Magnesium-based composite shielding material with three-dimensional network structure and preparation method of magnesium-based composite shielding material

By adopting a three-dimensional mesh structure and the continuous distribution of tungsten and boron carbide particles in magnesium-based composite materials, the problems of uneven distribution of shielding components and high production costs in traditional shielding materials are solved, and efficient radiation shielding effect is achieved and Low cost production, suitable for new nuclear reactor applications.

CN119020651AActive Publication Date: 2024-11-26GRIMAT ENG INST CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411041852.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-26
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Random uniform distribution of shielding components in traditional metal-based composite shielding materials leads to a low probability of interaction with shielding components when rays pass through, weakening the shielding effect, and increasing the volume fraction of shielding components is difficult to achieve uniform distribution, resulting in high production costs and shielding performance Limited improvement.

Method used

The magnesium-based composite material with a three-dimensional mesh structure is continuously distributed around the magnesium matrix particles through tungsten and boron carbide particles. Combined with mechanical mixing and thermal isostatic pressing technology, the three-dimensional mesh distribution of shielding components is realized, improving the shielding effect and Density uniformity.

Benefits of technology

It improves the continuity and shielding effect of shielding components in shielding materials, reduces production costs, is suitable for large-scale production, and is suitable for shielding component design in new nuclear reactors, with the characteristics of miniaturization, lightweighting and flexible adjustment of shielding performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020651A_ABST
    Figure CN119020651A_ABST
Patent Text Reader

Abstract

The invention discloses a magnesium-based composite shielding material with a three-dimensional network structure and a preparation method of the magnesium-based composite shielding material, and belongs to the technical field of magnesium-based composite shielding materials. The magnesium-based composite shielding material of the three-dimensional network structure comprises 30 wt%-60 wt% of tungsten, 30 wt%-50 wt% of boron carbide and 10 wt%-40 wt% of a magnesium matrix, the average particle size of the tungsten is smaller than or equal to 10 micrometers, the average particle size of the boron carbide is smaller than or equal to 40 micrometers, the average particle size of the magnesium matrix is smaller than or equal to 80 micrometers, and the ratio of the average particle size of the tungsten or the boron carbide to the average particle size of the magnesium matrix ranges from 1: 16 to 1: 2. The magnesium-based composite shielding material with shielding component particles in three-dimensional network distribution is obtained, and the density of the composite shielding material is 2.9 g / cm < 3 >-5.0 g / cm < 3 >. According to the invention, through particle size matching of powder particles, three-dimensional network distribution of shielding component particles is realized, and the problems of poor dispersity of shielding components and limited improvement of shielding performance caused by purely depending on improvement of volume fractions of the shielding components in a composite shielding material in the prior art are solved; the novel shielding material has the characteristics of miniaturization, light weight, flexible adjustment of shielding performance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of magnesium-based composite shielding materials, and specifically relates to a magnesium-based composite shielding material with a three-dimensional mesh structure and a preparation method thereof. Background Art

[0002] The statements in this section are merely intended to provide background information related to the technical solution of the present application to aid understanding, and they do not necessarily constitute prior art for the technical solution of the present application.

[0003] With the gradual depletion of traditional fossil energy reserves and the growth of energy supply demand, nuclear energy has gradually gained attention in the power generation industry. However, the neutrons and gamma rays released by nuclear reactions with strong penetrating power can cause serious damage to personnel and equipment around the reactor, and radiation shielding materials are necessary to reduce radiation damage. Among radiation shielding materials, heavy metals, concrete, hydrides, polyethylene, etc. commonly used in the nuclear power field generally have defects or deficiencies in high temperature performance, efficiency, stability, life and environmental friendliness. In contrast, metal-based radiation shielding composite materials such as magnesium-based, aluminum-based, iron-based, and titanium-based have the advantages of radiation resistance, high temperature resistance, good mechanical properties and processing properties, and are valued in the design of advanced nuclear energy systems today and in the future. In particular, magnesium alloys, due to their low density, high strength, high rigidity, good thermal conductivity and electromagnetic shielding capabilities, have become increasingly common choices for metal-based composite shielding material matrices.

