the same as Example 1, the only difference being that the mass percentages of the elements in the composition of the magnesium alloy are different.

[0144] The mechanical properties and corrosion resistance of the magnesium alloys of Examples 1-12 and Comparative Examples 1-6 were tested respectively:

[0145] The mechanical properties of magnesium alloys are tested by tensile test. The tensile test is carried out on a universal tensile testing machine. The tensile standard is implemented in accordance with GB / T 228.1.

[0146] The corrosion resistance of magnesium alloy is tested under neutral salt spray, and the salt spray corrosion test method is carried out in accordance with GB / T 10125 neutral salt spray test.

[0147]

[0148]

[0149] From the comparison of the results of Examples 1-12 and Comparative Examples 1-6 in Table 1, it can be seen that the embodiments of the present application, by adding at least one rare earth element among the additives Nd, La, and Ce, the magnesium alloy has good corrosion resistance while maintaining the basic stability or improving the mechanical properties of the magnesium alloy.

[0150] By comparing the results of Examples 5-7 with Examples 1-4 and 8-12, it can be seen that the present application controls the mass percentage of Nd to 0.4%-0.6%, the mass percentage of La to 1.0%-1.5%, and the mass percentage of Ce to 1.0%-1.5%, thereby achieving better corrosion resistance for the magnesium alloy while maintaining the mechanical properties of the magnesium alloy basically stable or improved.

[0151] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

Claims

1. A magnesium alloy, characterized in that: include: Aluminum (Al), wherein the mass percentage of Al is 5%-10.5%; Zinc (Zn), wherein the mass percentage of Zn is 0.5%-1.2%; Manganese (Mn), wherein the mass percentage of Mn is 0.1%-0.5%; Rare earth (RE) elements, the rare earth elements comprising at least one of neodymium (Nd), lanthanum (La), and cerium (Ce), wherein the mass percentage of Nd is 0.1%-1%, the mass percentage of La is 0.1%-3%, and the mass percentage of Ce is 0.1%-3%; The rest is magnesium (Mg) and impurities.

2. The magnesium alloy according to claim 1, characterized in that The mass percentage of Nd is 0.4%-0.6%, the mass percentage of La is 1.0%-1.5%, and the mass percentage of Ce is 1.0%-1.5%.

3. The magnesium alloy according to claim 1 or 2, characterized in that: The mass percentage of the impurities is less than or equal to 0.05%.

4. The magnesium alloy according to any one of claims 1 to 3, characterized in that: The impurities include at least one of Fe, Cu, Ni, and Si, wherein the mass percentage of Fe in the magnesium alloy is less than or equal to 0.004%, the mass percentage of Cu in the magnesium alloy is less than or equal to 0.02%, the mass percentage of Ni in the magnesium alloy is less than or equal to 0.001%, and the mass percentage of Si in the magnesium alloy is less than or equal to 0.05%.

5. A method for preparing a magnesium alloy according to any one of claims 1 to 4, characterized in that: include: Providing pure Mg, pure Al, pure Zn, Mg-Mn master alloy, and Mg-RE master alloy according to the mass percentages of Mg, Al, Zn, Mn, and rare earth elements in the magnesium alloy; The pure Mg, the pure Al, the pure Zn, the Mg-RE master alloy and the Mg-Mn master alloy are mixed and smelted to obtain a magnesium alloy liquid, wherein the smelting is performed in a protective gas; The magnesium alloy liquid is poured and die-casted in sequence to obtain the magnesium alloy.

6. The method for preparing a magnesium alloy according to claim 5, characterized in that: Add the pure Mg into a smelting furnace for melting, add the pure Al and the pure Zn after the pure Mg is completely melted, maintain the temperature of the smelting furnace and perform stirring treatment; increase the temperature, and when the temperature of the smelting furnace reaches 700-720° C., add the Mg-RE master alloy and perform stirring; The temperature is continued to be raised, and when the temperature of the smelting furnace reaches 720-740° C., the Mg—Mn master alloy is added and stirred to obtain the magnesium alloy liquid.

7. The method for preparing a magnesium alloy according to claim 6, characterized in that: After the step of adding the Mg-Mn master alloy and stirring, the temperature of the smelting furnace is maintained at 720-740° C. and allowed to stand for 10-15 minutes to obtain the magnesium alloy liquid.

8. The method for preparing a magnesium alloy according to any one of claims 5 to 7, characterized in that: The pouring temperature is 680-700°C.

9. The method for preparing a magnesium alloy according to any one of claims 5 to 8, characterized in that: The die casting is performed by a die casting machine, which includes an injection barrel. The poured magnesium alloy liquid is delivered into the injection barrel and stays in the injection barrel for 3-5 seconds.

10. The method for preparing a magnesium alloy according to claim 9, characterized in that: The die-casting process parameters include: injection pressure of 120-135 MPa, boost pressure of 100-120 MPa, cooling time of 3-5 s, injection speed of 9-14 m / s, and demoulding time of 5-8 s.

11. A battery, characterized in that: The invention comprises a magnesium alloy as described in any one of claims 1 to 4 or a magnesium alloy prepared by the method for preparing a magnesium alloy as described in any one of claims 5 to 10.

12. The battery according to claim 11, characterized in that The battery includes a battery module, the battery module includes an end plate, the end plate is located at an end of the battery module, and the magnesium alloy is used for the end plate.

13. An electrical device, characterized in that: Comprising a battery as claimed in claim 11 or 12.

Citation Information

Patent Citations

  • Cerium lanthanum containing high-strength anti-corrosion die-casting magnesium alloy

    CN101220432A

  • Magnesium alloy and preparation method thereof

    CN101921940A

  • High-strength and high-elongation cast magnesium alloy and production method thereof

    CN102644013A

  • Low-rare-earth high-corrosion-resistance magnesium alloy and preparation method thereof

    CN109825750A

  • Magnesium-beryllium rare-earth die-casting alloy and preparation method thereof

    CN111218594A