[0004] At present, most of the traditional metal-based composite shielding materials are composite materials with randomly and evenly distributed shielding components. If the shielding components are randomly and evenly distributed, micron shielding component particles and micron metal matrix particles with similar particle sizes are generally selected, or the particle size of the micron shielding component particles is slightly larger than the micron metal matrix particles. In the preparation process of the composite material of uniformly distributed micron reinforcement particles and micron metal particles, the tungsten particles need to be pre-dispersed with anhydrous ethanol, pre-dispersed with air flow milling, or pre-dispersed with both to prevent agglomeration. In addition, the uniform distribution method reduces the continuity of the shielding components per unit volume in the composite shielding material, thereby reducing the probability of the radiation interacting with the shielding components when passing through the shielding material, and weakening the shielding effect on the radiation. This weakening problem of the shielding effect is particularly prominent when the thickness of the traditional metal-based composite shielding material is thin. Therefore, to avoid this problem, material researchers often solve it by increasing the volume fraction of shielding components in composite shielding materials or thickening the overall thickness of the material. However, the addition of high volume fraction shielding components easily leads to new problems such as poor dispersion of shielding components and limited improvement in shielding performance. Therefore, multi-step pretreatment is usually required to achieve random and uniform distribution of high volume fraction shielding components, which leads to high production costs and long production processes, and is not suitable for large-scale production. In addition, traditional shielding materials must have sufficient thickness to ensure the shielding effect, which also limits the application scenarios of shielding materials.

[0005] The emerging composite materials with mesh distribution of reinforcements provide a new idea to solve this problem. This kind of structure with mesh distribution of reinforcements means that the reinforcement particles are continuously distributed between the matrix particles (or understood as "distributed around the matrix particles"). The reinforcement particles form a continuous "net", so it is called a mesh structure. Since the reinforcement particles and the matrix particles have a certain three-dimensional shape, the reinforcement is actually distributed in a mesh in three-dimensional space, so this structure is also called a three-dimensional mesh structure (3D mesh structure). This kind of mesh structure composite material does not pursue the uniform distribution of reinforcements but makes the reinforcement distributed in the matrix in a mesh. If the shielding components are distributed in the matrix in a mesh, compared with the traditional random and uniform distribution of shielding components, it will be beneficial to improve the continuity of the distribution of shielding components in the composite shielding material, and then increase the probability of the interaction between the radiation and the shielding components when passing through the shielding material, and improve the shielding effect. However, currently, composite materials with such shielding components (or reinforcements) in a network distribution usually require high-energy ball milling to disperse nano-reinforcement particles on the surface of micron metal matrix particles. For example, Chinese patent CN116987921A uses this method to prepare a high-strength full-lamellar network structure TiAl-based composite material. However, the efficiency of preparing powders by high-energy ball milling is low, and more fresh surfaces will be introduced, which is easy to cause safety problems such as combustion and explosion. Therefore, it is not suitable for large-scale production of large products. Summary of the invention

[0006] In order to solve the problems in the prior art, the present invention proposes a magnesium-based composite shielding material with a three-dimensional mesh structure and a preparation method thereof. The shielding material has a simple preparation process, good macroscopic uniformity of density and shielding effect, good continuity of shielding components per unit volume, and good shielding effect of the material.

[0007] The invention discloses a magnesium-based composite shielding material with a three-dimensional mesh structure, comprising shielding component particles and magnesium matrix particles, wherein the shielding component is tungsten and boron carbide, the magnesium matrix is ​​magnesium and / or magnesium alloy, and the shielding component is tungsten and boron carbide. continuousThe magnesium matrix is ​​distributed around the magnesium matrix particles; wherein the mass percentage of tungsten is 30wt%-60wt%, the mass percentage of boron carbide is 30wt%-50wt%, and the mass percentage of magnesium matrix is ​​10wt%-40wt%, and the total weight percentage of the tungsten particles, boron carbide particles and magnesium matrix particles in the magnesium-based composite material is ≤100%; the average particle size of the tungsten is ≤10μm, the average particle size of the boron carbide is ≤40μm, and the average particle size of the magnesium matrix is ​​≤80μm, preferably the average particle size of the tungsten is 1μm-10μm, the average particle size of the boron carbide is 1μm-40μm, and the average particle size of the magnesium matrix is ​​2μm-80μm; and the ratio of the average particle size of the tungsten to the magnesium matrix is ​​between 1:16-1:2, and the ratio of the average particle size of the boron carbide to the magnesium matrix is ​​between 1:16-1:2, preferably both are between 1:4-1:10. Furthermore, the density of the magnesium-based composite shielding material is 2.9 g / cm 3 -5.0g / cm 3 The purity of tungsten is ≥99wt%, and the total boron-carbon content of boron carbide is ≥98wt%. Tungsten as a shielding component can achieve the effects of γ-ray absorption and fast neutron slowing down, and boron as a shielding component can achieve the effect of thermal neutron absorption. The shielding component is distributed around the magnesium matrix (i.e., between the magnesium matrix) in a continuous, three-dimensional network in the form of a particle reinforcement. Preferably, the magnesium or magnesium alloy powder is selected from one or more mixed powders of commercial grade magnesium alloys of ZK, AZ, WE, VW, and VK or self-matched non-grade magnesium alloys.

[0008] In addition, the present invention also discloses a method for preparing the above-mentioned magnesium-based composite shielding material with a three-dimensional network structure, comprising the following steps:

[0009] (1) Mixing and dispersing: Mechanically mix powders of tungsten with an average particle size of ≤10 μm, boron carbide with an average particle size of ≤40 μm, and a magnesium matrix with an average particle size of ≤80 μm, wherein the average particle size ratio of the tungsten to the magnesium matrix is ​​between 1:16 and 1:2, and the average particle size ratio of the boron carbide to the magnesium matrix is ​​between 1:16 and 1:2. The mechanical mixing is carried out under the protection of an atmosphere of argon, nitrogen, carbon dioxide or a mixture thereof. Grinding balls are used during the mechanical mixing process, wherein the diameter of the grinding balls is Φ5 mm-Φ20 mm, the weight ratio of the grinding balls to the powder to be mixed is 0.5:1-2:1, and the mixing time is 8 h-16 h. After mixing, a mixed powder blank is obtained; wherein the mixing is preferably carried out in a mixer.

[0010] (2) Vacuum degassing: The mixed powder blank is placed in a metal package, and the mixed powder blank is heated and kept warm while being degassed. Then, the mixed powder blank is heated at a temperature of 400°C to 500°C and a vacuum degree of 10 -2 Pa-10-5 The metal sheath is welded and sealed under the condition of Pa;

[0011] (3) Hot isostatic pressing: The metal sheath containing the mixed powder blank is then subjected to hot isostatic pressing. The specific conditions of the hot isostatic pressing treatment are: a heating rate of 2°C / min-10°C / min, a sintering temperature of 400°C-550°C, a pressure of 100MPa-200MPa, and a heat and pressure holding time of 1h-4h. The metal sheath is then cooled in the furnace and the metal sheath is removed by lathing to obtain a magnesium-based composite shielding material.

[0012] In addition, vacuum hot pressing can be used to replace the above step (2) vacuum degassing and step (3) hot isostatic pressing. The specific process is: the mixed powder blank is loaded into the mold cavity of the vacuum hot press and vacuum hot pressed to obtain the magnesium-based composite shielding material. The reaction conditions of the vacuum hot pressing method are: sintering temperature of 400℃-550℃, pressure of 10t-50t, vacuum degree of 10 -2 Pa-10 - 5 Pa, the heat preservation and pressure holding time is 2h-6h, and then it is cooled with the furnace.

[0013] Compared with the prior art, the beneficial technical effects of the present invention are:

[0014] (1) Compared with the process technology of dispersing nano-reinforcement particles on the surface of micron metal particles by high-energy ball milling, the present invention creatively proposes to use the particle size ratio of two types of powders, namely, shielding component (reinforcement) and metal matrix: the particle size of the metal matrix particles in the shielding material is significantly larger than the particle size of the shielding component particles, so that the three-dimensional network distribution of micron shielding component (boron carbide, tungsten) particles around the micron metal matrix particles is achieved. The use of micron particles is more cost-effective, not easy to agglomerate or oxidize, and does not require various pretreatments of nano powders. The preparation process is simple, the process flow is short, the cost is low, and it is easy to implement.

[0015] (2) Compared with the traditional composite shielding materials that require multi-step pretreatment to achieve random and uniform distribution of high volume fraction shielding components, the present invention takes the opposite approach and does not pursue uniform distribution between shielding component particles at the microscopic level. Instead, it achieves three-dimensional mesh distribution of shielding components through reasonable particle size ratio to achieve macroscopic uniformity of measurable density and shielding effect, avoiding the current problem of shielding components being difficult to disperse uniformly in high volume fraction shielding materials. Therefore, there is no need to pretreat tungsten particles to prevent agglomeration. The material uses particle size ratio to relatively "concentrate" the shielding components around the magnesium matrix particles. Compared with the traditional random and uniform distribution of shielding components, this distribution method of shielding components can improve the continuity of the distribution of shielding components in the composite shielding material, increase the probability of radiation interacting with the shielding components when passing through the shielding material, and improve the shielding effect. It solves the problems of poor dispersion of shielding components, limited improvement of shielding performance, and sufficient thickness required to ensure shielding reliability caused by simply increasing the volume fraction of shielding components in composite shielding materials. The new shielding material has the characteristics of miniaturization, light weight, and flexible adjustment of shielding performance, and is particularly suitable for application scenarios where the thickness of shielding components in new nuclear reactors is limited. The invention has low production cost and short production process, is suitable for large-scale production, and can be promoted and applied to other aluminum-based, iron-based, and titanium-based composite shielding materials.

[0016] (3) The present invention uses a mixer for mechanical mixing, which can carry out large-scale mixing and dispersion processing, so the number of mixing times is small, the preparation process is simple, and the process flow is short; at the same time, the mixer does not introduce too much energy during the mixing process, the powder is not easy to be crushed and refined, and the oxidation exothermic combustion or explosion problem caused by the powder refinement can be effectively avoided. Therefore, it is safer than the high-energy ball milling method. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic diagram of the conventional uniform distribution of shielding components and the mesh distribution of shielding components of the present invention when rays are incident;

[0018] Figure 2 is an example SEM photo of magnesium alloy particles in Example 1;

[0019] Figure 3 is an example SEM photo of tungsten particles in Example 1;

[0020] Figure 4 is an example SEM photo of the boron carbide particles in Example 1;

[0021] Figure 5 This is an SEM example photo of the microstructure morphology of the magnesium-based composite shielding material in Example 1 (low magnification);

[0022] Figure 6This is an SEM example photo of the microstructure morphology of the magnesium-based composite shielding material in Example 1 (high magnification);

[0023] Figure 7 This is an SEM example photo of the microstructure morphology of the magnesium-based composite shielding material in Example 6 (low magnification);

[0024] Figure 8 This is an SEM example photo of the microstructure morphology of the magnesium-based composite shielding material in Example 1 (low magnification). DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solution and advantages of the present invention more clear, the following is a detailed description of the magnesium-based composite shielding material with a three-dimensional mesh structure and its preparation method in combination with the embodiments of the present invention. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0026] Example 1

[0027] The magnesium-based composite shielding material is made of 30wt% tungsten particles, 30wt% boron carbide particles and 40wt% WE43 magnesium alloy particles, with average particle sizes of 10μm, 20μm and 80μm respectively (see attached Figure 2 -Attached Figure 4 The preparation method is as follows:

[0028] (1) using a double cone mixer under argon protection, mixing the powders of tungsten particles, boron carbide particles and magnesium alloy particles for 12 hours, using grinding balls in the mechanical mixing process, the grinding balls having a diameter of Φ20 mm, and a weight ratio of the grinding balls to the mixed powders of 1:1, and obtaining a mixed powder blank after mixing;

[0029] (2) The mixed powder blank is placed in a prefabricated aluminum package, and the mixed powder blank is heated, kept warm and degassed. After keeping warm for 10 hours, the mixed powder blank is heated at 400°C and the vacuum degree is less than 1×10 -3 Welding seal under the condition of Pa;

[0030] (3) The temperature was raised to 420°C at a rate of 5°C / min, and the hot isostatic pressing conditions were 160 MPa and 4 h of heat preservation and pressure maintenance. The magnesium-based composite shielding material was formed by cooling to room temperature with the furnace, and the surface aluminum skin was removed to obtain the blank of the magnesium-based composite shielding material (its microstructure is shown in the attached figure). Figure 5 , Attachment Figure 6 As shown in Figure 4 and Figure 5 It can be seen that the gray matrix is ​​a magnesium alloy matrix, the white particles are tungsten particles, the black particles are boron carbide particles, and the shielding component particles are distributed around the matrix in a network shape.

[0031] Example 2

[0032] The magnesium-based composite shielding material is prepared by mixing 40wt% tungsten particles, 40wt% boron carbide particles and 20wt% AZ31 magnesium alloy particles, with average particle sizes of 10μm, 20μm and 80μm, respectively. The preparation method is carried out according to the following steps:

[0033] (1) Using a double cone mixer under argon protection, the powders of tungsten particles, boron carbide particles and magnesium alloy particles are mixed for 8 hours, and grinding balls are used in the mechanical mixing process. The diameter of the grinding balls is Φ10 mm, and the weight ratio of the grinding balls to the mixed powder is 2:1. After mixing, a mixed powder blank is obtained;

[0034] (2) The mixed powder blank is placed in a pre-made magnesium package, and the mixed powder blank is heated, kept warm and degassed. After keeping warm for 10 hours, the mixed powder blank is heated at 400°C and the vacuum degree is less than 1×10 -3 Welding seal under the condition of Pa;

[0035] (3) The temperature is raised to 430°C at a rate of 5°C / min, and the hot isostatic pressing conditions are a pressure of 120 MPa and heat preservation and pressure maintenance for 4 hours. The furnace is cooled to room temperature to realize the molding of the magnesium-based composite shielding material, and the surface magnesium skin is turned off to obtain the initial blank of the magnesium-based composite shielding material.

[0036] Example 3

[0037] The magnesium-based composite shielding material is prepared by the following steps: 30wt% tungsten particles, 30wt% boron carbide particles and 40wt% self-matched magnesium-gadolinium-zirconium (Mg-Gd-Zr, containing about 10wt% gadolinium and about 1wt% zirconium) magnesium alloy particles, with average particle sizes of 5μm, 10μm and 50μm, respectively:

[0038] (1) using a double cone mixer under argon protection, mixing the powders of tungsten particles, boron carbide particles and magnesium alloy particles for 12 hours, using grinding balls in the mechanical mixing process, the grinding balls having a diameter of Φ5 mm, and a weight ratio of the grinding balls to the mixed powders of 0.5:1, and obtaining a mixed powder blank after mixing;

[0039] (2) The mixed powder blank is placed in a prefabricated steel ladle, and the mixed powder blank is heated, kept warm and degassed. After keeping warm for 10 hours, the mixed powder blank is heated at 400°C and the vacuum degree is less than 1×10 -3 Welding seal under the condition of Pa;

[0040] (3) The temperature is raised to 530°C at a rate of 5°C / min, and the hot isostatic pressing conditions are a pressure of 125 MPa and heat preservation and pressure maintenance for 4 hours. The furnace is cooled to room temperature to realize the molding of the magnesium-based composite shielding material, and the surface steel skin is removed to obtain the initial blank of the magnesium-based composite shielding material.

[0041] Example 4

[0042] The magnesium-based composite shielding material is prepared by mixing 30wt% tungsten particles, 30wt% boron carbide particles and 40wt% self-matched magnesium-gadolinium-zirconium (Mg-Gd-Zr, containing about 10wt% gadolinium and about 1wt% zirconium) magnesium alloy particles, with average particle sizes of 10μm, 40μm and 80μm respectively. The preparation method is carried out according to the following steps:

[0043] (1) using a double cone mixer under argon protection, mixing the powders of tungsten particles, boron carbide particles and magnesium alloy particles for 12 hours, using grinding balls in the mechanical mixing process, the grinding balls having a diameter of Φ20 mm, and a weight ratio of the grinding balls to the mixed powders of 1.5:1, and obtaining a mixed powder blank after mixing;

[0044] (2) The mixed powder blank is placed in a prefabricated steel ladle, and the mixed powder blank is heated, kept warm and degassed. After keeping warm for 10 hours, the mixed powder blank is heated at 400°C and the vacuum degree is less than 1×10 -3 Welding seal under the condition of Pa;

[0045] (3) The temperature is raised to 530°C at a rate of 5°C / min, and the hot isostatic pressing conditions are a pressure of 130 MPa and heat preservation and pressure maintenance for 4 hours. The furnace is cooled to room temperature to realize the molding of the magnesium-based composite shielding material, and the surface steel skin is turned off to obtain the initial blank of the magnesium-based composite shielding material.

[0046] Example 5

[0047] The magnesium-based composite shielding material is prepared by mixing 30wt% tungsten particles, 50wt% boron carbide particles and 20wt% WE43 magnesium alloy particles, with average particle sizes of 10μm, 20μm and 80μm, respectively. The preparation method is carried out according to the following steps:

[0048] (1) using a double cone mixer under argon protection, mixing the powders of tungsten particles, boron carbide particles and magnesium alloy particles for 12 hours, using grinding balls in the mechanical mixing process, the grinding balls having a diameter of Φ20 mm, and a weight ratio of the grinding balls to the mixed powders of 1:1, and obtaining a mixed powder blank after mixing;

[0049] (2) The mixed powder blank is placed in a prefabricated steel ladle, and the mixed powder blank is heated, kept warm and degassed. After keeping warm for 10 hours, the mixed powder blank is heated at 400°C and the vacuum degree is less than 1×10 -3 Welding seal under the condition of Pa;

[0050] (3) The temperature is raised to 520°C at a rate of 5°C / min, and the hot isostatic pressing conditions are a pressure of 150 MPa and heat preservation and pressure maintenance for 4 hours. The furnace is cooled to room temperature to realize the molding of the magnesium-based composite shielding material, and the surface steel skin is removed to obtain the initial blank of the magnesium-based composite shielding material.

[0051] Example 6

[0052] The magnesium-based composite shielding material is prepared by mixing 30wt% tungsten particles, 30wt% boron carbide particles and 40wt% WE43 magnesium alloy particles, with average particle sizes of 10μm, 20μm and 80μm, respectively. The preparation method is as follows:

[0053] (1) using a double cone mixer under argon protection, mixing the powders of tungsten particles, boron carbide particles and magnesium alloy particles for 12 hours, using grinding balls in the mechanical mixing process, the grinding balls having a diameter of Φ20 mm, and a weight ratio of the grinding balls to the mixed powders of 1:1, and obtaining a mixed powder blank after mixing;

[0054] (2) The mixed powder blank was loaded into the mold cavity of a vacuum hot press and subjected to vacuum hot pressing. The sintering temperature was 430°C, the pressure was 40t, and the vacuum degree was 0.5×10 -3 Pa, the heat preservation and pressure preservation time is 4h, and then the furnace is cooled to obtain a magnesium-based composite shielding material.

[0055] Example 7

[0056] The magnesium-based composite shielding material is prepared by mixing 60wt% tungsten particles, 30wt% boron carbide particles and 10wt% WE43 magnesium alloy particles, with average particle sizes of 2μm, 5μm and 30μm, respectively. The preparation method is as follows:

[0057] (1) using a double cone mixer under argon protection, mixing the powders of tungsten particles, boron carbide particles and magnesium alloy particles for 12 hours, using grinding balls in the mechanical mixing process, the grinding balls having a diameter of Φ5 mm, and a weight ratio of the grinding balls to the mixed powders of 0.5:1, and obtaining a mixed powder blank after mixing;

[0058] (2) The mixed powder blank is placed in a prefabricated aluminum package, and the mixed powder blank is heated, kept warm and degassed. After keeping warm for 8 hours, the mixed powder blank is heated at 500°C and the vacuum degree is less than 1×10 -2 Welding seal under the condition of Pa;

[0059] (3) The temperature is raised to 400°C at a rate of 2°C / min, and the hot isostatic pressing conditions are a pressure of 200 MPa and heat preservation and pressure maintenance for 2 hours. The furnace is cooled to room temperature to realize the molding of the magnesium-based composite shielding material, and the surface aluminum skin is removed to obtain the initial blank of the magnesium-based composite shielding material.

[0060] Example 8

[0061] The magnesium-based composite shielding material is prepared by mixing 30wt% tungsten particles, 30wt% boron carbide particles and 40wt% WE43 magnesium alloy particles, with average particle sizes of 10μm, 40μm and 80μm, respectively. The preparation method is as follows:

[0062] (1) using a double cone mixer under argon protection, mixing the powders of tungsten particles, boron carbide particles and magnesium alloy particles for 12 hours, using grinding balls in the mechanical mixing process, the grinding balls having a diameter of Φ20 mm, and a weight ratio of the grinding balls to the mixed powders of 1:1, and obtaining a mixed powder blank after mixing;

[0063] (2) The mixed powder blank is placed in a prefabricated aluminum package, and the mixed powder blank is heated, kept warm and degassed. After keeping warm for 10 hours, the mixed powder blank is heated at 400°C and the vacuum degree is less than 1×10 -5 Welding seal under the condition of Pa;

[0064] (3) The temperature is raised to 550°C at a rate of 10°C / min, and the hot isostatic pressing conditions are a pressure of 100 MPa and heat preservation and pressure maintenance for 2 hours. The furnace is cooled to room temperature to realize the molding of the magnesium-based composite shielding material, and the surface aluminum skin is removed to obtain the initial blank of the magnesium-based composite shielding material.

[0065] Example 9

[0066] The magnesium-based composite shielding material is prepared by mixing 30wt% tungsten particles, 30wt% boron carbide particles and 40wt% WE43 magnesium alloy particles, with average particle sizes of 10μm, 20μm and 80μm, respectively. The preparation method is as follows:

[0067] (1) using a double cone mixer under argon protection, mixing the powders of tungsten particles, boron carbide particles and magnesium alloy particles for 12 hours, using grinding balls in the mechanical mixing process, the grinding balls having a diameter of Φ10 mm, and a weight ratio of the grinding balls to the mixed powders of 1:1, and obtaining a mixed powder blank after mixing;

[0068] (2) The mixed powder blank was loaded into the mold cavity of a vacuum hot press and subjected to vacuum hot pressing. The sintering temperature was 550°C, the pressure was 10t, and the vacuum degree was 1×10 -5 Pa, the heat preservation and pressure preservation time is 2h, and then the furnace is cooled to obtain a magnesium-based composite shielding material.

[0069] Example 10

[0070] The magnesium-based composite shielding material is prepared by mixing 30wt% tungsten particles, 30wt% boron carbide particles and 40wt% WE43 magnesium alloy particles, with average particle sizes of 10μm, 20μm and 80μm, respectively. The preparation method is as follows:

[0071] (1) using a double cone mixer under argon protection, mixing the powders of tungsten particles, boron carbide particles and magnesium alloy particles for 16 hours, using grinding balls in the mechanical mixing process, the grinding balls having a diameter of Φ20 mm, and a weight ratio of the grinding balls to the mixed powders of 2:1, and obtaining a mixed powder blank after mixing;

[0072] (2) The mixed powder blank was loaded into the mold cavity of a vacuum hot press and vacuum hot pressed at a sintering temperature of 400°C, a pressure of 50t, and a vacuum degree of 1×10 -2 Pa, the heat preservation and pressure preservation time is 6 hours, and then the furnace is cooled to obtain a magnesium-based composite shielding material.

[0073] The material properties of Examples 1-10 are shown in Table 1:

[0074] Table 1 Material properties of the above examples

[0075]

[0076] Comparative Example 1

[0077] The magnesium-based composite shielding material is prepared by mixing 30wt% tungsten particles, 30wt% boron carbide particles and 40wt% WE43 magnesium alloy particles, with average particle sizes of 25μm, 60μm and 50μm, respectively. The preparation method is carried out according to the following steps:

[0078] (1) Pre-grinding the boron carbide particles by jet milling to remove sharp edges of the particles, and pre-dispersing the tungsten particles by anhydrous ethanol, jet milling, or a combination of the two;

[0079] (2) Using a double cone mixer under argon protection, the powders of tungsten particles, boron carbide particles and magnesium alloy particles are mixed for 12 hours, and grinding balls are used in the mechanical mixing process. The diameter of the grinding balls is Φ20 mm, and the weight ratio of the grinding balls to the mixed powder is 1:1. After mixing, a mixed powder blank is obtained;

[0080] (3) The mixed powder blank is placed in a prefabricated aluminum package, and the mixed powder blank is heated, kept warm and degassed. After keeping warm for 10 hours, the mixed powder blank is heated at 400°C and the vacuum degree is less than 1×10 -3 Welding seal under the condition of Pa;

[0081] (4) The temperature was raised to 420°C at a rate of 5°C / min, and the hot isostatic pressing conditions were 160 MPa and 4 h of heat preservation and pressure maintenance. The magnesium-based composite shielding material was formed by cooling to room temperature with the furnace, and the surface aluminum skin was removed to obtain a blank of the magnesium-based composite shielding material (its microstructure is shown in the attached figure). Figure 8 shown). Figure 8 The medium gray matrix is ​​a magnesium alloy matrix, the white particles are tungsten particles, and the black particles are boron carbide particles, and the particle distribution is relatively uniform.

[0082] As shown in Table 2, the shielding performance of Example 1 and Comparative Example 1 is compared, wherein the larger the linear attenuation coefficient of the Cf fast neutron source is, the better the radiation protection performance is. Under the premise of the same amount of shielding component addition, density, and compactness, the shielding efficiency (Cf fast neutron source) of Example 1 is 3-8% higher than that of Comparative Example 1, and the thinner the thickness of the tested material is, the more obvious the improvement of the shielding efficiency is.

[0083] Table 2 Shielding performance comparison of Example 1 and Comparative Example 1

[0084]

[0085] It should be understood that the above embodiments are only used to illustrate the preferred implementation details of the present invention, and are not used to limit the content and scope of the present invention. For general R&D and technical personnel in this field and profession, the present invention can have various adjustments and variations; therefore, any adjustments, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention, without the relevant personnel making creative efforts, should be included in the scope of protection of the present invention.

Claims

1. A magnesium-based composite shielding material with a three-dimensional mesh structure, characterized in that: It comprises shielding component particles and magnesium matrix particles, wherein the shielding component is tungsten and boron carbide, the magnesium matrix is ​​magnesium and / or magnesium alloy, and the shielding component particles are continuously distributed around the magnesium matrix particles; The mass percentage of tungsten is 30wt%-60wt%, the mass percentage of boron carbide is 30wt%-50wt%, and the mass percentage of magnesium matrix is ​​10wt%-40wt%. The purity of tungsten is ≥99wt%, and the total boron-carbon content of boron carbide is ≥98wt%. The average particle size of tungsten is ≤10μm, the average particle size of boron carbide is ≤40μm, and the average particle size of magnesium matrix is ​​≤80μm. The ratio of the average particle size of tungsten to that of magnesium matrix is ​​between 1:16 and 1:2, and the ratio of the average particle size of boron carbide to that of magnesium matrix is ​​between 1:16 and 1:

2.

2. The magnesium-based composite shielding material with a three-dimensional mesh structure according to claim 1, characterized in that: The average particle size of the tungsten is 1 μm-10 μm, the average particle size of the boron carbide is 1 μm-40 μm, and the average particle size of the magnesium matrix is ​​2 μm-80 μm.

3. The magnesium-based composite shielding material with a three-dimensional mesh structure according to claim 1, characterized in that: The density of the magnesium-based composite shielding material is 2.9 g / cm 3 -5.0g / cm 3 .

4. A method for preparing a magnesium-based composite shielding material with a three-dimensional network structure as claimed in any one of claims 1 to 3, characterized in that: The following steps are involved: (1) Mixing and dispersing: mechanically mixing powders of tungsten with an average particle size of ≤10 μm, boron carbide with an average particle size of ≤40 μm, and a magnesium matrix with an average particle size of ≤80 μm, wherein the average particle size ratio of the tungsten to the magnesium matrix is ​​between 1:16 and 1:2, and the average particle size ratio of the boron carbide to the magnesium matrix is ​​between 1:16 and 1:

2. The mechanical mixing is performed under the protection of an atmosphere of argon, nitrogen, carbon dioxide or a mixture thereof. Grinding balls are used during the mechanical mixing process, wherein the diameter of the grinding balls is Φ5 mm-Φ20 mm, and the weight ratio of the grinding balls to the powder to be mixed is 0.5:1-2:

1. The mixing time is 8 h-16 h, and a mixed powder blank is obtained after mixing. (2) Vacuum degassing: The mixed powder blank is placed in a metal sheath, and the mixed powder blank is heated and kept warm while being degassed, and then the metal sheath is welded and sealed; (3) Hot isostatic pressing: The metal sheath containing the mixed powder blank is then subjected to hot isostatic pressing, and the metal sheath is finally removed by lathing to obtain a magnesium-based composite shielding material.

5. The method for preparing a magnesium-based composite shielding material with a three-dimensional network structure according to claim 4, characterized in that: Step (2) During the vacuum degassing process, the temperature is 400°C-500°C and the vacuum degree is 10 -2 Pa-10 -5 The metal sheath is welded and sealed under the condition of Pa.

6. The method for preparing a magnesium-based composite shielding material with a three-dimensional network structure according to claim 4, characterized in that: The specific conditions of the hot isostatic pressing treatment in step (3) are: heating rate of 2°C / min-10°C / min, sintering temperature of 400°C-550°C, pressure of 100MPa-200MPa, heat preservation and pressure holding time of 1h-4h, followed by furnace cooling.

7. A method for preparing a magnesium-based composite shielding material with a three-dimensional network structure as claimed in any one of claims 1 to 3, characterized in that: The following steps are involved: (1) Mixing and dispersing: mechanically mixing powders of tungsten with an average particle size of ≤10 μm, boron carbide with an average particle size of ≤40 μm, and a magnesium matrix with an average particle size of ≤80 μm, wherein the ratio of the average particle size of tungsten to that of the magnesium matrix is ​​between 1:16 and 1:2, and the ratio of the average particle size of boron carbide to that of the magnesium matrix is ​​between 1:16 and 1:2, to obtain a mixed powder blank; (2) Vacuum hot pressing: The mixed powder blank is loaded into the mold cavity of a vacuum hot press and vacuum hot pressed to obtain a magnesium-based composite shielding material.

8. The method for preparing a magnesium-based composite shielding material with a three-dimensional network structure according to claim 7, characterized in that: The specific conditions of vacuum hot pressing in step (2) are: sintering temperature is 400℃-550℃, pressure is 10t-50t, vacuum degree is 10 -2 Pa-10 -5 Pa, the heat preservation and pressure holding time is 2h-6h, and then it is cooled with the furnace.

Citation Information

Patent Citations

  • TiAl-based composite material with full-lamellar net-shaped structure and preparation method thereof

    CN116987921A

  • Preparation method of high-density boron-containing composite material

    CN112779455A

  • Anti-radiation magnesium-based composite material as well as preparation method and application thereof

    CN117721338A

  • Additive manufacturing process for producing aluminum-boron carbide metal matrix composites

    US20200269318A1